Leaching separation method for valuable metal of lithium cobalt oxide positive electrode material
By preparing a mixture of ternary deep eutectic solvent and lithium cobalt oxide cathode material, high selectivity and high leaching rate separation and recovery of valuable metals in lithium cobalt oxide batteries are achieved, solving the problems of low separation efficiency and pollution in the existing technology. , providing a green and environmentally friendly recycling solution.
Patent Information
- Application Number
- CN202411047947.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing technology cannot separate and recover valuable metals in lithium cobalt oxide batteries with high selectivity and high leaching rate. Moreover, traditional hydrometallurgy pollutes the environment and has low organic acid leaching efficiency, making it difficult to selectively separate multiple metals.
A ternary deep eutectic solvent is prepared by mixing a hydrogen bond acceptor, a hydrogen bond donor and an auxiliary ligand, mixed with the lithium cobalt oxide cathode material, and the lithium-containing leachate and cobalt-containing precipitate are obtained through solid-liquid separation, and are converted into Cobalt oxalate dihydrate solid achieves highly selective separation and recovery of valuable metals in lithium cobalt oxide cathode materials.
It achieves high selectivity and high leaching rate separation and recovery of valuable metals in lithium cobalt oxide cathode materials. The process is simple, environmentally friendly, and does not require a precipitant, which improves the efficiency and purity of waste lithium battery recycling.
Smart Images

Figure CN118773443A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a method for leaching and separating valuable metals from a lithium cobalt oxide positive electrode material. Background Art
[0002] In recent years, the rapid development of mobile equipment industries such as electric vehicles has led to a rapid increase in the demand and production capacity of lithium batteries. However, due to the limited cycle life of lithium-ion batteries, the generation of waste lithium-ion batteries has increased sharply. Waste lithium-ion batteries have outstanding resource characteristics and are rich in metal elements such as lithium (Li), cobalt (Co), nickel (Ni), manganese (Mn) and copper (Cu). Therefore, waste lithium-ion batteries are important valuable metal deposits. If they are not recycled, it will cause serious waste of resources. In addition, improper handling and large-scale consumption of resources such as Ni, Mn, and Co will also cause environmental pollution. Therefore, efficient and clean recovery of various valuable metals in waste lithium-ion batteries has become an urgent issue.
[0003] At present, the main recycling processes for waste lithium-ion batteries are pyrometallurgy, hydrometallurgy and biometallurgy. Hydrometallurgy is currently the most widely used technology for recovering valuable metals. However, traditional hydrometallurgy mainly relies on inorganic acids and organic acids to leach metal oxides, in which the inorganic acid leaching process not only pollutes the environment, but also causes strong corrosion to the equipment. Although organic acid leaching is less corrosive to equipment, its leaching efficiency is low, and it is difficult to achieve selective separation and leaching of multiple metals, resulting in complicated metal separation and treatment processes and low purity for subsequent recovery. Compared with the above methods, the method of using low eutectic solvents to selectively leach and separate the valuable metals in the positive electrode materials of waste lithium batteries is greener and cleaner and has better application prospects.
[0004] CN117821772A discloses a method for selectively leaching valuable metals from waste ternary lithium battery positive electrode materials using amino sugar eutectic solvents. The method uses a eutectic solvent prepared from betaine hydrochloride and D-glucosamine hydrochloride to selectively leach valuable metals from waste ternary lithium battery positive electrode materials. The method can efficiently leach lithium, nickel, cobalt, and manganese from waste ternary lithium battery NCM622. However, this method does not involve the recovery of valuable metals in waste ternary lithium battery NCM622 positive electrode materials. CN115522057A discloses a method for selectively leaching and separating transition metals from waste ternary lithium battery positive electrode materials using a eutectic solvent. The method uses a eutectic solvent prepared from malonic acid, choline chloride, and deionized water to selectively leach three valuable metals of lithium, cobalt, and manganese from waste ternary lithium battery positive electrode materials. However, the method does not effectively recover the valuable metal nickel in the ternary lithium battery positive electrode materials.
[0005] Therefore, there is an urgent need to develop a highly selective, simple to recover, high leaching rate, green and environmentally friendly method to selectively leach and separate the valuable metals in waste lithium batteries. Summary of the invention
[0006] The main purpose of the present invention is to provide a method for leaching and separating valuable metals in lithium cobalt oxide positive electrode materials to solve the problem that the valuable metals in lithium cobalt oxide batteries cannot be separated and recovered with high selectivity and high leaching rate in the prior art.
[0007] In order to achieve the above object, according to one aspect of the present invention, a method for leaching and separating valuable metals of a lithium cobalt oxide positive electrode material is provided, the method comprising the following steps:
[0008] Step S1: mixing a hydrogen bond acceptor, a hydrogen bond donor and an auxiliary ligand and heating I to obtain a ternary deep eutectic solvent;
[0009] Wherein, the hydrogen bond donor is oxalic acid, the auxiliary ligand is ethylene glycol, and the hydrogen bond acceptor is selected from one or more of betaine hydrochloride, choline chloride, tetramethylammonium chloride and tetrabutylammonium chloride;
[0010] Step S2: mixing the ternary deep eutectic solvent and the lithium cobalt oxide positive electrode active material and heating II to obtain a leaching product;
[0011] Step S3: performing solid-liquid separation on the leached product to obtain a lithium-containing leaching solution and a cobalt-containing precipitate;
[0012] Step S4: mixing the cobalt-containing precipitate with water, filtering, washing and drying to obtain cobalt oxalate dihydrate solid.
[0013] Furthermore, in step S1, the molar ratio of the hydrogen bond acceptor, the hydrogen bond donor and the auxiliary ligand is 1:(1-3):(3-20).
[0014] Furthermore, in step S1, the hydrogen bond donor is oxalic acid, the auxiliary ligand is ethylene glycol, and the hydrogen bond acceptor is selected from tetramethylammonium chloride and / or tetrabutylammonium chloride; the molar ratio of tetramethylammonium chloride and / or tetrabutylammonium chloride, oxalic acid, and ethylene glycol is 1:(1-3):(4-6).
