Control method and device for arc plasma auxiliary heating reinforced self-propagating magnesium reduction reaction
The self-propagating magnesium reduction reaction is strengthened by arc plasma assisted heat, which solves the problems of high energy consumption and low efficiency in the traditional Pidgeon magnesium metallurgical process, and realizes high-efficiency, low-carbon magnesium metallurgical production, which is suitable for large-scale production and reduces costs. production costs.
Patent Information
- Application Number
- CN202410974509.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The traditional Pidgeon magnesium metallurgical process has problems such as high energy consumption, long time, low efficiency and intermittent production methods, resulting in high carbon emissions and environmental pollution, making it difficult to meet national energy conservation and emission reduction requirements.
The method uses arc plasma auxiliary heat to strengthen the self-propagating magnesium reduction reaction. Through the high-temperature auxiliary heat of the plasma torch, the calcined dolomite, ferrosilicon and fluorite are pressed into sheets for rapid heating, forming a coordinated transmission of conduction, convection and radiation. Thermal conditions improve heat transfer efficiency, and promote reactions through perforated plate design and electric field force to accelerate magnesium vapor overflow and self-propagation reactions.
It significantly reduces the energy consumption of the magnesium metallurgical process, improves reaction efficiency, realizes continuous and low-carbon production, is suitable for large-scale production, simplifies device design and process flow, and reduces production costs.
Smart Images

Figure CN118773435A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal smelting, and in particular to a control method and device for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction. Background Art
[0002] As a new type of structural and functional material, magnesium and magnesium alloys have been widely used in many aspects of the transportation field in recent years. As the lightest structural material, magnesium alloys can meet the increasingly stringent energy-saving and exhaust emission requirements of the transportation industry. Magnesium alloys have excellent thin-wall casting performance and good specific strength, stiffness and collision resistance, which can fully meet the requirements of 3C products for high integration, lightness, miniaturization, anti-fall and electromagnetic shielding, heat dissipation and environmental protection. Magnesium sacrificial anode is one of the effective methods to prevent metal corrosion. With the continuous development of the functions and applications of magnesium metal materials, magnesium metal has become one of the most important materials after steel.
[0003] my country is rich in magnesium resources and is the country with the largest magnesium production in the world. There are two main technologies for magnesium metallurgy: electrolysis and Pidgeon process. In the last century, due to the high cost of Pidgeon process, electrolysis was the main method used internationally. After entering this century, due to the significant decline in my country's energy costs, coupled with the advantages of Pidgeon process such as small investment, simple process and convenient operation, Pidgeon process has developed rapidly in my country's primary magnesium industry and has become the world's largest supplier of primary magnesium. At present, more than 90% of primary magnesium in my country is produced by Pidgeon process.
[0004] Although China's Pijiang process represents the best level in the world, it has not yet gotten rid of the problems of high energy consumption and high pollution, and belongs to the development field of national restrictions. With the proposal of the national "dual carbon" goal, magnesium metallurgy has become the main metal variety of carbon emissions among non-ferrous metals, and has attracted much attention from national policies. The newly promulgated "Energy Consumption Limits for Industrial Silicon and Magnesium Unit Products" (GB21347-2023) reduces the energy consumption standard from 6 tons of standard coal / ton of magnesium to 3.5-5.0 tons of standard coal / ton of magnesium. More stringent conditions are put forward for new magnesium metallurgical projects.
[0005] It can be seen that the magnesium metallurgical industry is facing a development environment of "ice and fire". On the one hand, my country has large reserves of magnesium resources, a good industrial foundation, many related industries, and great market prospects; on the other hand, it has high energy consumption, large carbon emissions, and serious environmental pollution, and belongs to a restricted industry. Therefore, achieving energy conservation and emission reduction in magnesium metallurgy has become a must in Xuanzhijian. The purpose of this invention is to propose a high-efficiency and low-emission magnesium metallurgical technology in response to the newly promulgated "Industrial Silicon and Magnesium Unit Product Energy Consumption Limit" (GB21347-2023) standard and the national dual-carbon target requirements, which has achieved substantial energy conservation and emission reduction in the magnesium metallurgical industry.
[0006] Whether it is horizontal tube or vertical tank reduction, the traditional Pidgeon process mainly includes three major processes, also known as the "three-step" magnesium smelting process, namely dolomite calcination, ball reduction and crude magnesium refining. The energy consumption of magnesium smelting is also mainly composed of these three parts. From dolomite calcination to batching, grinding, ball making, to high temperature vacuum reduction, and finally crude magnesium refining and ingot casting, it becomes commercial magnesium. In 1941, Pidgeon Lavery (L.M. Pidgeon), a professor at the University of Toronto in Canada, developed the Pidgeon process. The calcined dolomite, ferrosilicon and fluorite were ground and balled in a certain proportion, and the pellets were added to the reduction tank made of heat-resistant alloy steel. The temperature in the reduction tank was maintained at 1150℃~1200℃ and the vacuum degree was about 10Pa~20Pa. The reduction reaction occurred at high temperature, and the generated magnesium vapor flowed to the cooling area with a crystallization water jacket to condense into crystalline magnesium. Professor Pidgeon used this process to build a test device in Ottawa to reduce calcined white using ferrosilicon as a reducing agent. The following year, the world's first Pidgeon magnesium smelting plant with an annual output of 5,000 tons was built in Haley, Ontario, Canada. This is the earliest magnesium metallurgical horizontal tube reduction process.
