Method for regulating and controlling toughness of tungsten alloy by doping BN and rhenium

By using layered boron nitride as the second phase doping material in tungsten alloy, combined with high-energy ball milling and hot-pressing sintering processes, the problems of insufficient strength and difficult processing of tungsten alloy in high-temperature environments are solved, and the tungsten alloy's It balances high-temperature strength with room-temperature plastic toughness, reduces rhenium resource consumption, and promotes the technological progress of tungsten alloy materials.

CN118773464APending Publication Date: 2024-10-15XI AN JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410834088.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Tungsten alloys have insufficient high-temperature strength in high-temperature environments and are difficult to process. Traditional dispersion strengthening methods cannot take into account room temperature plastic toughness and high-temperature strength at the same time. Moreover, the rhenium element is expensive, and it is uneconomical to increase the rhenium content to make it stronger and tougher.

Method used

Layered boron nitride (BN) is used as the second phase doping material, and a BN-doped tungsten-rhenium alloy with good plastic toughness and high-temperature strength is prepared through powder metallurgy technology and high-energy ball milling combined with hot-pressing sintering process. The layered structure decomposes at high temperatures to form nanosheets and hard particles, which enhance the strength and toughness of the alloy.

Benefits of technology

It achieves dual improvements in the medium and low-temperature processing performance and high-temperature strength performance of tungsten alloy, reduces rhenium resource consumption, solves the common problem of insufficient strength and toughness of tungsten alloy, and improves the material's high-temperature application capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004912662180000011
    Figure HDA0004912662180000011
  • Figure HDA0004912662180000012
    Figure HDA0004912662180000012
  • Figure HDA0004912662180000013
    Figure HDA0004912662180000013
Patent Text Reader

Abstract

The invention discloses a method for regulating and controlling the strength and toughness of a tungsten alloy through BN and rhenium doping, and aims to solve the problems of intrinsic brittleness of the tungsten alloy and high strength and low ductility caused by traditional second-phase dispersion strengthening. According to different requirements on the characteristics of second-phase particles under two temperature conditions of processing and high-temperature service, the second-phase particles are deformable and multiplied in quantity under the action of processing stress, so that stress concentration is reduced, and the toughness of the material is improved; and in a high-temperature environment, a large number of second phases are used as grain boundary or dislocation pinning phases to improve the strength. According to the method, on the basis of the solid solution strengthening tungsten-rhenium alloy, through second-phase BN doping dispersion strengthening and proliferation characteristics of the second-phase BN doping dispersion strengthening in the machining process, double synergy of the good machining characteristic and the high-temperature characteristic of the tungsten alloy is achieved. According to the invention, the problem that the ductility and toughness at room temperature and the high-temperature strength cannot be obtained at the same time in the tungsten alloy is solved, the strengthening and ductility of the tungsten alloy can be obviously improved, and the method is subverted and greatly expanded for the second-phase characteristic requirement of traditional dispersion strengthening.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of material preparation, and in particular relates to a method for regulating the strength and toughness of tungsten alloy by doping with BN and rhenium. Background Art

[0002] Tungsten is the metal with the highest melting point (about 3422℃), with high density, good thermal conductivity and high elastic modulus. Tungsten alloy is an important structural material with excellent properties such as high density, high strength, high hardness and high wear resistance. It is widely used in aerospace, national defense, energy, machinery manufacturing and other fields. However, as a body-centered cubic metal, tungsten has a high ductile-brittle transition temperature and is difficult to process under low temperature pressure. At the same time, as a high-temperature structural material, tungsten alloy faces the problem of insufficient high-temperature strength under high temperature environment. The dispersion strengthening, fine grain strengthening and deformation strengthening methods commonly used in traditional metals have limited ability to regulate the strength and toughness of tungsten alloys. Therefore, the problem of high performance of tungsten alloys has never been completely solved. Due to the existence of the "rhenium effect", tungsten-rhenium alloy has become the common expectation and direction of vigorous development of industry insiders. However, due to the high cost of rhenium metal, it is neither economical nor realistic to strengthen tungsten alloys by simply increasing the rhenium content. Therefore, how to achieve high strength and toughness of tungsten alloys has always been one of the main problems facing the industry.