[0015] Furthermore, in step S1, the hydrogen bond donor is oxalic acid, the auxiliary ligand is ethylene glycol, and the hydrogen bond acceptor is selected from betaine hydrochloride; the molar ratio of betaine hydrochloride, oxalic acid, and ethylene glycol is 1:(1-2):(15-20).
[0016] Furthermore, in step S1, the hydrogen bond donor is oxalic acid, the auxiliary ligand is ethylene glycol, and the hydrogen bond acceptor is selected from choline chloride; the molar ratio of choline chloride, oxalic acid, and ethylene glycol is 1:(1-2):(4-8).
[0017] Furthermore, in step S2, the mass ratio of the lithium cobalt oxide positive electrode active material to the ternary deep eutectic solvent is 1:(10-100).
[0018] Furthermore, the mass ratio of the lithium cobalt oxide positive electrode active material to the ternary low eutectic solvent is 1:(40-70).
[0019] Furthermore, in step S4, the water is deionized water; the amount of deionized water used is 30wt% to 60wt% of the cobalt-containing precipitate.
[0020] Furthermore, in step S1, the temperature of heating I is 70°C to 100°C, and the time of heating I is 30 minutes to 3 hours.
[0021] Furthermore, the temperature of heating I is 80° C. to 90° C., and the time of heating I is 1 h to 2 h.
[0022] Furthermore, in step S2, the temperature of heating II is 30°C to 130°C, and the time of heating II is 2 to 12 hours.
[0023] Furthermore, the temperature of heating II is 80° C. to 120° C., and the time of heating II is 4 to 10 hours.
[0024] Furthermore, the temperature of the heating II is 90° C. to 120° C., and the time of the heating II is 6 to 10 hours.
[0025] Furthermore, the temperature of the heating II is 100° C. to 120° C., and the time of the heating II is 6 to 10 hours.
[0026] Furthermore, in step S1, the lithium cobalt oxide positive electrode active material is in powder form.
[0027] Furthermore, heating I is performed by oil bath heating.
[0028] Furthermore, in step S3, centrifugal solid-liquid separation is adopted, and the centrifugal speed is 8000-10000 rpm.
[0029] By applying the technical solution of the present invention, a method for selectively leaching, separating and recovering valuable metals in lithium cobalt oxide positive electrode materials by using a ternary low eutectic solvent is provided. The method can highly selectively leach valuable metals in waste lithium battery positive electrode materials, has a simple process and a high leaching rate. In addition, the present invention can achieve the recovery of valuable metal Co in lithium cobalt oxide positive electrode materials by introducing solvent water, without the need for a precipitant, thereby achieving highly selective separation and recovery of valuable metals in lithium cobalt oxide positive electrode materials. The method of the present invention has the advantages of high selectivity, high leaching rate, and environmental friendliness, and provides a new idea for the recycling scheme in the field of waste lithium battery recycling, and has a good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0031] Figure 1 The Fourier transform infrared spectrum of the deep eutectic solvent prepared in Example 1 of the present invention is shown;
[0032] Figure 2 The X-ray powder diffraction spectrum of the main product of Co in the process of selective leaching, separation and recovery of valuable metals of lithium cobalt oxide positive electrode material in Example 1 of the present invention is shown;
[0033] Figure 3 A schematic diagram of the process route for separating and recovering valuable metals from lithium cobalt oxide positive electrode materials in Example 1 of the present invention is shown. DETAILED DESCRIPTION
[0034] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0035] In order to improve the high selectivity and high leaching rate of valuable metal separation and recovery of lithium cobalt oxide positive electrode materials, the present invention studies a leaching and separation method of valuable metals of lithium cobalt oxide positive electrode materials, and the method comprises the following steps:
[0036] Step S1: mixing a hydrogen bond acceptor, a hydrogen bond donor and an auxiliary ligand and heating I to obtain a ternary deep eutectic solvent;
[0037] Wherein, the hydrogen bond donor is oxalic acid, the auxiliary ligand is ethylene glycol, and the hydrogen bond acceptor is selected from one or more of betaine hydrochloride, choline chloride, tetramethylammonium chloride and tetrabutylammonium chloride;
[0038] Step S2: mixing the ternary deep eutectic solvent and the lithium cobalt oxide positive electrode active material and heating II to obtain a leaching product;
[0039] Step S3: performing solid-liquid separation on the leached product to obtain a lithium-containing leaching solution and a cobalt-containing precipitate;
[0040] Step S4: mixing the cobalt-containing precipitate with water, filtering, washing and drying to obtain cobalt oxalate dihydrate solid.
[0041] The present invention selects three specific components to prepare a novel ternary low eutectic solvent, which has a very high leaching rate for lithium and cobalt in lithium cobalt oxide positive electrode active materials and a very high selectivity for lithium. Almost all of the lithium is leached into the supernatant, while the solid precipitate is basically all cobalt-containing substances, and the separation effect of lithium and cobalt is very good.
[0042] The above method of the present invention uses an oxalic acid-type ternary low eutectic solvent to highly selectively leach the valuable metal Li in the lithium cobalt oxide positive electrode material without additional consumption of a precipitant, and realizes the recovery of the valuable metal Co in the lithium cobalt oxide positive electrode material by introducing solvent water; the method has a simple process and realizes the one-step highly selective separation and recovery effect of the valuable metals Li and Co in the lithium cobalt oxide positive electrode material.
[0043] In order to prepare a low eutectic solvent with better leaching effect, the present invention optimizes the ratio between the three components of the solvent. With this ratio, the three components can form a low eutectic solvent with better use effect; that is, the molar ratio of the hydrogen bond acceptor, the hydrogen bond donor and the auxiliary ligand is 1: (1-3): (3-20); within this ratio range, the molar ratio of the hydrogen bond acceptor and the hydrogen bond donor is 1: 1, 1: 2 or 1: 3, and the molar ratio of the hydrogen bond acceptor and the auxiliary ligand is 1: 3, 1: 4, 1: 5, 1: 6, 1: 7, 1: 8, 1: 9, 1: 10, 1: 11, 1: 12, 1: 13, 1: 14, 1: 15, 1: 16, 1: 17, 1: 18, 1: 19, 1: 20, any value or any range value between two of them. The low eutectic solvent formed by the three components within the above ratio range can play a better effect of achieving high selectivity and high leaching rate.