[0007] Similar to the horizontal tube reduction, the vertical tank reduction of magnesium metallurgy uses the same raw materials and preparation process, the same temperature and vacuum, and both use external heating methods and heat-resistant steel alloy tanks. The difference is that the reduction tank is installed vertically, and there are upper feeding and upper slag discharge modes and upper feeding and lower slag discharge modes, which helps to achieve the continuity of magnesium metallurgy. However, after a long period of operation of the vertical tube reduction furnace, practice has proved that the vertical tube reduction time is shorter than the horizontal tube reduction time, but the suspension device is lifted out of the reduction tank under high temperature environment, the operating environment is harsh, and it is easy to oxidize, the life is short, and the reliability is poor. Because of this, although the vertical tube reduction has attracted much attention and expectations, it has always been difficult to develop.
[0008] During this period, Professor Wang Xiaogang's team at Xi'an University of Science and Technology proposed the idea of internal and external heating for vertical tube reduction. Professor Zhang Ting'an's team at the Department of Metallurgy at Northeastern University proposed a method of continuous calcination of dolomite and magnesium reduction to reduce the heat loss of calcined dolomite. Che Yusi's team at Zhengzhou University used argon enhanced convection to improve the efficiency of pellet heating and magnesium vapor overflow. Due to the small thermal melting point of argon, its industrial application is limited.
[0009] The above research has a certain impact on reducing the problem of high energy consumption in magnesium metallurgy. However, it does not fundamentally solve the problem of high energy consumption in magnesium metallurgy. Looking back at the process of reducing magnesium by the Pijiang method, dolomite is first calcined to convert it into magnesium oxide and calcium oxide, and the reaction activity is increased. Then it is crushed into a certain fineness and mixed with ferrosilicon and fluorite in a certain proportion. Sometimes a binder is added to improve the molding quality of the pellets. After that, the mixed powder is prepared into balls or blocks of a certain size by a ball press; finally, these blocks are loaded into a horizontal or vertical tube reduction furnace, and the reduction reaction is carried out under high temperature and vacuum conditions. The generated magnesium vapor is condensed to form crystalline magnesium. The reason why the process is energy-intensive is firstly because calcined dolomite is a poor thermal conductor. In a systematic vacuum environment, there is no convection mechanism for heat transfer, and the heat transfer efficiency is significantly reduced. Secondly, radiation heat transfer has the characteristics of surface heat transfer. The larger the direct irradiation area, the better the heat transfer effect. However, due to the limitation of the pellet pile state, the outer surface of the pellet pile is mainly radiative heat transfer, and the inner part is mainly conductive mechanism. Finally, point contact is the main method for contact between pellets in the pile and between powder particles in the pellets, which significantly reduces the contact surface of the heat conduction mechanism and the heat transfer efficiency between pellets in the pile and between particles in the pellets. It can be seen that the inefficiency of heat transfer in the magnesium metallurgical process is the root cause of the following problems in Pidgeon magnesium metallurgy.
[0010] First: high energy consumption. In terms of heat source, the heat source of external heating in my country's Pijiang method is basically the heat generated by liquid fuel, gas fuel and solid fuel, and most of the magnesium plants use solid coal as fuel. It consumes 8 to 12 tons of high-quality coal to produce one ton of magnesium. It has high energy consumption and large CO2 emissions, which cannot meet the requirements of the new national energy consumption standards.
[0011] Second: Long time and low efficiency: The horizontal tube reduction time is as long as 8 to 12 hours. Even if the internal and external heating is used, it still takes more than 5 hours, which is inefficient.
[0012] Third: intermittent production method; although the vertical tube type has continuous characteristics, its stability is poor and it has not yet become the mainstream of industrial application. The horizontal tube is widely used, but it belongs to multi-tube intermittent continuous production. The working and thermal efficiency are not high. Summary of the invention
[0013] The purpose of the present invention is to provide a control method and device for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction. The device has the characteristics of simple design, safe process and cost saving. The reaction method of the device is energy-saving, efficient and can realize large-scale production.
[0014] In order to achieve the above-mentioned purpose, the technical solution of the present invention is an arc plasma assisted heating enhanced self-propagating magnesium reduction reaction device, the principle of which is to quickly heat the sheet material formed by pressing calcined dolomite + ferrosilicon + fluorite with a "honeycomb coal" structure through the high-temperature auxiliary heating effect of the plasma torch, so that the sheet material undergoes a self-propagating reaction, and the generated magnesium vapor leaves the sheet material under the carrying of the plasma torch to complete the solid-gas separation. The method has the following effects: first, the convection heat transfer mechanism of the plasma is increased in the magnesium metallurgical process, forming a heat transfer condition in which the three mechanisms of conduction, convection and radiation are coordinated, and the heat transfer efficiency is significantly improved; second, the structural design of the sheet material formed by pressing calcined dolomite + ferrosilicon + fluorite reduces the heat transfer distance and accelerates the heat transfer efficiency; third, the carrying effect of the plasma torch on magnesium vapor accelerates the overflow of magnesium vapor and promotes the self-propagating reduction reaction to the unreacted area.