[0003] Adding fine dispersed second phase particles to the solid solution strengthened W-Re alloy of rhenium element for dispersion strengthening can further improve the high temperature mechanical properties of tungsten-rhenium alloy. At present, the commonly used dispersion strengthening phases are carbides such as titanium carbide (TiC), niobium carbide (NbC), zirconium carbide (ZrC) and oxides such as lanthanum oxide (La2O3), aluminum oxide (Al2O3), and yttrium oxide (Y2O3), which can eventually be prepared into carbide-strengthened tungsten alloy (CDS-W) and oxide-strengthened tungsten alloy (ODS-W). Adding La2O3 and Y2O3 as strengthening phases to tungsten alloys can significantly refine the grains and obtain good performance. Compared with rare earth oxides such as La2O3 and Y2O3, zirconium oxide ceramics and carbides have higher melting points and hardness, and can still maintain good mechanical properties at high temperatures. Carbides will also form solid solutions with tungsten during the sintering process, which can avoid the formation of metastable or low melting point phases and improve the thermodynamic properties of the material. The above second-phase particle doping can improve the strength and mechanical properties of the alloy by refining the grains, but it cannot take into account both room temperature plasticity and toughness. Therefore, it is necessary to consider another second-phase doping material that can achieve both room temperature plasticity and toughness and high temperature strength.

[0004] Chen Yong et al. prepared a tungsten alloy with good strength and density by adding La2O3 and using high-energy ball milling combined with hot isostatic pressing. However, when conducting electron beam thermal shock tests, micro cracks began to appear when the current density reached 3MW / m2. When the current density was further increased to 5MW / m 2, serious melting phenomenon has appeared on the surface, and holes have appeared. It can be seen that although oxides can improve the strength of tungsten-rhenium alloys and reduce their ductile-brittle transition temperature, the high-temperature strength and ablation resistance of oxide-reinforced tungsten-rhenium alloys are low. It is difficult to meet the application requirements under high temperature. To this end, Chen Yong, Wu Yucheng, Yu Fuwen, etc., in response to the current high-temperature strength problems of tungsten-rhenium alloys, conducted a study on the microstructure and properties of La2O3 dispersion-strengthened tungsten alloys (Rare Metal Materials and Engineering, 2007,

[0005] 36(5):3.DOI:10.3321 / j.issn:1002-185X.2007.05.016.) pointed out that it is necessary to consider new ways of doping the second phase to enhance the high temperature strength performance.

[0006] The main mechanism of second phase dispersion strengthening is that it can pin dislocations and grain boundaries, refine grains, and improve the strength of tungsten-rhenium alloys; at the same time, it can increase the grain boundary area, reduce the impurity concentration at the grain boundary, strengthen the grain boundary bonding force, and then reduce the plastic-brittle transition temperature and improve the plasticity of the material. However, although the excessive second phase content helps to improve the high-temperature strength of the material, it also deteriorates the processing plasticity of the material. As a result, the second phase particle dispersion strengthening can only play a role within a certain range. This is the fundamental reason why high-performance tungsten alloys are difficult to prepare. Analysis of the preparation process and service environment of tungsten alloys shows that temperature is the first factor in the service environment. As the temperature increases, the plasticity of the material improves or the grain grows. Therefore, the pinning effect of the second phase is very important. The more the second phase, the more significant the pinning effect, and the better the high-temperature stability of the material; and in the processing process, the magnitude of the processing stress is the main factor in the deformation of the material. The stronger the pinning effect of the second phase, the more difficult the material is to process. Therefore, in the face of two different ambient temperatures and stress conditions, the most ideal second phase should have stability to temperature and compromise to stress. That is to say, it can change phase under the action of external force and is very stable under the action of temperature.

[0007] BN has a melting point of up to 3000℃, which is one of the highest melting points among inorganic materials and has good chemical stability. Layered boron nitride materials can slip between layers under the action of external forces, reducing resistance to external forces and thus reducing the difficulty of material processing. Therefore, it can be used as an ideal second phase material for tungsten alloys.

[0008] BN as a doping phase in metals has attracted extensive academic research. The following are some of the research directions:

[0009] (1) Improve the hardness and strength of metal materials. BN has the characteristics of high hardness and high strength, so it can be introduced into metals to improve the hardness and strength of metal materials, such as stainless steel, tungsten alloy, etc. Studies have shown that doping BN into tungsten alloys can significantly improve their hardness and strength, especially showing good mechanical properties at high temperatures.