[0044] In order to further improve the selectivity and leaching rate of valuable metals in lithium cobalt oxide positive electrode materials, the method of the present invention provides several specific low eutectic solvents formed by different components in different ratios, and these low eutectic solvents have high leaching rates and selectivities for lithium and cobalt in lithium cobalt oxide; for example: the hydrogen bond donor is oxalic acid, the auxiliary ligand is ethylene glycol, and the hydrogen bond acceptor is selected from tetramethylammonium chloride and / or tetrabutylammonium chloride; the molar ratio of tetramethylammonium chloride and / or tetrabutylammonium chloride, oxalic acid, and ethylene glycol is 1:(1-3):(4-6).
[0045] Based on the same considerations, the present invention selects oxalic acid as the hydrogen bond donor, ethylene glycol as the auxiliary ligand, and betaine hydrochloride as the hydrogen bond acceptor; the molar ratio of betaine hydrochloride, oxalic acid, and ethylene glycol is 1:(1-2):(15-20).
[0046] The present invention provides another specific component used in a specific ratio, which has better selectivity for lithium; for example, the hydrogen bond donor is oxalic acid, the auxiliary ligand is ethylene glycol, and the hydrogen bond acceptor is selected from choline chloride; the molar ratio of choline chloride, oxalic acid, and ethylene glycol is 1:(1-2):(4-8).
[0047] In order to fully mix the lithium cobalt oxide positive electrode material and the low eutectic solvent and maximize the leaching effect as much as possible, the mass ratio of the lithium cobalt oxide positive electrode active material and the ternary low eutectic solvent in the method of the present invention is 1: (10-100); in this ratio, the mass ratio of the lithium cobalt oxide positive electrode active material and the ternary low eutectic solvent is selected from any value of 1:10, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100 or any range value between the two.
[0048] In order to improve the above-mentioned optimal leaching effect, the mass ratio of the lithium cobalt oxide positive electrode active material and the ternary low eutectic solvent in the method of the present invention is designed to be 1: (40-70).
[0049] The present invention realizes the recovery of valuable metal Co in the lithium cobalt oxide positive electrode material by introducing solvent water; in order to more fully recover the cobalt-containing precipitate, the weight of the added deionized water is 30wt% to 60wt% of the weight of the cobalt-containing precipitate; within this range, the amount of deionized water can be selected from any value of 30wt%, 40wt%, 50wt%, 60wt% or any range value between the two.
[0050] In the above method of the present invention, the leached product contains lithium and cobalt. After solid-liquid separation, the supernatant is basically all lithium dissolved in the liquid, while the insoluble part is the cobalt-containing precipitate. At this time, there is no need to use the method of adding oxalic acid to form cobalt oxalate precipitate in the prior art, but directly add water (specifically deionized water) to convert the cobalt-containing precipitate into cobalt oxalate dihydrate solid, and wash and dry the solid; at this time, lithium exists in the leachate, and cobalt is in the form of cobalt oxalate dihydrate solid, thereby achieving complete separation and recovery.
[0051] The principle of adding water to the cobalt-containing precipitate to form a cobalt oxalate dihydrate solid in the method of the present invention is that Li exists in the LCO lattice gap, and the leaching of Li is achieved by the weak acidity of oxalic acid; the leaching process of Co mainly relies on the reducing ability of the low eutectic solvent to convert Co 3+ Reduction to Co 2+ , forming metal chloride salt [CoCl4] 2- ; H2O, as a strong ligand, can hydrolyze the cobalt polymer in the precipitate, making Co 2+ Dissolves in water and reacts with H2O to form [Co(H2O)6] 2+ At the same time, due to the addition of water, the acidity of the solution is weakened, resulting in HC2O4 - Ionization occurs, generating C2O4 2- . Ultimately promote the C2O4 2- With [Co(H2O)6] 2+ The reaction generates precipitated cobalt oxalate dihydrate, thereby achieving the purpose of selective separation and recovery.
[0052] Before adding water to the leaching product in the method of the present invention, the cobalt-containing precipitate is a high molecular weight cobalt polymer. It is preliminarily inferred that the polymer compound is a large amount of Co 2+ 、HC2O4 - , Cl - The cobalt oxalate precipitate is not contained in the complex of other ions and cannot be directly extracted; therefore, the present invention hydrolyzes the high molecular weight cobalt polymer by adding water to the cobalt-containing polymer precipitate to make Co 2+ Transfer from the solid phase to the aqueous phase to form a new complex structure with C2O4 2- Combined into cobalt oxalate dihydrate, thereby achieving the purpose of extracting cobalt.
[0053] When preparing a low eutectic solvent according to the present invention, the raw materials are mixed and the low eutectic solvent is obtained by constant temperature heating and stirring, wherein the temperature of heating I is set to 70°C to 100°C, and the time of heating I is 30min to 3h; the temperature of heating I is selected from any value of 70°C, 80°C, 90°C, and 100°C, or a range between any two of them; the time of heating I is selected from any value of 0.5h, 1h, 1.5h, 2h, 2.5h, and 3h, or a range between any two of them.
[0054] In order to achieve the best reaction effect and save energy while controlling temperature and time, a better temperature and time are designed, for example, the temperature of heating I is set to 80°C to 90°C, and the time of heating I is set to 1h to 2h. The present invention adopts this temperature, and the three components are heated and fully mixed to better form a low eutectic solvent.
[0055] In order to further improve the leaching rate of valuable metals in the lithium cobalt oxide positive electrode material, the temperature of heating II in step S2 of the present invention is 30°C to 130°C, and the time of heating II is 2 to 12h; the temperature of heating II is selected from any value of 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C or any range between two thereof; the time of heating II is selected from any value of 2h, 3h, 5h, 7h, 10h, 12h or any range between two thereof.
