Treatment method for two-stage pressure leaching of low-zinc material
By mixing zinc sulfide concentrate and low-zinc materials and then performing one-stage pressure leaching and neutralization and iron removal treatment, combined with two-stage pressure leaching, and adjusting the liquid-to-solid ratio, the safety liquid problem caused by low-zinc materials in wet zinc smelting is solved. Solve the problem of solid ratio imbalance and realize the continuous and stable operation of the all-wet zinc system and increase the zinc recovery rate.
Patent Information
- Application Number
- CN202410814148.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-15
AI Technical Summary
During the wet zinc refining process, low-zinc materials lead to an imbalance in the safe liquid-to-solid ratio of the two-stage pressurized kettle, which affects continuous and stable operation. The circulation volume of the zinc system increases, the output is limited, and the processing cost increases.
Zinc sulfide concentrate and low-zinc materials are mixed and then subjected to one-stage pressure leaching. After copper precipitation and neutralization iron removal treatment, the two-stage pressure leaching is carried out after mixing. By adjusting the liquid-to-solid ratio and adding lignin and flocculant, ensure The pressurized kettle system is balanced to achieve continuous and stable operation.
The balance of the two-stage pressurized leaching slag liquid is achieved, the zinc recovery rate is increased, the slag zinc loss is reduced, the safe, continuous and stable operation of the full wet zinc smelting system is ensured, and the company's efficiency is improved.
Smart Images

Figure CN118773448A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrometallurgy, and in particular relates to a two-stage pressure leaching method for treating low-zinc materials. Background Art
[0002] Zinc metal is an indispensable strategic metal in the fields of aerospace, transportation, energy industry, etc. Sulfide ore is the main raw material for extracting zinc. At present, more than 85% of the world's zinc sulfide ore is produced by the main wet process of roasting-leaching-purification-electrodeposition. According to the different leaching methods and leaching residue treatment methods, the treatment methods of zinc-containing materials are divided into conventional treatment processes and hot acid leaching processes.
[0003] At present, in the process of hydrometallurgical zinc smelting, due to the low grade of zinc-containing materials, generally the zinc grade is 25-35%. When a large amount of low-zinc materials are added to the two-stage pressure kettle for leaching and recovery, the safe liquid-solid ratio of the two-stage pressure kettle is seriously affected, the balance of pressurized leaching slag liquid is seriously unbalanced, and the two-stage pressure leaching cannot be operated safely, continuously and stably; at the same time, after using low-zinc materials, the zinc content of the pressurized leaching solution in the first stage is low, the circulation volume of the zinc system increases, the output is limited, and the processing cost increases.
[0004] Therefore, how to provide a method for treating low-zinc materials that is conducive to the safe, continuous and stable operation of the full wet zinc system is one of the difficult problems faced in this field. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a two-stage pressure leaching method for treating low-zinc materials.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A two-stage pressure leaching method for treating low-zinc materials, specifically comprising the following steps:
[0008] (1) mixing the zinc sulfide concentrate and the low-zinc material and performing a stage of pressure leaching to obtain a stage of supernatant and a stage of pressure leaching underflow (ore pulp);
[0009] (2) subjecting the supernatant liquid of the first stage to copper precipitation and neutralization and iron removal operations to obtain an iron-removing supernatant liquid and a neutralization and iron-removing oxidized low-zinc material (ore pulp);
[0010] (3) The neutralized iron-deoxidized low-zinc material (ore pulp) and the first-stage pressure leaching underflow (ore pulp) are mixed and then subjected to second-stage pressure leaching to obtain a second-stage supernatant and a second-stage leaching residue.
[0011] Preferably, the zinc content of the zinc sulfide concentrate and the low-zinc material after mixing in step (1) is 42-46%.
[0012] Preferably, the mass ratio of the zinc sulfide concentrate to the low-zinc material is 1:6 to 1:5.
[0013] According to this ratio, the two-stage pressure leaching can operate continuously and stably, making full use of the low-zinc materials stored in the system, recovering valuable metals and improving enterprise efficiency.
[0014] Preferably, the liquid-to-solid ratio of the one-stage pressurized leaching in step (1) is 5.0 to 8.5.