[0010] (2) Improve the high temperature resistance of metal materials. BN has high temperature stability and can be used to prepare high temperature materials, such as high temperature alloys and ceramics. Adding it to metals can improve the high temperature resistance of metals.

[0011] (3) Used to prepare composite materials. Composite materials with special properties such as high strength, high toughness, high electrical conductivity, and high thermal conductivity can be prepared by combining BN with metal. Such composite materials have broad application prospects in aerospace, electronics, energy and other fields.

[0012] BN doping can improve the hardness, strength and wear resistance of metals, but it will also affect the ductility of metals. Generally speaking, BN doping will make metals more brittle, thereby reducing their ductility. However, some studies have shown that under appropriate doping conditions, BN doping can improve the ductility of metals. The following are some examples of how BN doping can improve the ductility of metals:

[0013] (1) Steel: Some studies have shown that doping BN into steel can improve its toughness, especially at low temperatures. This is because BN doping can form fine nitride particles, thereby increasing the amount of dispersed phase in the steel, inhibiting grain boundary expansion, and improving the fracture toughness of the material.

[0014] (2) Aluminum alloy: Some studies have shown that adding an appropriate amount of BN to aluminum alloys can improve their toughness. This is because BN doping can refine the grains of aluminum alloys and improve the grain boundary strengthening effect, thereby improving the ductility and toughness of the material.

[0015] In summary, although BN doping has been used in the above-mentioned metal strengthening, the research on its strengthening mechanism is still not in-depth. The performance regulation of tungsten alloys is even less involved. Based on the preparation of tungsten alloy materials and the role of the second phase and its functional requirements in high-temperature service environments, the present invention proposes a method of using layered boron nitride to disperse strengthen tungsten alloys to achieve a win-win goal of improving processing plasticity at low temperatures and improving strength at high temperatures. In order to achieve a technological breakthrough in high-performance tungsten alloy materials. Summary of the invention

[0016] The object of the present invention is to provide a method for regulating the toughness of tungsten alloy by doping with BN and rhenium, that is, by adding BN to a tungsten-rhenium alloy, the alloy has fine grains, uniform and dense structure, good plasticity, toughness and high-temperature strength properties.

[0017] In order to achieve the above object, the technical solution adopted by the present invention is:

[0018] Step 1, tungsten powder and rhenium powder are mixed in a mass ratio of 95-90:5-10, and then loaded into a ball mill, and ball milled under argon protection to obtain a uniformly mixed powder;

[0019] Step 2, adding 0.3% by weight of BN to the uniformly mixed powder, placing the mixture in a ball mill, and performing ball milling under argon protection to obtain a uniformly mixed powder;

[0020] Step 3, ball milling the uniformly mixed powder obtained in step 2 under argon protection to obtain a uniformly mixed powder;

[0021] Step 4: Place the mixed powder into a graphite mold, and then place the graphite mold containing the mixed powder into a vacuum chamber with a degree of vacuum of 5×10 -3 Pa~1×10 -2 The sintering is carried out in a hot pressing furnace of Pa, the sintering temperature is 1400℃~1500℃, the holding time is 3~10min, the applied pressure is 30~50MPa, and the furnace is cooled. The sintered body obtained after demoulding is processed to remove 0.3~0.5mm of the surface layer to obtain BN tungsten-rhenium alloy;

[0022] Step 5, high-temperature rolling the obtained BN tungsten-rhenium alloy at 1100-1800° C. for 4 times, and annealing the rolled product at 1000-1400° C. for 1-3 hours.

[0023] The ball milling in step 1 and step 2 is carried out in a planetary ball mill, the ball mill jar and the grinding balls are made of agate, the ball-to-material ratio is 1:1-2:1, the ball milling time is 6-12h, and the ball mill speed is 300-500r / min.

[0024] The ball milling in step 3 is performed in a planetary ball mill, the ball mill jar and the grinding balls are both made of tungsten carbide, the ball-to-material ratio is 10:1-20:1, the ball milling time is 6-12 hours, and the ball mill speed is 300-500 r / min.