[0056] In order to achieve the best leaching rate when the lithium cobalt oxide positive electrode material and the low eutectic solvent are mixed, the present invention designs the temperature of heating II to be 80°C to 110°C, and the time of heating II is 4 to 10h. In order to further improve the leaching rate and lithium selectivity, it is preferred that the temperature of heating II is 80°C to 120°C, and the time of heating II is 4 to 10h; more preferably, the temperature of heating II is 90°C to 120°C, and the time of heating II is 6 to 10h; more preferably, the temperature of heating II is 100°C to 120°C, and the time of heating II is 6 to 10h, and the leaching rate and selectivity of Li are the highest at 100°C; because higher temperatures promote the leaching reaction by increasing the kinetic energy of molecules, resulting in an increase in the frequency and energy of collisions between molecules, thereby accelerating the leaching process; and too high a temperature will greatly increase energy consumption. Therefore, the lithium cobalt oxide positive electrode active material and the low eutectic solvent can better achieve the leaching of lithium and cobalt at the above temperature.
[0057] In order to fully and well mix with the low eutectic solvent, the lithium cobalt oxide positive electrode active material in the method of the present invention is in powder form. The positive electrode active material of the lithium cobalt oxide battery mainly comes from waste lithium cobalt oxide batteries. When leaching and separation are performed, the binder, aluminum foil and other materials in the battery positive electrode material can be removed by existing technology to obtain the active material of the positive electrode of the waste lithium cobalt oxide battery, and the lithium and cobalt in the positive electrode active material are extracted, separated and recovered.
[0058] In the present invention, when preparing the low eutectic solvent, heating I is performed by oil bath heating; when performing solid-liquid separation on the leached product, centrifugal separation is performed, and the centrifugal rate is 8000-10000 rpm. The above-mentioned heating I and heating II methods and the solid-liquid separation method can be selected from the prior art by those skilled in the art according to actual needs.
[0059] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0060] In the following examples, the content of valuable metals in the leachate was measured using an inductively coupled plasma atomic emission spectrometer (ICP), and the leaching efficiency (η) of the valuable metals was calculated;
[0061] Calculation formula: η=(C x V / m x )×100%;
[0062] Among them, C x is the metal ion concentration in the leachate;
[0063] V is the volume of the leachate;
[0064] m x is the mass of different metals in LiCoO2 powder;
[0065] In addition, the lithium selectivity term was introduced in the following examples to evaluate the selective leaching ability of oxalate-type ternary DES for lithium;
[0066] Calculation formula:
[0067] Among them, the selectivity of Li is A; η Li and η Co are the leaching efficiencies of Li and Co, respectively.
[0068] The battery powder of the lithium cobalt oxide positive electrode material to be processed in the present invention comes from McLean Co., Ltd.
[0069] The abbreviations of the chemical substances of the present invention are explained as follows:
[0070] Tetramethylammonium chloride TMAC, oxalic acid OA, ethylene glycol EG, deep eutectic solvent DES.
[0071] Example 1
[0072] Method for selectively leaching and separating and recovering valuable metals of lithium cobalt oxide positive electrode materials by ternary deep eutectic solvents Figure 3 The following steps are involved:
[0073] (1) Synthesis of ternary deep eutectic solvent: Tetramethylammonium chloride as a hydrogen bond acceptor, oxalic acid as a hydrogen bond donor, and ethylene glycol as an auxiliary ligand are mixed in a molar ratio of 1:2:4 at room temperature, and heated and stirred in an oil bath at 80°C for 2 h to obtain a clear and transparent solution, which is an oxalic acid-type ternary deep eutectic solvent;
[0074] (2) Valuable metal leaching: Add the battery powder of lithium cobalt oxide positive electrode material into the oxalic acid type ternary deep eutectic solvent prepared in step (1) at a mass ratio of 1:60, and heat and stir at 100° C. for 10 h;
[0075] (3) solid-liquid separation: centrifuging the solution obtained in step (2) at a centrifugal speed of 8000 rpm to obtain a lithium-containing leaching solution and a cobalt-containing precipitate;
[0076] (4) Precipitation of valuable metal Co: The cobalt-containing precipitate obtained in step (3) is added with 60 wt % deionized water, filtered, washed and dried to obtain cobalt oxalate dihydrate solid.
[0077] The following tests were conducted on the method of selectively leaching and separating and recovering valuable metals of lithium cobalt oxide positive electrode materials using a ternary deep eutectic solvent in Example 1: successful verification of the preparation of the deep eutectic solvent DES, detection of lithium and cobalt leaching rates, product composition analysis, etc. The experimental results are as follows: Figure 1 And as shown in Table 1.
[0078] (1) Verification of deep eutectic solvent DES:
[0079] The oxalic acid ternary DES prepared in Example 1 was detected by Fourier transform infrared spectrometer, and the following was obtained after treatment: Figure 1 Before the infrared test, tetramethylammonium chloride, oxalic acid, ethylene glycol and synthesized DES were placed in a 70°C oven and dried for 3 h to remove as much moisture as possible, thereby reducing the impact of moisture on the test results.
[0080] like Figure 1 As shown in the figure, four curves of TMAC, OA, EG and DES were obtained. By comparing the infrared spectra of DES with those of the original components, it can be found that DES retains the original characteristic peaks of each component. At the same time, the stretching vibration peak of the hydroxyl group in DES appears at 3401cm -1 At 3428cm in oxalic acid -1 and 3385cm in ethylene glycol -1 This indicates that intermolecular hydrogen bonds are indeed formed, that is, the oxalic acid-type ternary DES is successfully prepared.
[0081] (2) Lithium and cobalt leaching rate detection: The leaching effect of oxalic acid-type ternary DES on lithium cobalt oxide positive electrode material battery powder in Example 1 of the present invention was tested by inductively coupled plasma emission spectrometry (ICP for short) to obtain the leaching concentration of lithium and cobalt. The leaching rate of oxalic acid-type ternary DES on the valuable metals in the lithium cobalt oxide positive electrode material was finally obtained by calculation; the leaching results of Example 1 are as follows:
[0082] Table 1
[0083]
[0084] The calculated leaching rate of lithium in the supernatant is 95.29%, the leaching rate of cobalt is 2.51%, and the selective leaching capacity of lithium reaches 97.36%.