[0015] The slag balance between the first and second stages of the autoclave is adjusted by adjusting the liquid-to-solid ratio, and finally the slag and liquid in the autoclave system are balanced, ensuring the safe, stable and continuous operation of the autoclave.
[0016] Preferably, the one-stage pressure leaching method in step (1) is: after mixing the zinc sulfide concentrate and the low-zinc material, adding lignin for pressure leaching, and then adding a flocculant to separate to obtain a supernatant and a pressure leaching underflow (slurry).
[0017] Preferably,
[0018] 0.35-0.65 kg of lignin (lignin content of 8-12 g / L) is added to one ton of the zinc sulfide concentrate;
[0019] The oxygen pressure of the pressure leaching is 1.2-1.5 MPa, the reaction temperature is 120-160°C, the reaction time is 45-60 min, and the stirring speed is 100-120 r / min;
[0020] 0.1-0.5 kg of flocculant is added to one ton of the zinc sulfide concentrate.
[0021] Preferably, the copper deposition in step (2) is carried out by replacing the copper with iron powder;
[0022] The iron removal operation is to add a neutralizer and an oxidant to react, wherein the neutralizer is zinc roasted sand, high-purity zinc oxide powder, etc., the oxidant is air, oxygen, anode mud, etc., and the reaction conditions are that the solution temperature is controlled at 70-85°C, the stirring speed is 50-75r / min, and the neutralization and iron removal time is 3-5 hours.
[0023] Preferably, the mass ratio of the neutralized iron-removing and oxidized low-zinc material (ore pulp) to the first-stage pressurized leaching underflow (ore pulp) in step (3) is 1:5 to 1:4.
[0024] The secondary leaching of the low-zinc material (ore pulp) after neutralization and de-ironization in a pressure autoclave can increase the zinc leaching rate, reduce the loss of slag zinc, and increase the wet zinc recovery rate by 2-3%.
[0025] The liquid-to-solid ratio of the second-stage pressure leaching in step (3) is 3.8 to 5.0.
[0026] The slag balance between the first and second stages of the autoclave is adjusted by adjusting the liquid-to-solid ratio, and finally the slag and liquid in the autoclave system are balanced, ensuring the safe, stable and continuous operation of the autoclave.
[0027] Preferably, the method of the two-stage pressure leaching in step (3) is: after mixing the neutralized iron-deoxidized low-zinc material (slurry) and the one-stage pressure leaching underflow (slurry), adding lignin and waste electrolyte for pressure leaching, and then adding a flocculant to separate and obtain a two-stage supernatant and a two-stage leaching residue.
[0028] 0.05-0.12 kg of lignin (lignin content of 8-12 g / L) is added to one ton of the first stage pressurized leaching underflow (slurry);
[0029] The oxygen pressure of the pressure leaching is 1.2-1.5 MPa, the reaction temperature is 120-170°C, and the reaction time is 90-150 min;
[0030] 0.1-0.5 kg of flocculant is added to one ton of the first stage pressurized leaching underflow.
[0031] The supernatant from the second stage is returned to the first stage for pressure leaching for utilization.