[0025] The present invention first proposes a tungsten-rhenium alloy as a substrate for the realization of high-performance tungsten alloys, and then uses a tungsten-rhenium alloy with a low rhenium content, and then performs BN doping as a second phase. BN is added as a reinforcing phase, and a tungsten-rhenium alloy doped with BN is prepared using powder metallurgy technology. The tungsten alloy strengthening and toughening performance that even high-rhenium alloys cannot achieve is achieved, and the shortage of rhenium resources in my country can be greatly solved. The present invention adopts a tungsten alloy doping scheme to solve the problem that tungsten alloys generally have room temperature plastic toughness and high temperature strength that cannot be achieved at the same time, and achieves the dual synergy of good processing characteristics and high temperature characteristics of tungsten alloys. The layered BN phase is used as the dispersion-strengthened second phase, and the characteristic of its own nano-layered structure that can slide is used to achieve toughening of refractory metal-based alloys, thereby improving the medium and low temperature processing performance of the alloy. At the same time, after the BN phase decomposes at high temperature, a large amount of tungsten boride and oxide hard particles are formed, which hinder dislocation sliding and grain boundary climbing, and enhance the strength of refractory metal-based alloys at high temperatures. Thereby achieving a dual improvement in medium and room temperature plastic toughness and high temperature strength performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a scanning electron microscope image of the sintered sample of Example 1 of the present invention.

[0027] Figure 2 This is a scanning electron microscope of the rolled sample of Example 1 of the present invention.

[0028] Figure 3 The mechanical properties of tungsten metal in the document "Mechanical properties and thermal stability of pure W and W-0.5wt% ZrC alloy manufactured with the same technology" and the tensile behaviors of pure W at different temperatures (a) rolled, (b) 1200℃, (c) 1300℃ and 1600℃ annealed can be used as a reference for the tungsten alloy in this patent.

[0029] Figure 4 These are the high temperature mechanical properties of the gold sample prepared in Example 1 of the present invention.

[0030] Figure 5 yes Figure 1 A magnified picture of the situation. DETAILED DESCRIPTION

[0031] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0032] Embodiment 1:

[0033] Step 1, the mass ratio of tungsten powder to rhenium powder is 90:10; the mixed powder is loaded into a ball mill, argon gas is introduced, and the mixed powder is put into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of agate, the ball-to-material ratio is 1:1, the effective time of ball milling is 12h, and the speed of the ball mill is 300r / min;

[0034] Step 2, adding 0.3% BN to the above-mentioned uniformly mixed powder for ball milling, passing argon gas, and putting it into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of agate, the ball-to-material ratio is 2:1, the effective time of ball milling is 9 hours, and the ball mill speed is 300r / min;

[0035] Step 3, high-energy ball milling the uniformly mixed powder, passing argon gas, and putting it into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of tungsten carbide, the ball-to-material ratio is 10:1, the effective time of ball milling is 12 hours, and the ball mill speed is 300r / min;

[0036] Step 4: Place the mixed powder into a graphite mold with an inner diameter of 30-60 mm, and then place the graphite mold containing the mixed powder into a vacuum chamber with a degree of vacuum of 5×10 -3 The sintering is carried out in a hot pressing furnace of Pa, the sintering temperature is 1400°C, the holding time is 10 min, the applied pressure is 30 MPa, and the furnace is cooled. The sintered body obtained after demoulding is processed to remove 0.3-0.5 mm of the surface layer to obtain BN tungsten-rhenium alloy.

[0037] Step 5, subjecting the obtained alloy to a high temperature rolling process at a temperature of 1100° C. for 4 passes, and then subjecting the obtained product to an annealing treatment at 1000° C. for 3 hours.

[0038] The tungsten alloy structure of the sintered sample of Example 1 was analyzed by scanning electron microscope. Figure 1 In the metallographic structure of the high-density tungsten alloy sintered sample of this embodiment, in addition to tungsten grains, there are also dispersed small black holes in the bonding phase. The holes are caused by the BN particles falling during the scanning sample preparation process. (The holes are not pores, and there is a second phase related to BN in them)

[0039] from Figure 2 It can be seen that the density of the sample prepared in Example 1 is higher after rolling. The density of the tungsten alloy is measured to be 18.8 g / cm 3 .

[0040] from Figure 3It can be seen that the tensile properties of tungsten alloys at different temperatures in the literature are such that the highest strength is 700MPa at 250 degrees Celsius, the lowest strength is less than 500, and the elongation is about 15%.

[0041] from Figure 4 It can be seen that the high temperature strength is generally above 1000MPa, which is a very significant improvement in high temperature performance. This also corresponds to the application background requirement of tungsten alloy as a structural material, which needs to maintain high strength at high temperatures. And the elongation is also maintained at about 10%, with no obvious decrease.