[0085] (3) Product composition analysis: The product of Example 1 of the present invention was analyzed by X-ray diffractometer (XRD) to obtain the following composition: Figure 2 X-ray diffraction pattern shown. Figure 2 This is the X-ray diffraction pattern of CoC2O4·2H2O obtained in Example 1 of the present invention. It can be seen that the product cobalt oxalate dihydrate is successfully synthesized, and its diffraction peak position corresponds to the standard PDF card, which proves that the method of selectively leaching, separating and recovering valuable metals of lithium cobalt oxide positive electrode materials using a ternary low eutectic solvent has good feasibility.
[0086] Example 2
[0087] (1) Synthesis of ternary deep eutectic solvent: Tetramethylammonium chloride as a hydrogen bond acceptor, oxalic acid as a hydrogen bond donor, and ethylene glycol as an auxiliary ligand are mixed at a molar ratio of 1:2:4 at room temperature, and heated and stirred at 80°C in an oil bath for 2 h to obtain a clear and transparent solution, which is an oxalic acid-type ternary deep eutectic solvent;
[0088] (2) Valuable metal leaching: Add the battery powder of lithium cobalt oxide positive electrode material into the oxalic acid type ternary deep eutectic solvent prepared in step (1) at a mass ratio of 1:50, and heat and stir at 100° C. for 10 h;
[0089] (3) solid-liquid separation: centrifuge the solution obtained in step (2) at a centrifugal speed of 8000 rpm;
[0090] (4) Precipitation of valuable metal Co: The cobalt-containing precipitate obtained in step (3) is added with 60 wt % deionized water, filtered, washed and dried to obtain cobalt oxalate dihydrate solid.
[0091] (5) The lithium and cobalt contents of the leaching solution obtained by centrifugation were determined. The test results are shown in Table 2.
[0092] Table 2
[0093]
[0094] The calculated leaching rate of lithium is 91.36%, the leaching rate of cobalt is 4%, and the selective leaching capacity of lithium reaches 95.63%.
[0095] Example 3
[0096] (1) Synthesis of ternary deep eutectic solvent: Tetramethylammonium chloride as a hydrogen bond acceptor, oxalic acid as a hydrogen bond donor, and ethylene glycol as an auxiliary ligand are mixed at a molar ratio of 1:2:4 at room temperature, and heated and stirred at 80°C in an oil bath for 2 h to obtain a clear and transparent solution, which is an oxalic acid-type ternary deep eutectic solvent;
[0097] (2) Valuable metal leaching: Add the battery powder of lithium cobalt oxide positive electrode material into the oxalic acid type ternary deep eutectic solvent prepared in step (1) at a mass ratio of 1:50, and heat and stir at 80° C. for 10 h;
[0098] (3) solid-liquid separation: centrifuge the solution obtained in step (2) at a centrifugal speed of 8000 rpm;
[0099] (4) Precipitation of valuable metal Co: The cobalt-containing precipitate obtained in step (3) is added with 60 wt % deionized water, filtered, washed and dried to obtain cobalt oxalate dihydrate solid.
[0100] (5) The lithium and cobalt contents of the leaching solution obtained by centrifugation were determined. The test results are shown in Table 3.
[0101] Table 3
[0102]
[0103] The calculated leaching rate of lithium is 72.81%, the leaching rate of cobalt is 24.47%, and the selective leaching capacity of lithium reaches 66.39%.
[0104] Example 4
[0105] (1) Synthesis of ternary deep eutectic solvent: Tetramethylammonium chloride as a hydrogen bond acceptor, oxalic acid as a hydrogen bond donor, and ethylene glycol as an auxiliary ligand are mixed at a molar ratio of 1:2:4 at room temperature, and heated and stirred at 80°C in an oil bath for 2 h to obtain a clear and transparent solution, which is an oxalic acid-type ternary deep eutectic solvent;
[0106] (2) Valuable metal leaching: Add the battery powder of lithium cobalt oxide positive electrode material into the oxalic acid type ternary deep eutectic solvent prepared in step (1) at a mass ratio of 1:40, and heat and stir at 90° C. for 10 h;
[0107] (3) solid-liquid separation: centrifuge the solution obtained in step (2) at a centrifugal speed of 8000 rpm;
[0108] (4) Precipitation of valuable metal Co: Add 60 wt % deionized water to the cobalt-containing precipitate obtained in step (3), filter, wash and dry to obtain cobalt oxalate dihydrate solid;
[0109] (5) The lithium and cobalt contents of the leaching solution obtained by centrifugation were determined. The test results are shown in Table 4.
[0110] Table 4
[0111]
[0112] The calculated leaching rate of lithium is 86.94%, the leaching rate of cobalt is 1.69%, and the selective leaching capacity of lithium reaches 98.05%.
[0113] Example 5
[0114] (1) Synthesis of ternary deep eutectic solvent: Tetramethylammonium chloride as a hydrogen bond acceptor, oxalic acid as a hydrogen bond donor, and ethylene glycol as an auxiliary ligand are mixed at a molar ratio of 1:2:4 at room temperature, and heated and stirred at 80°C in an oil bath for 2 h to obtain a clear and transparent solution, which is an oxalic acid-type ternary deep eutectic solvent;
[0115] (2) Valuable metal leaching: Add the battery powder of lithium cobalt oxide positive electrode material into the oxalic acid type ternary deep eutectic solvent prepared in step (1) at a mass ratio of 1:50, and heat and stir at 110° C. for 10 h;
[0116] (3) solid-liquid separation: centrifuge the solution obtained in step (2) at a centrifugal speed of 8000 rpm;
[0117] (4) Precipitation of valuable metal Co: Add 60 wt % deionized water to the cobalt-containing precipitate obtained in step (3), filter, wash and dry to obtain cobalt oxalate dihydrate solid;
[0118] (5) The lithium and cobalt contents of the leaching solution obtained by centrifugation were determined. The test results are shown in Table 5.