[0015] The device used includes an integrated vertical vacuum furnace body consisting of a furnace shell and an insulation layer and a refractory layer arranged in the furnace shell. A cold slag bin, a secondary slag unloading vacuum valve, a primary slag unloading vacuum valve, a lower control valve, an upper control valve, a secondary feeding vacuum valve, a storage bin, a primary feeding vacuum valve and a feeding port are arranged in the furnace body from bottom to top. A reaction zone for placing a honeycomb perforated plate material made of calcined dolomite powder, fluorite and ferrosilicon reducing agent is formed between the upper control valve and the lower control valve. An arc plasma generator for producing a plasma torch connected to the reaction zone is arranged on one side of the reaction zone. One or more crystallization zones for collecting magnesium vapor connected to the reaction zone through a magnesium outlet vacuum valve are arranged on the other side of the reaction zone. A plurality of magnesium crystallizers for crystallizing vapor are installed in the crystallization zone.
[0016] Furthermore, the arc plasma generator includes an air inlet and an air outlet opened on the side, and a power supply system is arranged inside the arc plasma generator. The power supply system is respectively connected to the cathode and the double anode on the side close to the reaction zone.
[0017] Furthermore, the holes of the perforated plate are evenly distributed honeycomb holes, the average distance £ between adjacent holes is equal, £ is (1 / 6-1 / 5)*L, the plate thickness is h=(2-4)L, and L is the plate length.
[0018] Furthermore, the outer shell of the crystallization zone is provided with a crystallization zone cold water jacket.
[0019] Furthermore, the outer shell of the cold slag bin is provided with a cooling water jacket.
[0020] A control method for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction comprises the following steps:
[0021] S1: Integrate calcined dolomite powder, fluorite and ferrosilicon reducing agent into a perforated plate for standby use;
[0022] S2: placing the perforated sheet material into the reaction zone through the feed port, then closing all valves in the device and ensuring that the interior of the vertical vacuum furnace is in the same vacuum state;
[0023] S3: Open the vacuum system of the crystallization zone, and then open the magnesium vacuum valve;
[0024] S4: setting the current intensity and voltage of the power supply system so that the power of the arc plasma generator reaches 18-22 kW, obtaining a stable plasma torch whose length exceeds the length of the perforated sheet, and the perforated sheet fully reacts under the interaction of the plasma torch and the self-propagating reaction;
[0025] S5: The magnesium vapor generated by the reaction gathers in the crystallization area under the combined action of the plasma torch and the vacuum pumping system of the crystallization area. After the magnesium vapor is collected, the magnesium vacuum valve is closed, the lower control valve is opened to discharge the residue in the reaction area, and the first-level slag discharge vacuum valve and the second-level slag discharge vacuum valve are opened at the same time to discharge the cold slag into the cold slag bin;
[0026] S6: The magnesium vapor collected in the crystallization zone is cooled and crystallized in the magnesium crystallizer, and then the magnesium crystallizer is taken out to obtain the final product.
[0027] Furthermore, the ferrosilicon reducing agent is one of metallic silicon, silicon-based ferroalloy, calcium silicon, silicon aluminum, silicon aluminum iron, and silicon calcium iron.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The device of the present invention completes the reaction by arranging an arc plasma generator and a crystallization zone on both sides of a vertical vacuum furnace body. The device has a simple design, a safe process, and saves the cost of industrial production equipment.
[0030] (2) The present invention adopts an arc plasma generator. Arc plasma releases energy in a short time and can quickly promote the reaction, that is, reduce the electrical energy consumed by the reducing agent and thermal energy, reduce energy consumption and increase generation efficiency.
[0031] (3) The present invention reduces the potential barrier required for the reaction by means of the electric field force and the Coulomb force during the self-propagating reaction with the help of the perforated plate material pre-filled with magnesium ore and the reducing agent, thereby accelerating the reaction and changing the reaction mechanism dominated by high-temperature step-by-step reaction in traditional reactions; at the same time, the honeycomb-like design of the perforated plate material can improve the uniform distribution of the current, further realize the contact area of the reactants, and timely separate the reacted phase, thereby greatly improving the efficiency of the reduction reaction.
[0032] (4) The present invention realizes continuous, large-scale and low-carbon manufacturing through reduction under vacuum and efficient self-propagating step-by-step reaction.
[0033] (5) The present invention can be applied to any reduction alloy reaction similar to the Pidgeon process or other alloy component diffusion, and has inspiring significance for changing the traditional metal smelting method.
[0034] Furthermore, the present invention controls the reaction kinetic energy and reaction efficiency in the reaction solid-solid system by adjusting the ratio of the perforated material plate, and at the same time controls the current intensity and voltage of the power supply system to control the magnesium reduction reaction from multiple aspects, ultimately achieving a high-efficiency, high-purity reaction product. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a schematic structural diagram of the self-propagating reaction device for magnesium reduction discharge plasma assisted heat enhancement according to the present invention;
[0036] Figure 2 It is a schematic diagram of the structure of the perforated sheet material of the present invention;
[0037] Figure 3 It is a schematic diagram of the structure of the arc plasma generator of the present invention.