[0042] from Figure 5 It can be seen that there is a second phase structure in the pores, which is also the innovation of the present invention. Its internal structure can explain the mechanism of sample performance improvement. And the result of the second phase energy spectrum point scan, the result includes the composition ratio of the elements in this part, which can show the approximate composition of the second phase)

[0043] The Vickers hardness of the sample prepared by the present invention was tested to be about 500 HV, which proves that the method of the present invention can increase the hardness of tungsten alloy.

[0044] It can be seen from the above that the tungsten alloy of the present invention can maintain high density, not only without much difference in plasticity and toughness, but also shows great superiority in high temperature strength.

[0045] Embodiment 2:

[0046] Step 1, the mass ratio of tungsten powder to rhenium powder is 93:7; the mixed powder is loaded into a ball mill, argon gas is introduced, and the mixed powder is put into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of agate, the ball-to-material ratio is 2:1, the effective time of ball milling is 6 hours, and the speed of the ball mill is 500r / min;

[0047] Step 2, adding 0.3% BN to the above-mentioned uniformly mixed powder for ball milling, passing argon gas, and putting it into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of agate, the ball-to-material ratio is 1:1, the effective time of ball milling is 8h, and the ball mill speed is 500r / min;

[0048] Step 3, high-energy ball milling the uniformly mixed powders, passing argon gas, and putting them into a planetary ball mill for ball milling to obtain uniformly mixed powders. During the ball milling, the ball mill and the grinding balls are both made of tungsten carbide, the ball-to-material ratio is 15:1, the effective time of ball milling is 6 hours, and the ball mill speed is 500 r / min;

[0049] Step 4: Place the mixed powder into a graphite mold with an inner diameter of 30-60 mm, and then place the graphite mold containing the mixed powder into a vacuum chamber with a degree of vacuum of 8×10 -3 The sintering is carried out in a hot pressing furnace of Pa, the sintering temperature is 1480°C, the holding time is 5 min, the applied pressure is 50 MPa, and the furnace is cooled. The sintered body obtained after demoulding is processed to remove 0.3-0.5 mm of the surface layer to obtain BN tungsten-rhenium alloy.

[0050] Step 5, subjecting the obtained alloy to a high temperature rolling process at a temperature of 1500° C. for 4 passes, and then subjecting the obtained product to an annealing treatment at a certain temperature point within a temperature range of 1200° C. for 2 hours.

[0051] Embodiment 3:

[0052] Step 1, the mass ratio of tungsten powder to rhenium powder is 95:5; the mixed powder is loaded into a ball mill, argon gas is introduced, and the mixed powder is put into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of agate, the ball-to-material ratio is 1.5:1, the effective time of ball milling is 9 hours, and the speed of the ball mill is 400r / min;

[0053] Step 2, adding 0.3% BN to the above-mentioned uniformly mixed powder for ball milling, passing argon gas, and putting it into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of agate, the ball-to-material ratio is 1.5:1, the effective time of ball milling is 10 hours, and the ball mill speed is 400r / min;

[0054] Step 3, high-energy ball milling the uniformly mixed powder, passing argon gas, and putting it into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of tungsten carbide, the ball-to-material ratio is 13:1, the effective time of ball milling is 9 hours, and the ball mill speed is 400r / min;

[0055] Step 4: Place the mixed powder into a graphite mold with an inner diameter of 30-60 mm, and then place the graphite mold containing the mixed powder into a vacuum chamber with a degree of vacuum of 6×10 -3 The sintering is carried out in a hot pressing furnace of Pa, the sintering temperature is 1430°C, the holding time is 8 minutes, the applied pressure is 35 MPa, and the furnace is cooled. The sintered body obtained after demoulding is processed to remove 0.3-0.5 mm of the surface layer to obtain BN tungsten-rhenium alloy.

[0056] Step 5, subjecting the obtained alloy to a high temperature rolling process at a temperature of 1200° C. for 4 passes, and then subjecting the obtained product to an annealing treatment at a certain temperature point within a temperature range of 1100° C. for 1 hour.