[0119] Table 5
[0120]
[0121] The calculated leaching rate of lithium is 84.89%, the leaching rate of cobalt is 1.06%, and the selective leaching capacity of lithium reaches 98.75%.
[0122] Example 6
[0123] (1) Synthesis of ternary deep eutectic solvent: Betaine hydrochloride as a hydrogen bond acceptor, oxalic acid as a hydrogen bond donor, and ethylene glycol as an auxiliary ligand are mixed at a molar ratio of 1:1:20 at room temperature, and heated and stirred at 90°C in an oil bath for 2 h to obtain a clear and transparent solution, which is an oxalic acid-type ternary deep eutectic solvent;
[0124] (2) Valuable metal leaching: Add the battery powder of lithium cobalt oxide positive electrode material into the oxalic acid type ternary deep eutectic solvent prepared in step (1) at a mass ratio of 1:50, and heat and stir at 100° C. for 8 h;
[0125] (3) solid-liquid separation: centrifuge the solution obtained in step (2) at a centrifugal speed of 8000 rpm;
[0126] (4) Precipitation of valuable metal Co: The cobalt-containing precipitate obtained in step (3) is added with 60 wt % deionized water, filtered, washed and dried to obtain cobalt oxalate dihydrate solid.
[0127] (5) The lithium and cobalt contents of the leaching solution obtained by centrifugation were determined. The test results are shown in Table 6.
[0128] Table 6
[0129]
[0130] The calculated leaching rate of lithium is 30.05%, the leaching rate of cobalt is 0.53%, and the selective leaching capacity of lithium reaches 98.23%.
[0131] Example 7
[0132] (1) Synthesis of ternary deep eutectic solvent: Betaine hydrochloride as a hydrogen bond acceptor, oxalic acid as a hydrogen bond donor, and ethylene glycol as an auxiliary ligand are mixed at a molar ratio of 1:1:15 at room temperature, and heated and stirred in an oil bath at 90°C for 2 h to obtain a clear and transparent solution, which is an oxalic acid-type ternary deep eutectic solvent;
[0133] (2) Valuable metal leaching: Add the battery powder of lithium cobalt oxide positive electrode material into the oxalic acid type ternary deep eutectic solvent prepared in step (1) at a mass ratio of 1:70, and heat and stir at 90° C. for 6 h;
[0134] (3) solid-liquid separation: centrifuge the solution obtained in step (2) at a centrifugal speed of 8000 rpm;
[0135] (4) Precipitation of valuable metal Co: Add 60 wt % deionized water to the cobalt-containing precipitate obtained in step (3), filter, wash and dry to obtain cobalt oxalate dihydrate solid;
[0136] (5) The lithium and cobalt contents of the leaching solution obtained by centrifugation were determined. The test results are shown in Table 7.
[0137] Table 7
[0138]
[0139] The calculated leaching rate of lithium is 73.63%, the leaching rate of cobalt is 1.50%, and the selective leaching capacity of lithium reaches 97.96%.
[0140] Example 8
[0141] (1) Synthesis of ternary deep eutectic solvent: Choline chloride as a hydrogen bond acceptor, oxalic acid as a hydrogen bond donor, and ethylene glycol as an auxiliary ligand are mixed at a molar ratio of 1:1:6 at room temperature, and heated and stirred in an oil bath at 80°C for 1 h to obtain a clear and transparent solution, which is an oxalic acid-type ternary deep eutectic solvent;
[0142] (2) Valuable metal leaching: Add the battery powder of lithium cobalt oxide positive electrode material into the oxalic acid type ternary deep eutectic solvent prepared in step (1) at a mass ratio of 1:60, and heat and stir at 80° C. for 6 h;
[0143] (3) solid-liquid separation: centrifuge the solution obtained in step (2) at a centrifugal speed of 8000 rpm;
[0144] (4) Precipitation of valuable metal Co: The cobalt-containing precipitate obtained in step (3) is added with 60 wt % deionized water, filtered, washed and dried to obtain cobalt oxalate dihydrate solid.
[0145] (5) The lithium and cobalt contents of the leaching solution obtained by centrifugation were determined. The test results are shown in Table 8.
[0146] Table 8
[0147]
[0148] The calculated leaching rate of lithium is 47.97%, the leaching rate of cobalt is 1.56%, and the selective leaching capacity of lithium reaches 96.76%.
[0149] Example 9
[0150] (1) Tetramethylammonium chloride as a hydrogen bond acceptor, oxalic acid as a hydrogen bond donor, and ethylene glycol as an auxiliary ligand are mixed at a molar ratio of 1:2:4 at room temperature, and heated and stirred in an oil bath at 80° C. for 2 h to obtain a clear and transparent solution, which is an oxalic acid-type ternary deep eutectic solvent;
[0151] (2) Valuable metal leaching: Add the battery powder of lithium cobalt oxide positive electrode material into the oxalic acid type ternary deep eutectic solvent prepared in step (1) at a mass ratio of 1:60, and heat and stir at 80° C. for 6 h;
[0152] (3) solid-liquid separation: centrifuge the solution obtained in step (2) at a centrifugal speed of 8000 rpm;
[0153] (4) Precipitation of valuable metal Co: The cobalt-containing precipitate obtained in step (3) is added with 60 wt % deionized water, filtered, washed and dried to obtain cobalt oxalate dihydrate solid.
[0154] (5) The lithium and cobalt contents of the leached solution obtained by centrifugation were determined. Under the above conditions, the leached metal concentration (ppm) of Li in DES was 0.82; the Li leaching rate was 69.59%; the leached metal concentration (ppm) of Co in DES was 3.38; the Co leaching rate was 33.88%; and the Li selectivity was 51.31%.
[0155] Comparative Example 1
[0156] "Recovering Cobalt and Lithium from Waste Lithium Cobalt Oxide Battery Positive Electrode Materials Based on Organic Acid: Ethylene Glycol Low Eutectic Solvent System" discloses a method for extracting and recovering valuable metals from waste lithium cobalt oxide positive electrode materials using maleic acid: ethylene glycol low eutectic solvent; this method has a high leaching efficiency for both Li and Co, but Co and Li do not form precipitation in MA:EG DES, and both exist in the solution in the form of maleate, so oxalic acid needs to be added as a precipitant to recover them; during the recovery process, the different solubility of Co and Li oxalates in the low eutectic solvent is used to separate the two by adding anhydrous oxalic acid in batches. The recovery operation is relatively complex and the process is cumbersome.