[0038] Among them: 1. Cold slag bin; 2. Secondary slag unloading vacuum valve; 3. Primary slag unloading vacuum valve; 4. Arc plasma generator; 5. Upper control valve; 6. Secondary feeding vacuum valve; 7. Primary feeding vacuum valve; 8. Feeding port; 9. Plate with holes; 10. Lower control valve; 11. Magnesium outlet vacuum valve; 12. Cold water jacket in crystallization zone; 13. Crystallization zone; 14. Furnace shell; 15. Insulation layer; 16. Storage bin; 17. Air inlet; 18. Air outlet; 19. Cathode; 20. Double anode; 21. Power supply system. DETAILED DESCRIPTION
[0039] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0040] like Figure 1 The device for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction shown in the figure comprises a vertical vacuum furnace body composed of a furnace shell 14 and an insulation layer 15 and a refractory layer arranged in the furnace shell 14, wherein a cold slag bin 1, a secondary slag unloading vacuum valve 2, a primary slag unloading vacuum valve 3, a lower control valve 10, an upper control valve 5, a secondary feed vacuum valve 6, a storage bin 16, a primary feed vacuum valve 7 and a feed port 8 are arranged from bottom to top in the furnace body, and a reaction zone for placing a honeycomb perforated plate material 9 made of calcined dolomite powder, fluorite and ferrosilicon reducing agent is formed between the upper control valve 5 and the lower control valve 10, see Figure 2It should be noted that the holes of the perforated plate 9 are uniformly distributed honeycomb holes, and the average distance £ between adjacent holes is equal, £ is (1 / 6~1 / 5)*L, the plate thickness is h=(2~4)L, L is the plate length, and the size of the perforated plate 9 is adjusted according to actual work needs to regulate the reaction kinetic energy and reaction efficiency in the reaction solid-solid system; an arc plasma generator 4 for generating a plasma torch is provided on one side of the reaction zone, and one or more crystallization zones 13 for collecting magnesium vapor are provided on the other side of the reaction zone, and a plurality of magnesium crystallizers for crystallizing the vapor are installed in the crystallization zone 13, and a magnesium outlet vacuum valve 11 is provided between the crystallization zone 13 and the reaction zone. It should be noted that a cooling water jacket is provided on the outside of the cold slag bin 1 to accelerate the rapid cooling of the residue after the reaction to ensure subsequent treatment; a crystallization zone cold water jacket 12 is provided on the outside of the crystallization zone to accelerate the crystallization rate of the crystallization zone and shorten the preparation time.
[0041] like Figure 3 As shown, the arc plasma generator 4 includes an air inlet 17 and an air outlet 18 opened on the side. A power supply system 21 is arranged inside the arc plasma generator 4. The power supply system 21 is respectively connected to the cathode 19 and the double anode 20 on the side close to the reaction zone. The arc plasma generator 4 is adopted because arc thermal plasma releases energy in a short time, which can quickly promote the reaction and increase the generation efficiency.
[0042] Embodiment 1 A control method for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction comprises the following steps:
[0043] S1: Integrate calcined dolomite powder, fluorite and metallic silicon to form a perforated plate 9 for standby use;
[0044] It should be noted that the particle size and particle size distribution should be reasonable, and the agglomeration pressure should also be reasonably controlled. Because it is dry pressing, no adhesive is allowed to be added, and the finished agglomerate must have a certain compressive strength and appropriate density. Too high a density (that is, the agglomerate is too dense) affects the smooth (diffusion) escape of the reduced gaseous magnesium; too low a density (that is, the agglomerate is not dense enough) not only affects the effective contact between the reactant particles and the reduction effect, but also affects the agglomerate strength (easy to break); and the shape and size of the raw materials are selected and designed with the fundamental purpose of facilitating the reduction reaction, shortening the reduction time as much as possible, and increasing the magnesium production of a single tank; the role of the hole is to allow the plasma torch to extend into the hole, "ignite" the boundary material, promote the self-propagating reaction, and do a good job of sealing and drying;
[0045] S2: After closing all valves in the device, evacuate, then open the primary feed vacuum valve 7 to add the perforated sheet material 9 from the feed port 8 to the storage bin 16, close the primary feed vacuum valve 7, and after the storage bin 16 is evacuated to the vacuum degree consistent with that in the reaction zone, open the secondary feed vacuum valve 6 and the upper control valve 5 to bring the perforated sheet material 9 into the reaction zone, and close the upper control valve 5;
[0046] It should be noted that in order to ensure continuous operation, the furnace must be kept in a vacuum state for a long time;
[0047] S3: According to the amount of magnesium vapor theoretically obtained in the reaction zone, a corresponding number of magnesium crystallizers are assembled in the crystallization zone 13, the vacuum pumping system of the crystallization zone 13 is turned on, and then the magnesium outlet vacuum valve 11 is opened;
[0048] S4: Setting the current intensity and voltage of the power supply system 21 so that the power of the arc plasma generator 4 reaches 20Kw, obtaining a stable plasma torch whose length exceeds that of the perforated sheet 9. Under the interaction of the plasma torch and the self-propagating reaction, the perforated sheet 9 starts to self-propagate from the hole to the inside, thereby ensuring the full reaction. At the same time, the thermal insulation layer 15 can keep the magnesium in a vapor state, further reducing the power loss;
[0049] S5: The magnesium vapor generated by the reaction is gathered toward the crystallization area 13 under the joint action of the plasma torch and the vacuum pumping system of the crystallization area 13. After the magnesium vapor is collected, the magnesium outlet vacuum valve 11 is closed, and the lower control valve 10 is opened to discharge the residue in the reaction area. At the same time, the first-level slag discharge vacuum valve 1 and the second-level slag discharge vacuum valve 2 are opened to discharge the cold slag into the cold slag bin 1;
[0050] S6: After the magnesium vapor collected in the crystallization zone 13 is cooled and crystallized in the magnesium crystallizer, the magnesium crystallizer is taken out to obtain the final product.