[0057] Embodiment 4:

[0058] Step 1, the mass ratio of tungsten powder to rhenium powder is 92:8; the mixed powder is loaded into a ball mill, argon gas is introduced, and the mixed powder is put into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of agate, the ball-to-material ratio is 2:1, the effective time of ball milling is 8 hours, and the speed of the ball mill is 500r / min;

[0059] Step 2, adding 0.3% BN to the above-mentioned uniformly mixed powder for ball milling, passing argon gas, and putting it into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of agate, the ball-to-material ratio is 2:1, the effective time of ball milling is 11h, and the ball mill speed is 500r / min;

[0060] Step 3, high-energy ball milling the uniformly mixed powder, passing argon gas, and putting it into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of tungsten carbide, the ball-to-material ratio is 20:1, the effective time of ball milling is 8 hours, and the ball mill speed is 500r / min;

[0061] Step 4: Place the mixed powder into a graphite mold with an inner diameter of 30-60 mm, and then place the graphite mold containing the mixed powder into a vacuum chamber with a vacuum degree of 9×10 -3 The sintering is carried out in a hot pressing furnace of Pa, the sintering temperature is 1500°C, the holding time is 3 minutes, the applied pressure is 45MPa, and the furnace is cooled. The sintered body obtained after demoulding is processed to remove 0.3-0.5mm of the surface layer to obtain BN tungsten-rhenium alloy.

[0062] Step 5, subjecting the obtained alloy to a high temperature rolling process at a temperature of 1600° C. for 4 passes, and then subjecting the obtained product to an annealing treatment at a certain temperature point within a temperature range of 1300° C. for 3 hours.

[0063] Embodiment 5:

[0064] Step 1, the mass ratio of tungsten powder to rhenium powder is 94:6; the mixed powder is loaded into a ball mill, argon gas is introduced, and the mixed powder is put into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of agate, the ball-to-material ratio is 1.5:1, the effective time of ball milling is 10 hours, and the speed of the ball mill is 400r / min;

[0065] Step 2, adding 0.3% BN to the above-mentioned uniformly mixed powder for ball milling, passing argon gas, and putting it into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball milling jar and the grinding balls are both made of agate, the ball-to-material ratio is 1:1, the effective time of ball milling is 12h, and the ball mill speed is 400r / min;

[0066] Step 3, high-energy ball milling the uniformly mixed powders, passing argon gas, and putting them into a planetary ball mill for ball milling to obtain uniformly mixed powders. During the ball milling, the ball mill and the grinding balls are both made of tungsten carbide, the ball-to-material ratio is 16:1, the effective time of ball milling is 10 hours, and the ball mill speed is 400 r / min;

[0067] Step 4: Place the mixed powder into a graphite mold with an inner diameter of 30-60 mm, and then place the graphite mold containing the mixed powder into a vacuum chamber with a vacuum degree of 7×10 -3 The sintering is carried out in a hot pressing furnace of Pa, the sintering temperature is 1450°C, the holding time is 6 minutes, the applied pressure is 40 MPa, and the furnace is cooled. The sintered body obtained after demoulding is processed to remove 0.3-0.5 mm of the surface layer to obtain BN tungsten-rhenium alloy.

[0068] Step 5, subjecting the obtained alloy to a high temperature rolling process at a temperature of 1800° C. for 4 passes, and then subjecting the obtained product to an annealing treatment at a certain temperature point within a temperature range of 1400° C. for 2 hours.

[0069] Embodiment 6:

[0070] Step 1, the mass ratio of tungsten powder to rhenium powder is 91:9; the mixed powder is put into a ball mill, argon gas is introduced, and the mixed powder is put into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of agate, the ball-to-material ratio is 1:1, the effective time of ball milling is 11 hours, and the speed of the ball mill is 300r / min;

[0071] Step 2, adding 0.3% BN to the above-mentioned uniformly mixed powder for ball milling, passing argon gas, and putting it into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of agate, the ball-to-material ratio is 2:1, the effective time of ball milling is 6 hours, and the ball mill speed is 300r / min;

[0072] Step 3, high-energy ball milling the uniformly mixed powder, passing argon gas, and putting it into a planetary ball mill for ball milling to obtain a uniformly mixed powder. During the ball milling, the ball mill and the grinding balls are both made of tungsten carbide, the ball-to-material ratio is 18:1, the effective time of ball milling is 11 hours, and the ball mill speed is 300r / min;

[0073] Step 4: Place the mixed powder into a graphite mold with an inner diameter of 30-60 mm, and then place the graphite mold containing the mixed powder into a vacuum chamber with a degree of vacuum of 1×10 -2 The sintering is carried out in a hot pressing furnace of Pa, the sintering temperature is 1460°C, the holding time is 7 minutes, the applied pressure is 50 MPa, and the furnace is cooled. The sintered body obtained after demoulding is processed to remove 0.3-0.5 mm of the surface layer to obtain BN tungsten-rhenium alloy.