[0157] Comparative Example 2
[0158] CN116845408A discloses a method for leaching waste lithium cobalt oxide powder by preparing a low eutectic solvent using choline chloride (ChCl) and lactic acid (LA), and adding water to form a water-based DES. This method is in an oil bath at 90°C for 24 hours, and the leaching rate of Li is only about 80%, and the leaching rate of Co is only about 60%. Under the optimal temperature of 100°C, the oil bath is in an oil bath for 36 hours, and the leaching rates of Li and Co can reach more than 95%, which consumes a lot of energy; considering the leaching efficiency and energy consumption, the effect is not as good as the present invention.
[0159] It can be seen from the test results of Tables 1 to 8 that the leaching rates of lithium in the supernatant of the leached products in Example 1, Example 2, Example 4, and Example 5 are 95.29%, 91.36%, 86.94%, and 84.89%, respectively, and the selectivity of lithium is 97.36%, 95.63%, 98.05%, and 98.75%, respectively. The leaching rate and selectivity for lithium are both high, and the separation effect is better.
[0160] The leaching rates of lithium in the supernatant of the leached products of Example 3 and Example 7 were 72.81% and 73.63%, and the selectivity for lithium was 66.39% and 97.96%, respectively. The leaching rate effect was second best, and the latter had a relatively high selectivity for lithium.
[0161] The leaching rates of lithium in the supernatant of the leached products of Example 6 and Example 8 were 30.05% and 47.97% respectively, and the selectivity for lithium was 98.23% and 96.75%; the leaching rate effect was average, but the selectivity for lithium was high.
[0162] Comparing Example 2 and Example 3, the temperatures for mixed leaching of lithium cobalt oxide and ternary low eutectic solvent in the two schemes are different. In Example 2, heating is heated and stirred at 100°C for 10 hours, and the lithium leaching rate is 91.36%, and the lithium selectivity is 95.63%; in Example 3, heating is heated and stirred at 80°C for 10 hours, and the lithium leaching rate is 72.81%, and the lithium selectivity is 66.39%; it can be seen that in the two methods, due to the difference of 20°C in the heating temperature of the leaching process, the effect on the leaching rate and selectivity of lithium is more obvious, which shows that the temperature has a relatively important influence on improving lithium leaching and lithium selectivity.
[0163] Comparing Example 1 and Example 5, the leaching process temperature of lithium cobalt oxide and the ternary low eutectic solvent in Example 5 of the two schemes is 10°C higher than that in Example 1, and the ratio of the two in Example 5 is 1:50, and the ratio of the two in Example 1 is 1:60; the leaching rate of Example 1 is 95.29%, which is greater than the leaching rate of Example 5, which is 84.89%, but the selectivity of Example 1 for lithium is slightly lower than the selectivity of Example 5 for lithium; the above results show that the heating temperature of the leaching process is not the only factor affecting the leaching rate and selectivity; the ratio of lithium cobalt oxide and the low eutectic solvent also has a significant effect on the leaching rate and selectivity.
[0164] Comparing the ternary low eutectic solvents of Example 2 and Example 6, the hydrogen bond acceptors in the two schemes are different. Example 2 uses tetramethylammonium chloride, oxalic acid and ethylene glycol, and Example 6 uses betaine hydrochloride, oxalic acid and ethylene glycol; the leaching temperature of the two schemes is 100°C; the lithium leaching rate of Example 2 is 91.36%, and the lithium selectivity is 95.63%; the leaching rate of Example 6 is 30.05%, and the lithium selectivity is 98.23%; in terms of the comparison of leaching rates, the ternary low eutectic solvent prepared by using tetramethylammonium chloride, oxalic acid and ethylene glycol selected in Example 2 has a significantly higher leaching effect on lithium and cobalt in lithium cobalt oxide than the leaching effect of betaine hydrochloride with oxalic acid and ethylene glycol in Example 6; the above results show that the component selection of the ternary low eutectic solvent affects the leaching effect of lithium and cobalt in lithium cobalt oxide.
[0165] Comparing Example 6 and Example 7, the low eutectic solvent components are the same, the mixing ratios are slightly different, but the mixing ratios of the lithium cobalt oxide positive electrode active material and the low eutectic solvent are different; the mass ratio of Example 7 is 1:70, the lithium leaching rate is 73.63%, and the lithium selectivity is 97.96%, indicating that during the leaching process, whether the mixing ratio of the positive electrode active material and the solvent is reasonable also affects the lithium leaching rate.
[0166] Comparing Example 3 and Example 8, the leaching temperature is 80° C.; the component of the low eutectic solvent of Example 8 uses choline chloride as a hydrogen bond acceptor, and the leaching rate of lithium in lithium cobalt oxide is 47.97%, which is significantly lower than the leaching rate of lithium in Example 3 of 72.81%. Once again, it is explained that only by selecting a suitable low eutectic solvent component and a reasonable component ratio can a better leaching rate and selectivity be obtained.
[0167] Comparing Example 8 and Example 9, the two have different hydrogen bond acceptors and the same leaching temperature. The lithium leaching rate in Example 9 is greater than the lithium leaching rate in Example 8, but the lithium selectivity in Example 8 is much greater than the lithium selectivity in Example 9. This once again shows that only by selecting a suitable low eutectic solvent component and a reasonable component ratio can a better leaching rate and selectivity be obtained.
[0168] Comparative Examples 1 and 2 are compared with Example 1 of the present invention respectively, and it is found that Comparative Example 1 cannot separate cobalt and lithium in one step, but cobalt and lithium exist in the leachate at the same time, and cobalt is not in a precipitated state at this time, and oxalic acid and cobalt need to be further added to form a cobalt oxalate precipitate to achieve the separation of lithium and cobalt. The method of Comparative Example 1 has an additional step of adding oxalic acid to form a cobalt precipitate, and the operation is relatively cumbersome.