[0051] It should be noted that when discharging the residue, the temperature in the reaction zone is kept constant and the above steps are repeated, so that continuous operation can be carried out, efficiency can be improved and energy consumption can be saved.
[0052] Example 2 A control method for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction, comprising the following steps: (The subsequent examples are added to support the raw materials used for the ferrosilicon reducing agent in the claims)
[0053] S1: Integrate calcined dolomite powder, fluorite and silicon-based ferroalloy into a perforated plate 9 for standby use;
[0054] It should be noted that the particle size and particle size distribution should be reasonable, and the agglomeration pressure should also be reasonably controlled. Because it is dry pressing, no adhesive is allowed to be added, and the finished agglomerate must have a certain compressive strength and appropriate density. Too high a density (that is, the agglomerate is too dense) affects the smooth (diffusion) escape of the reduced gaseous magnesium; too low a density (that is, the agglomerate is not dense enough) not only affects the effective contact between the reactant particles and the reduction effect, but also affects the agglomerate strength (easy to break); and the shape and size of the raw materials are selected and designed with the fundamental purpose of facilitating the reduction reaction, shortening the reduction time as much as possible, and increasing the magnesium production of a single tank; the role of the hole is to allow the plasma torch to extend into the hole, "ignite" the boundary material, promote the self-propagating reaction, and do a good job of sealing and drying;
[0055] S2: After closing all valves in the device, evacuate, then open the primary feed vacuum valve 7 to add the perforated sheet material 9 from the feed port 8 to the storage bin 16, close the primary feed vacuum valve 7, and after the storage bin 16 is evacuated to the vacuum degree consistent with that in the reaction zone, open the secondary feed vacuum valve 6 and the upper control valve 5 to bring the perforated sheet material 9 into the reaction zone, and close the upper control valve 5;
[0056] It should be noted that in order to ensure continuous operation, the furnace must be kept in a vacuum state for a long time;
[0057] S3: According to the amount of magnesium vapor theoretically obtained in the reaction zone, a corresponding number of magnesium crystallizers are assembled in the crystallization zone 13, the vacuum pumping system of the crystallization zone 13 is turned on, and then the magnesium outlet vacuum valve 11 is opened;
[0058] S4: Setting the current intensity and voltage of the power supply system 21 so that the power of the arc plasma generator 4 reaches 18Kw, obtaining a stable plasma torch whose length exceeds that of the perforated sheet 9. Under the interaction of the plasma torch and the self-propagating reaction, the perforated sheet 9 starts to self-propagate from the hole to the inside, thereby ensuring the full reaction. At the same time, the thermal insulation layer 15 can keep the magnesium in a vapor state, further reducing the power loss;
[0059] S5: The magnesium vapor generated by the reaction is gathered toward the crystallization area 13 under the joint action of the plasma torch and the vacuum pumping system of the crystallization area 13. After the magnesium vapor is collected, the magnesium outlet vacuum valve 11 is closed, and the lower control valve 10 is opened to discharge the residue in the reaction area. At the same time, the first-level slag discharge vacuum valve 1 and the second-level slag discharge vacuum valve 2 are opened to discharge the cold slag into the cold slag bin 1;
[0060] S6: After the magnesium vapor collected in the crystallization zone 13 is cooled and crystallized in the magnesium crystallizer, the magnesium crystallizer is taken out to obtain the final product.
[0061] It should be noted that when discharging the residue, the temperature in the reaction zone is kept constant and the above steps are repeated, so that continuous operation can be carried out, efficiency can be improved and energy consumption can be saved.