[0032] The invention provides a method in which low-zinc materials and partially oxidized zinc-containing materials generated after further processing the zinc sulfide concentrate mixed materials on the screen in the zinc system material preparation and slurry mixing process section are sent to the zinc system material preparation section, uniformly configured, slurried and ground with the zinc sulfide concentrate in a certain proportion, and pumped to a first-stage pressure kettle for leaching through a hydraulic diaphragm pump; then, the neutralized, de-ironized and oxidized low-zinc materials (ore pulp) are slurried and uniformly mixed with the first-stage pressurized leaching underflow (ore pulp), and then continuously transported to a second-stage pressurized leaching kettle for leaching through a hydraulic diaphragm pump; through the above stages, a two-stage pressurized leaching full wet zinc smelting process is realized to further recover valuable metals such as zinc, copper, silver, etc., and a two-stage pressurized leaching slag-liquid balance is achieved in the full wet method, and the first-stage pressurized leaching solution is obtained, which contains zinc greater than or equal to 150 g / L, thereby ensuring the safe, continuous and stable operation of the full wet method pressurized leaching zinc smelting system.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The present invention provides a two-stage pressure leaching method for treating low-zinc materials. The present invention adjusts the zinc content of the low-zinc materials and the zinc sulfide concentrate, adjusts the liquid-solid ratio of the first-stage pressure leaching to 5.0-8.5, and adjusts the liquid-solid ratio of the second-stage pressure leaching to 3.8-5.0, and simultaneously obtains a first-stage pressure leaching solution with a zinc content of greater than or equal to 150 g / L, realizes the slag-liquid balance of the two-stage pressure leaching, and ensures the continuous and stable operation of the full-wet zinc smelting system. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0036] Figure 1 The figure is a flow chart of the processing method of the present invention. DETAILED DESCRIPTION
[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Example 1
[0039] like Figure 1 The present invention provides a two-stage pressure leaching method for treating low-zinc materials, comprising the following specific steps:
[0040] (1) After the zinc sulfide concentrate is crushed, configured, and slurried, the slurry is filtered through a vibrating screen, the undersize material is directly ground and leached, and the oversize material is further processed with debris and then sent to the zinc system preparation section for classification and placement. The oxidized zinc-containing materials produced abnormally by the zinc system are simultaneously sent to the zinc system preparation section for classification and placement;
[0041] The low-zinc material and zinc sulfide concentrate are mixed in a certain proportion, and the zinc content of the mixed material is controlled at 42-46%. The uniformly mixed ore is slurried and ground, and then pumped into a pressure autoclave through a pressure pump (oxygen pressure is 1.22MPa, liquid-solid ratio is 6.5, reaction temperature is 125-150°C, reaction time is 55-60min, stirring speed is 120r / min, and 0.50 kg of lignin (lignin content is 0.03677 kg) is added to one ton of zinc sulfide concentrate. After leaching in the slag (10g / L), powdered polyacrylamide (0.3 kg of powdered polyacrylamide is added to one ton of zinc sulfide concentrate) is added for a stage of thickening to obtain a supernatant (the solution contains 8.5g / L acid, 2.8g / L iron, and 152g / L zinc) and a pressurized leaching underflow (slurry) (the slag contains 18% zinc), and the low-zinc material is effectively recovered. The grades of the sulfide low-zinc material and the oxidized low-zinc material are shown in Table 1, and the ore blending ratio and results are shown in Table 2;
[0042] Table 1 Grades of sulfided low-zinc materials and oxidized low-zinc materials
[0043] name Zn(%) Ag(g / t) Pb(%) Fe(%) Cu(%) Sulfide low zinc material 27.22 67 0.69 13.34 0.95 Oxidized low zinc materials 31.12 195 3.55 8.67 1.14
[0044] Table 2 Ore matching scheme
[0045] name Proportion Proportion Zn(%) Ag(%) Cu(%) 1 1.5 15% 48.91 262 0.20 2 1.0 10% 48.80 158 0.97 3 1.5 15% 47.04 157 0.50 4 0.5 5% 47.14 213 1.59 5 1.0 10% 51.36 76 0.59 6 1.0 10% 44.72 232 0.54 7 1.0 10% 49.23 166 0.49 8 1.0 10% 33.66 33 4.13 Oxidized low zinc materials 1.0 10% 27.22 67 0.95 Sulfide low zinc material 0.5 5% 31.12 195 1.14 Mixed material mineral content 10.0 100% 43.80 156 1.01
[0046] (2) subjecting a section of the supernatant to iron powder replacement copper precipitation (iron powder addition amount is 1.1 times of copper content, reaction temperature is 80-85° C., reaction time is 50-55 min), and iron removal operation (air and oxygen are used as oxidants, and zinc roasted sand is used as a neutralizer (1.35 g of neutralizer per gram of acid), reaction time is 3-4 h, and reaction temperature is 80-85° C., to obtain iron-removed supernatant and neutralized iron-removed oxidized low-zinc material (slurry);
[0047] (3) The neutralized iron-deoxidized low-zinc material (slurry) is mixed with the first-stage pressurized leaching bottom flow (slurry) in the form of slurry and then pumped into the second-stage pressure autoclave for leaching (oxygen pressure is 1.22 MPa, liquid-to-solid ratio is 4.2, reaction temperature is 130-155° C., reaction time is 90-150 min, stirring speed is 120 r / min, 0.10 kg of lignin (lignin content is 10 g / L) is added to one ton of the first-stage pressurized leaching bottom flow, and then powdered polyacrylamide is added for second-stage thickening (0.3 kg of powdered polyacrylamide is added to one ton of the first-stage pressurized leaching bottom flow (slurry)), and a second-stage supernatant (solution free acid 32 g / L, iron content 18 g / L, zinc content 92 g / L) and a second-stage leaching slag containing 2.1% insoluble zinc are obtained, and the low-zinc material is effectively recovered, wherein the second-stage supernatant returns to the first-stage pressurized leaching for repeated use.