[0074] Step 5, subjecting the obtained alloy to a high temperature rolling process at a temperature of 1700° C. for 4 passes, and then subjecting the obtained product to an annealing treatment at a certain temperature point within a temperature range of 1000° C. for 3 hours.

[0075] The present invention adopts a layered BN phase as the second phase of dispersion strengthening, and utilizes its own layered structure and slip characteristics to achieve toughening of the refractory metal-based tungsten alloy, thereby improving the high-temperature strength performance of the alloy. The layered BN phase partially decomposes during the synthesis process and at high temperatures to form BNNSs (boron nitride nanosheets) and hard boride particles, which hinder dislocation slip and grain boundary climb, and enhance the hardness of the refractory metal-based alloy and its strength at high temperatures.

[0076] The tungsten alloy of the present invention not only has no big gap in plasticity and toughness, but also shows great superiority in high temperature strength; using BN as the second phase, its slippable layered structure is used to enhance the plasticity and toughness of tungsten alloy. Under the action of processing stress, the second phase particles can be deformed and multiplied in number to reduce stress concentration and thus improve the toughness of the material. Under high temperature environment, a large number of second phases act as pinning phases of grain boundaries or dislocations to improve strength; combined with the excellent strengthening and toughening properties of tungsten-rhenium alloy itself, the good processing characteristics and high temperature characteristics of tungsten alloy are achieved. In order to obtain a high-density refractory alloy, the present invention proposes to first use high-energy ball milling to activate the matrix powder, and then combine hot pressing sintering technology to achieve high density of the alloy. The preparation process is simple and highly controllable. Through appropriate second phase doping and sintering process, it is expected to achieve the same strength and toughness improvement as that achieved by common high-rhenium tungsten alloys (Re≥15%) at a low rhenium (Re≦10%) tungsten alloy ratio, which will greatly solve the current shortage of rhenium resources and is of great significance to reducing the waste of expensive rhenium resources, reducing the cost of tungsten alloys, and promoting the technological progress of tungsten alloy materials.

Claims

1. A method for regulating the toughness of tungsten alloy by doping with BN and rhenium, characterized in that The following steps are involved: Step 1, tungsten powder and rhenium powder are mixed in a mass ratio of 95-90:5-10, and then loaded into a ball mill, and ball milled under argon protection to obtain a uniformly mixed powder; Step 2, adding 0.3% by weight of BN to the uniformly mixed powder, placing the mixture in a ball mill, and performing ball milling under argon protection to obtain a uniformly mixed powder; Step 3, ball milling the uniformly mixed powder obtained in step 2 under argon protection to obtain a uniformly mixed powder; Step 4: Place the mixed powder into a graphite mold, and then place the graphite mold containing the mixed powder into a vacuum chamber with a degree of vacuum of 5×10 -3 Pa~1×10 -2 The sintering is carried out in a hot pressing furnace of Pa, the sintering temperature is 1400℃~1500℃, the holding time is 3~10min, the applied pressure is 30~50MPa, and the furnace is cooled. The sintered body obtained after demoulding is processed to remove 0.3~0.5mm of the surface layer to obtain BN tungsten-rhenium alloy; Step 5, high-temperature rolling the obtained BN tungsten-rhenium alloy at 1100-1800° C. for 4 times, and annealing the rolled product at 1000-1400° C. for 1-3 hours.

2. The method for regulating the toughness of tungsten alloy by BN and rhenium doping according to claim 1, characterized in that: The ball milling in step 1 and step 2 is carried out in a planetary ball mill, the ball mill jar and the grinding balls are made of agate, the ball-to-material ratio is 1:1-2:1, the ball milling time is 6-12h, and the ball mill speed is 300-500r / min.

3. The method for regulating the toughness of tungsten alloy by BN and rhenium doping according to claim 1, characterized in that: The ball milling in step 3 is performed in a planetary ball mill, the ball mill jar and the grinding balls are both made of tungsten carbide, the ball-to-material ratio is 10:1-20:1, the ball milling time is 6-12 hours, and the ball mill speed is 300-500 r / min.