[0062] Embodiment 3 A control method for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction comprises the following steps:
[0063] S1: Integrate calcined dolomite powder, fluorite and calcium silicate into a perforated plate 9 for standby use;
[0064] It should be noted that the particle size and particle size distribution should be reasonable, and the agglomeration pressure should also be reasonably controlled. Because it is dry pressing, no adhesive is allowed to be added, and the finished agglomerate must have a certain compressive strength and appropriate density. Too high a density (that is, the agglomerate is too dense) affects the smooth (diffusion) escape of the reduced gaseous magnesium; too low a density (that is, the agglomerate is not dense enough) not only affects the effective contact between the reactant particles and the reduction effect, but also affects the agglomerate strength (easy to break); and the shape and size of the raw materials are selected and designed with the fundamental purpose of facilitating the reduction reaction, shortening the reduction time as much as possible, and increasing the magnesium production of a single tank; the role of the hole is to allow the plasma torch to extend into the hole, "ignite" the boundary material, promote the self-propagating reaction, and do a good job of sealing and drying;
[0065] S2: After closing all valves in the device, evacuate, then open the primary feed vacuum valve 7 to add the perforated sheet material 9 from the feed port 8 to the storage bin 16, close the primary feed vacuum valve 7, and after the storage bin 16 is evacuated to the vacuum degree consistent with that in the reaction zone, open the secondary feed vacuum valve 6 and the upper control valve 5 to bring the perforated sheet material 9 into the reaction zone, and close the upper control valve 5;
[0066] It should be noted that in order to ensure continuous operation, the furnace must be kept in a vacuum state for a long time;
[0067] S3: According to the amount of magnesium vapor theoretically obtained in the reaction zone, a corresponding number of magnesium crystallizers are assembled in the crystallization zone 13, the vacuum pumping system of the crystallization zone 13 is turned on, and then the magnesium outlet vacuum valve 11 is opened;
[0068] S4: Setting the current intensity and voltage of the power supply system 21 so that the power of the arc plasma generator 4 reaches 22Kw, obtaining a stable plasma torch whose length exceeds that of the perforated sheet 9. Under the interaction of the plasma torch and the self-propagating reaction, the perforated sheet 9 starts to self-propagate from the hole to the inside, thereby ensuring the full reaction. At the same time, the thermal insulation layer 15 can keep the magnesium in a vapor state, further reducing the power loss;
[0069] S5: The magnesium vapor generated by the reaction is gathered toward the crystallization area 13 under the joint action of the plasma torch and the vacuum pumping system of the crystallization area 13. After the magnesium vapor is collected, the magnesium outlet vacuum valve 11 is closed, and the lower control valve 10 is opened to discharge the residue in the reaction area. At the same time, the first-level slag discharge vacuum valve 1 and the second-level slag discharge vacuum valve 2 are opened to discharge the cold slag into the cold slag bin 1;
[0070] S6: After the magnesium vapor collected in the crystallization zone 13 is cooled and crystallized in the magnesium crystallizer, the magnesium crystallizer is taken out to obtain the final product.
[0071] It should be noted that when discharging the residue, the temperature in the reaction zone is kept constant and the above steps are repeated, so that continuous operation can be carried out, efficiency can be improved and energy consumption can be saved.
[0072] Embodiment 4 A control method for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction comprises the following steps:
[0073] S1: Integrate calcined dolomite powder, fluorite and silicon aluminum into a perforated plate 9 for standby use;
[0074] It should be noted that the particle size and particle size distribution should be reasonable, and the agglomeration pressure should also be reasonably controlled. Because it is dry pressing, no adhesive is allowed to be added, and the finished agglomerate must have a certain compressive strength and appropriate density. Too high a density (that is, the agglomerate is too dense) affects the smooth (diffusion) escape of the reduced gaseous magnesium; too low a density (that is, the agglomerate is not dense enough) not only affects the effective contact between the reactant particles and the reduction effect, but also affects the agglomerate strength (easy to break); and the shape and size of the raw materials are selected and designed with the fundamental purpose of facilitating the reduction reaction, shortening the reduction time as much as possible, and increasing the magnesium production of a single tank; the role of the hole is to allow the plasma torch to extend into the hole, "ignite" the boundary material, promote the self-propagating reaction, and do a good job of sealing and drying;
[0075] S2: After closing all valves in the device, evacuate, then open the primary feed vacuum valve 7 to add the perforated sheet material 9 from the feed port 8 to the storage bin 16, close the primary feed vacuum valve 7, and after the storage bin 16 is evacuated to the vacuum degree consistent with that in the reaction zone, open the secondary feed vacuum valve 6 and the upper control valve 5 to bring the perforated sheet material 9 into the reaction zone, and close the upper control valve 5;
[0076] It should be noted that in order to ensure continuous operation, the furnace must be kept in a vacuum state for a long time;
[0077] S3: According to the amount of magnesium vapor theoretically obtained in the reaction zone, a corresponding number of magnesium crystallizers are assembled in the crystallization zone 13, the vacuum pumping system of the crystallization zone 13 is turned on, and then the magnesium outlet vacuum valve 11 is opened;
[0078] S4: Setting the current intensity and voltage of the power supply system 21 so that the power of the arc plasma generator 4 reaches 20Kw, obtaining a stable plasma torch whose length exceeds that of the perforated sheet 9. Under the interaction of the plasma torch and the self-propagating reaction, the perforated sheet 9 starts to self-propagate from the hole to the inside, thereby ensuring the full reaction. At the same time, the thermal insulation layer 15 can keep the magnesium in a vapor state, further reducing the power loss;
[0079] S5: The magnesium vapor generated by the reaction is gathered toward the crystallization area 13 under the joint action of the plasma torch and the vacuum pumping system of the crystallization area 13. After the magnesium vapor is collected, the magnesium outlet vacuum valve 11 is closed, and the lower control valve 10 is opened to discharge the residue in the reaction area. At the same time, the first-level slag discharge vacuum valve 1 and the second-level slag discharge vacuum valve 2 are opened to discharge the cold slag into the cold slag bin 1;
[0080] S6: After the magnesium vapor collected in the crystallization zone 13 is cooled and crystallized in the magnesium crystallizer, the magnesium crystallizer is taken out to obtain the final product.
[0081] It should be noted that when discharging the residue, the temperature in the reaction zone is kept constant and the above steps are repeated, so that continuous operation can be carried out, efficiency can be improved and energy consumption can be saved.