[0048] Example 2
[0049] like Figure 1 The present invention provides a two-stage pressure leaching method for treating low-zinc materials, comprising the following specific steps:
[0050] (2) After the zinc sulfide concentrate is crushed, configured, and slurried, the slurry is filtered through a vibrating screen, the undersize material is directly ground and leached, and the oversize material is further processed with debris and then sent to the zinc system preparation section for classification and placement. The oxidized zinc-containing materials produced abnormally by the zinc system are simultaneously sent to the zinc system preparation section for classification and placement;
[0051] The low-zinc material and zinc sulfide concentrate are mixed in a certain proportion, and the zinc content of the mixed material is controlled at 42-46%. The uniformly mixed ore is slurried and ground, and then pumped into a pressure autoclave through a pressure pump (oxygen pressure is 1.25MPa, liquid-solid ratio is 6.8, reaction temperature is 128-155°C, reaction time is 55-60min, stirring speed is 120r / min, and 0.52kg lignin (lignin content is 1 After leaching in the slag, powdered polyacrylamide (0.28 kg of powdered polyacrylamide is added to one ton of zinc sulfide concentrate) is added for a stage of thickening to obtain a supernatant (the solution contains 6.5 g / L of acid, 2.0 g / L of iron, and 154 g / L of zinc) and a pressurized leaching underflow (slurry) (the slag contains 22% zinc), and the low-zinc material is effectively recovered. The grades of the sulfide low-zinc material and the oxidized low-zinc material are shown in Table 3, and the ore blending ratio and results are shown in Table 4;
[0052] Table 3 Grades of sulfide low zinc materials and oxidized low zinc materials
[0053] name Zn(%) Ag(g / t) Pb(%) Fe(%) Cu(%) Sulfide low zinc material 25.02 30 0.33 13.34 1.28 Oxidized low zinc materials 31.12 195 3.55 8.67 1.14
[0054] Table 4 Ore matching scheme
[0055]
[0056]
[0057] (2) subjecting a section of the supernatant to iron powder replacement copper precipitation (iron powder addition amount is 1.1 times of copper content, reaction temperature is 80-85° C., reaction time is 50-55 min), and iron removal operation (air and oxygen are used as oxidants, and zinc roasted sand is used as a neutralizer (1.35 g of neutralizer per gram of acid), reaction time is 3-4 h, and reaction temperature is 80-85° C., to obtain iron-removed supernatant and neutralized iron-removed oxidized low-zinc material (slurry);
[0058] (3) The neutralized iron-deoxidized low-zinc material (slurry) is mixed with the first-stage pressurized leaching bottom flow (slurry) in the form of slurry and then pumped into the second-stage pressure autoclave for leaching (oxygen pressure of 1.25 MPa, liquid-to-solid ratio of 4.4, reaction temperature of 132-158° C., reaction time of 90-150 min, stirring speed of 120 r / min, 0.10 kg of lignin (lignin content of 10 g / L) is added to one ton of the first-stage pressurized leaching bottom flow (slurry), and then powdered polyacrylamide is added for second-stage thickening (0.25 kg of powdered polyacrylamide is added to one ton of the first-stage pressurized leaching bottom flow (slurry)) to obtain a second-stage supernatant (solution free acid 29 g / L, iron content 15 g / L, zinc content 98 g / L) and a second-stage leaching slag containing 2.3% insoluble zinc, and the low-zinc material is effectively recovered, wherein the second-stage supernatant is returned to the first-stage pressurized leaching for repeated use.