[0169] Comparative Example 2 uses different binary low eutectic solvents to leach active materials such as lithium cobalt oxide. Due to the inappropriate selection of the low eutectic solvent components, the lithium leaching rate is relatively low and the lithium selectivity is also lower than that of the present invention.
[0170] By comparing the results of the above embodiments, it can be seen that the method designed by the present invention can better achieve the separation and recovery of lithium and cobalt in the lithium cobalt oxide positive electrode active material by selecting a suitable and matching low eutectic solvent and reasonable leaching process parameters, and after multi-faceted coordination and matching; and by further optimizing the components of the synergistic low eutectic solvent and the leaching temperature and other factors, a better lithium leaching rate and lithium selectivity can be obtained, such as a lithium leaching rate of more than 90%, a lithium selectivity of more than 90%, and a one-step operation (adding deionized water to the cobalt-containing precipitate to form cobalt oxalate dihydrate) The method of the present invention can achieve the effect of simultaneously separating and recovering lithium and cobalt.
[0171] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for leaching and separating valuable metals from lithium cobalt oxide positive electrode materials, characterized in that: The method comprises the following steps: Step S1: mixing a hydrogen bond acceptor, a hydrogen bond donor and an auxiliary ligand and heating I to obtain a ternary deep eutectic solvent; Wherein, the hydrogen bond donor is oxalic acid, the auxiliary ligand is ethylene glycol, and the hydrogen bond acceptor is selected from one or more of betaine hydrochloride, choline chloride, tetramethylammonium chloride and tetrabutylammonium chloride; Step S2: mixing the ternary deep eutectic solvent and the lithium cobalt oxide positive electrode active material and heating II to obtain a leaching product; Step S3: performing solid-liquid separation on the leached product to obtain a lithium-containing leaching solution and a cobalt-containing precipitate; Step S4: mixing the cobalt-containing precipitate with water, filtering, washing and drying to obtain cobalt oxalate dihydrate solid.
2. The method for leaching and separating valuable metals of lithium cobalt oxide positive electrode material according to claim 1, characterized in that: In step S1, the molar ratio of the hydrogen bond acceptor, the hydrogen bond donor and the auxiliary ligand is 1:(1-3):(3-20).
3. The method for leaching and separating valuable metals of lithium cobalt oxide positive electrode material according to claim 1 or 2, characterized in that: In step S1, the hydrogen bond donor is oxalic acid, the auxiliary ligand is ethylene glycol, and the hydrogen bond acceptor is selected from tetramethylammonium chloride and / or tetrabutylammonium chloride; preferably, the molar ratio of the tetramethylammonium chloride and / or tetrabutylammonium chloride, the oxalic acid, and the ethylene glycol is 1:(1-3):(3-6).
4. The method for leaching and separating valuable metals of lithium cobalt oxide positive electrode materials according to any one of claims 1 to 3, characterized in that: In step S1, the hydrogen bond donor is oxalic acid, the auxiliary ligand is ethylene glycol, and the hydrogen bond acceptor is selected from betaine hydrochloride; preferably, the molar ratio of the betaine hydrochloride, the oxalic acid, and the ethylene glycol is 1:(1-2):(15-20).
5. The method for leaching and separating valuable metals of lithium cobalt oxide positive electrode materials according to any one of claims 1 to 4, characterized in that: In step S1, the hydrogen bond donor is oxalic acid, the auxiliary ligand is ethylene glycol, and the hydrogen bond acceptor is selected from choline chloride; Preferably, the molar ratio of the choline chloride, the oxalic acid and the ethylene glycol is 1:(1-2):(4-8).
6. The method for leaching and separating valuable metals of lithium cobalt oxide positive electrode material according to any one of claims 1 to 5, characterized in that: In step S2, the mass ratio of the lithium cobalt oxide positive electrode active material to the ternary deep eutectic solvent is 1:(10-100); Preferably, the mass ratio of the lithium cobalt oxide positive electrode active material to the ternary deep eutectic solvent is 1:(40-70).
7. The method for leaching and separating valuable metals of lithium cobalt oxide positive electrode materials according to any one of claims 1 to 6, characterized in that: In step S4, the water is deionized water; the amount of the deionized water is 30wt% to 60wt% of the cobalt-containing precipitate.
8. The method for leaching and separating valuable metals of lithium cobalt oxide positive electrode materials according to any one of claims 1 to 7, characterized in that: In step S1, the temperature of the heating I is 70°C to 100°C, and the time of the heating I is 30 minutes to 3 hours; preferably, the temperature of the heating I is 80°C to 90°C, and the time of the heating I is 1 hour to 2 hours.
9. The method for leaching and separating valuable metals of lithium cobalt oxide positive electrode materials according to any one of claims 1 to 8, characterized in that: In step S2, the temperature of heating II is 30°C to 130°C, and the time of heating II is 2 to 12 hours; preferably, the temperature of heating II is 80°C to 120°C, and the time of heating II is 4 to 10 hours; more preferably, the temperature of heating II is 90°C to 120°C, and the time of heating II is 6 to 10 hours; more preferably, the temperature of heating II is 100°C to 120°C, and the time of heating II is 6 to 10 hours.
10. The method for leaching and separating valuable metals of lithium cobalt oxide positive electrode materials according to any one of claims 1 to 9, characterized in that: In step S1, the lithium cobalt oxide positive electrode active material is in powder form; and / or, the heating I is performed by oil bath heating; and / or, in step S3, centrifugal solid-liquid separation is performed at a centrifugal rate of 8000 to 10000 rpm.
Citation Information
Patent Citations
Method for selectively leaching and separating transition metal from waste ternary lithium battery positive electrode material by using deep eutectic solvent
CN115522057A
Method for recycling positive electrode material of waste lithium cobalt oxide battery by using water-based eutectic solvent
CN116845408A
Method for selectively leaching valuable metal from waste ternary lithium battery positive electrode material by using amino sugar eutectic melting
CN117821772A
Cited By
Method for recycling valuable metal from waste lithium battery
CN122081656A