[0082] Embodiment 5 A control method for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction comprises the following steps:
[0083] S1: Integrate calcined dolomite powder, fluorite and silicon-aluminum-iron to form a perforated plate 9 for standby use;
[0084] It should be noted that the particle size and particle size distribution should be reasonable, and the agglomeration pressure should also be reasonably controlled. Because it is dry pressing, no adhesive is allowed to be added, and the finished agglomerate must have a certain compressive strength and appropriate density. Too high a density (that is, the agglomerate is too dense) affects the smooth (diffusion) escape of the reduced gaseous magnesium; too low a density (that is, the agglomerate is not dense enough) not only affects the effective contact between the reactant particles and the reduction effect, but also affects the agglomerate strength (easy to break); and the shape and size of the raw materials are selected and designed with the fundamental purpose of facilitating the reduction reaction, shortening the reduction time as much as possible, and increasing the magnesium production of a single tank; the role of the hole is to allow the plasma torch to extend into the hole, "ignite" the boundary material, promote the self-propagating reaction, and do a good job of sealing and drying;
[0085] S2: After closing all valves in the device, evacuate, then open the primary feed vacuum valve 7 to add the perforated sheet material 9 from the feed port 8 to the storage bin 16, close the primary feed vacuum valve 7, and after the storage bin 16 is evacuated to the vacuum degree consistent with that in the reaction zone, open the secondary feed vacuum valve 6 and the upper control valve 5 to bring the perforated sheet material 9 into the reaction zone, and close the upper control valve 5;
[0086] It should be noted that in order to ensure continuous operation, the furnace must be kept in a vacuum state for a long time;
[0087] S3: According to the amount of magnesium vapor theoretically obtained in the reaction zone, a corresponding number of magnesium crystallizers are assembled in the crystallization zone 13, the vacuum pumping system of the crystallization zone 13 is turned on, and then the magnesium outlet vacuum valve 11 is opened;
[0088] S4: Setting the current intensity and voltage of the power supply system 21 so that the power of the arc plasma generator 4 reaches 19Kw, obtaining a stable plasma torch whose length exceeds that of the perforated sheet 9. Under the interaction of the plasma torch and the self-propagating reaction, the perforated sheet 9 starts to self-propagate from the hole to the inside, thereby ensuring the full reaction. At the same time, the thermal insulation layer 15 can keep the magnesium in a vapor state, further reducing the power loss;
[0089] S5: The magnesium vapor generated by the reaction is gathered toward the crystallization area 13 under the joint action of the plasma torch and the vacuum pumping system of the crystallization area 13. After the magnesium vapor is collected, the magnesium outlet vacuum valve 11 is closed, and the lower control valve 10 is opened to discharge the residue in the reaction area. At the same time, the first-level slag discharge vacuum valve 1 and the second-level slag discharge vacuum valve 2 are opened to discharge the cold slag into the cold slag bin 1;
[0090] S6: After the magnesium vapor collected in the crystallization zone 13 is cooled and crystallized in the magnesium crystallizer, the magnesium crystallizer is taken out to obtain the final product.
[0091] It should be noted that when discharging the residue, the temperature in the reaction zone is kept constant and the above steps are repeated, so that continuous operation can be carried out, efficiency can be improved and energy consumption can be saved.
[0092] Embodiment 6 A control method for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction comprises the following steps:
[0093] S1: Integrate calcined dolomite powder, fluorite and silicon-calcium-iron to form a perforated plate 9 for standby use;
[0094] It should be noted that the particle size and particle size distribution should be reasonable, and the agglomeration pressure should also be reasonably controlled. Because it is dry pressing, no adhesive is allowed to be added, and the finished agglomerate must have a certain compressive strength and appropriate density. Too high a density (that is, the agglomerate is too dense) affects the smooth (diffusion) escape of the reduced gaseous magnesium; too low a density (that is, the agglomerate is not dense enough) not only affects the effective contact between the reactant particles and the reduction effect, but also affects the agglomerate strength (easy to break); and the shape and size of the raw materials are selected and designed with the fundamental purpose of facilitating the reduction reaction, shortening the reduction time as much as possible, and increasing the magnesium production of a single tank; the role of the hole is to allow the plasma torch to extend into the hole, "ignite" the boundary material, promote the self-propagating reaction, and do a good job of sealing and drying;
[0095] S2: After closing all valves in the device, evacuate, then open the primary feed vacuum valve 7 to add the perforated sheet material 9 from the feed port 8 to the storage bin 16, close the primary feed vacuum valve 7, and after the storage bin 16 is evacuated to the vacuum degree consistent with that in the reaction zone, open the secondary feed vacuum valve 6 and the upper control valve 5 to bring the perforated sheet material 9 into the reaction zone, and close the upper control valve 5;
[0096] It should be noted that in order to ensure continuous operation, the furnace must be kept in a vacuum state for a long time;
[0097] S3: According to the amount of magnesium vapor theoretically obtained in the reaction zone, a corresponding number of magnesium crystallizers are assembled in the crystallization zone 13, the vacuum pumping system of the crystallization zone 13 is turned on, and then the magnesium outlet vacuum valve 11 is opened;
[0098] S4: Setting the current intensity and voltage of the power supply system 21 so that the power of the arc plasma generator 4 reaches 21Kw, obtaining a stable plasma torch whose length exceeds that of the perforated sheet 9. Under the interaction of the plasma torch and the self-propagating reaction, the perforated sheet 9 starts to self-propagate from the hole to the inside, thereby ensuring the full reaction. At the same time, the thermal insulation layer 15 can keep the magnesium in a vapor state, further reducing the power loss;
[0099] S5: The magnesium vapor generated by the reaction is gathered toward the crystallization area 13 under the joint action of the plasma torch and the vacuum pumping system of the crystallization area 13. After the magnesium vapor is collected, the magnesium outlet vacuum valve 11 is closed, and the lower control valve 10 is opened to discharge the residue in the reaction area. At the same time, the first-level slag discharge vacuum valve 1 and the second-level slag discharge vacuum valve 2 are opened to discharge the cold slag into the cold slag bin 1;
[0100] S6: After the magnesium vapor collected in the crystallization zone 13 is cooled and crystallized in the magnesium crystallizer, the magnesium crystallizer is taken out to obtain the final product.