[0059] After the implementation of the present invention, the low-zinc materials stored in the system are put to good use, and the direct recovery rate of zinc by wet method is 94.0-94.5%, which is 2-3% higher than that before the implementation of the invention. The zinc metal is recovered, and there is a significant progress and improvement in economic benefits and production operations.
[0060] The various embodiments are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to in detail.
[0061] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A two-stage pressure leaching method for treating low-zinc materials, characterized in that: The specific steps include: (1) mixing the zinc sulfide concentrate and the low-zinc material and performing a stage of pressure leaching to obtain a stage of supernatant and a stage of pressure leaching underflow; (2) subjecting the first stage supernatant to copper precipitation and neutralization and iron removal operations to obtain an iron-removing supernatant and a neutralization and iron-removing oxidized low-zinc material; (3) The neutralized iron-removed and oxidized low-zinc material is mixed with the first-stage pressure leaching underflow and then subjected to second-stage pressure leaching to obtain a second-stage supernatant and a second-stage leaching residue.
2. A two-stage pressure leaching method for treating low-zinc materials according to claim 1, characterized in that: The zinc content of the zinc sulfide concentrate and the low-zinc material after mixing in step (1) is 42-46%.
3. A two-stage pressure leaching method for treating low-zinc materials according to claim 2, characterized in that: The mass ratio of the zinc sulfide concentrate to the low-zinc material is 1:6 to 1:
5.
4. A two-stage pressure leaching method for treating low-zinc materials according to claim 1, characterized in that: The liquid-to-solid ratio of the one-stage pressure leaching in step (1) is 5.0 to 8.
5.
5. A two-stage pressure leaching method for treating low-zinc materials according to claim 1, characterized in that: The method of the one-stage pressure leaching in step (1) is: after mixing the zinc sulfide concentrate and the low-zinc material, adding lignin for pressure leaching, and then adding a flocculant to separate to obtain a supernatant and a pressure leaching underflow.
6. A two-stage pressure leaching method for treating low-zinc materials according to claim 4, characterized in that: 0.35-0.65 kg of lignin is added to one ton of the zinc sulfide concentrate; The oxygen pressure of the pressure leaching is 1.2-1.5 MPa, the reaction temperature is 120-160°C, the reaction time is 45-60 min, and the stirring speed is 100-120 r / min; 0.1-0.5 kg of flocculant is added to one ton of the zinc sulfide concentrate.
7. A two-stage pressure leaching method for treating low-zinc materials according to claim 1, characterized in that: The copper deposition in step (2) is carried out by replacing the copper deposition with iron powder; The iron removal operation is to add a neutralizer and an oxidant to react, wherein the reaction conditions are: the temperature is controlled at 70-85°C, the stirring speed is 50-75r / min, and the neutralization and iron removal time is 3-5h.
8. A two-stage pressure leaching method for treating low-zinc materials according to claim 1, characterized in that: The mass ratio of the neutralized iron-removing and low-zinc-oxidizing material to the first-stage pressurized leaching underflow in step (3) is 1:5 to 1:4; The liquid-to-solid ratio of the second-stage pressure leaching in step (3) is 3.8 to 5.
0.
9. A two-stage pressure leaching method for treating low-zinc materials according to claim 1, characterized in that: The method of the two-stage pressure leaching in step (3) is: after the neutralized iron-removed and oxidized low-zinc material is mixed with the one-stage pressure leaching underflow, lignin and waste electrolyte are added for pressure leaching, and then a flocculant is added to separate and obtain a two-stage supernatant and a two-stage leaching residue.
10. A two-stage pressure leaching method for treating low-zinc materials according to claim 9, characterized in that: 0.05-0.12 kg of lignin is added to one ton of the first stage pressurized leaching underflow; The oxygen pressure of the pressure leaching is 1.2-1.5 MPa, the reaction temperature is 120-170°C, and the reaction time is 90-150 min; Add 0.1-0.5 kg of flocculant to one ton of the first stage pressurized leaching underflow; The supernatant from the second stage is returned to the first stage for pressure leaching for utilization.