[0101] It should be noted that when discharging the residue, the temperature in the reaction zone is kept constant and the above steps are repeated, so that continuous operation can be carried out, efficiency can be improved and energy consumption can be saved.
[0102] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An arc plasma assisted heat enhanced self-propagating magnesium reduction reaction device, characterized in that: The invention comprises a vertical vacuum furnace body which is composed of a furnace shell (14) and a heat-insulating layer (15) and a refractory layer arranged in the furnace shell (14). The furnace body is provided with a cold slag bin (1), a secondary slag unloading vacuum valve (2), a primary slag unloading vacuum valve (3), a lower control valve (10), an upper control valve (5), a secondary feeding vacuum valve (6), a storage bin (16), a primary feeding vacuum valve (7) and a feeding port (8) from bottom to top. A reaction zone is formed for placing a honeycomb perforated plate material (9) made of calcined dolomite powder, fluorite and ferrosilicon reducing agent. An arc plasma generator (4) for generating a plasma torch connected to the reaction zone is arranged on one side of the reaction zone. One or more crystallization zones (13) for collecting magnesium vapor are arranged on the other side of the reaction zone and connected to the reaction zone through a magnesium outlet vacuum valve (11). A plurality of magnesium crystallizers for crystallizing the vapor are installed in the crystallization zone (13).
2. The arc plasma assisted heat enhanced self-propagating magnesium reduction reaction device according to claim 1, characterized in that: The arc plasma generator (4) comprises an air inlet (17) and an air outlet (18) opened on the side. A power supply system (21) is arranged inside the arc plasma generator (4). The power supply system (21) is respectively connected to the cathode (19) and the dual anode (20) on the side close to the reaction zone.
3. The arc plasma assisted heat enhanced self-propagating magnesium reduction reaction device according to claim 1, characterized in that: The holes of the perforated plate (9) are evenly distributed honeycomb holes, the average distance £ between adjacent holes is equal, £ is (1 / 6-1 / 5)*L, the plate thickness is h=(2-4)L, wherein L is the length of the plate.
4. The arc plasma assisted heat enhanced self-propagating magnesium reduction reaction device according to claim 1, characterized in that: The crystallization zone (13) is externally jacketed with a crystallization zone cold water jacket (12).
5. The arc plasma assisted heat enhanced self-propagating magnesium reduction reaction device according to claim 1, characterized in that: The cold slag bin (1) is externally provided with a cooling water jacket.
6. A control method for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction based on the reaction device according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: Integrate calcined dolomite powder, fluorite and ferrosilicon reducing agent into a perforated plate (9) for standby use; S2: placing the perforated plate (9) into the reaction zone through the feed port (8), then closing all valves in the device and ensuring that the interior of the vertical vacuum furnace is in the same vacuum state; S3: Open the vacuum system of the crystallization zone (13), and then open the magnesium outlet vacuum valve (11); S4: setting the current intensity and voltage of the power supply system (21) so that the power of the arc plasma generator (4) reaches 18 to 22 kW, obtaining a stable plasma torch whose length exceeds the length of the perforated sheet (9), and the perforated sheet (9) fully reacts under the interaction of the plasma torch and the self-propagating reaction; S5: The magnesium vapor generated by the reaction is gathered toward the crystallization zone (13) under the joint action of the plasma torch and the vacuum pumping system of the crystallization zone (13). After the magnesium vapor is collected, the magnesium outlet vacuum valve (11) is closed, and the lower control valve (10) is opened to discharge the residue in the reaction zone. At the same time, the first slag discharge vacuum valve (1) and the second slag discharge vacuum valve (2) are opened to discharge the cold slag into the cold slag bin (1); S6: After the magnesium vapor collected in the crystallization zone (13) is cooled and crystallized in a magnesium crystallizer, the magnesium crystallizer is taken out to obtain the final product.
7. The control method for arc plasma assisted heat-enhanced self-propagating magnesium reduction reaction according to claim 6, characterized in that: The ferrosilicon reducing agent is one of metallic silicon, silicon-based ferroalloy, calcium silicon, aluminum silicon, aluminum silicon iron, and calcium silicon iron.
Citation Information
Patent Citations
Induction heating continuous magnesium-smelting system and continuous magnesium-smelting technique
CN101157989A
Double-dip pipe ferrosilicon bath vacuum circular flow magnesium-smelting device and method thereof
CN101906544A
Improved pidgeon-process magnesium refining process
CN103602833A
Metallurgy device and method for thermally reducing magnesium without silicon carbide
CN114293014A
Improved Pidgeon process magnesium smelting production process
CN114892026A
Cited By
Magnesium-containing conductive raw material and preparation method thereof, and method for smelting magnesium by arc plasma reinforced molten pool reduction
CN122706977A