Preparation method of metastable beta titanium alloy with matched high strength and plasticity
Ti-12Mo metastable beta titanium alloy is prepared through homogenization, hot rolling and annealing treatment, which solves the problem of strength and plasticity matching of existing titanium alloys, achieves a combination of high strength and high plasticity properties, and reduces the material cost cost.
Patent Information
- Application Number
- CN202310361495.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-15
AI Technical Summary
Existing high-strength β-type titanium alloys cannot achieve high plasticity while increasing strength, resulting in performance matching problems in applications and high costs.
Ti-12Mo metastable beta titanium alloy is prepared by homogenization, hot rolling and annealing. The martensite phase is generated by hot rolling to improve the slip ability, and the strong plasticity properties of the material are controlled by annealing.
A metastable beta titanium alloy that matches high strength and high plasticity has been achieved, reducing the types and costs of alloy elements while improving the comprehensive mechanical properties of the material.
Smart Images

Figure CN118773530A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal materials, and in particular relates to a method for preparing a high-strength and plasticity-matched metastable β titanium alloy. Background Art
[0002] Titanium alloys are indispensable engineering structures and functional materials used in aerospace, petrochemical, shipbuilding, biomedicine and other fields due to their light weight, high specific strength and good corrosion resistance. However, with the development of science and technology, our requirements for the strength, service performance and fatigue resistance of materials are getting higher and higher. In recent years, with the in-depth study of the deformation mechanism of titanium alloy materials, it has been found that titanium alloys have great potential in strengthening and toughening properties. However, in the current field of titanium alloy research, the existing high-strength β-type titanium alloys face the prominent problem of not being able to obtain a high strength and plasticity match while improving their strength. Therefore, how to prepare ultra-high strength and toughness β-titanium alloys has become an important research content in the field of titanium alloy research.
[0003] In previous studies, general high-performance titanium alloys are precipitation strengthening mechanisms. After solution aging treatment, fine, high-volume-fraction strengthening phase α phase is precipitated in the β matrix, thereby forming a β / α interface to hinder dislocation slip and produce a strengthening effect. Currently developed alloy grades include Ti-1023, Ti-15-3, Ti-5553, β21s, TB2 and TB10, etc. These alloys have been successfully used to prepare aircraft landing gear, fuselage frames, fasteners, connectors, etc. Although this alloy has a high yield strength, it has low plasticity. Another strengthening strategy is solid solution strengthening, which adds more types of solid solution alloying elements to a single β-phase titanium alloy, but the cost of the material will greatly increase. Therefore, we are in urgent need of finding a low-cost and high-performance titanium alloy. Summary of the invention
[0004] The purpose of the present invention is to provide a metastable β titanium alloy having both high strength and high plasticity and a preparation method thereof. The present invention obtains a metastable β titanium alloy having high strength and high plasticity matching by successively using homogenization, hot rolling and annealing methods.
[0005] To achieve the above purpose, the technical route adopted by the present invention is as follows:
[0006] A method for preparing a high-strength and plasticity-matched metastable β titanium alloy, wherein the metastable β titanium alloy is a titanium-molybdenum alloy, comprising the following steps:
[0007] Step 1, preparing a Ti-12Mo alloy ingot by arc melting method, and suction casting it into a 5.8 mm plate;
[0008] Step 2, placing the ingot from step 1 in a muffle furnace, heating it to 1000° C. and keeping it at that temperature for 3 hours, and then quickly water quenching it;
[0009] Step 3, hot rolling the ingot obtained in step 2, the rolling temperature is 900° C., and the total hot rolling reduction rate is 80%;
[0010] Step 4, take the alloy sheet obtained in step 3, perform low-temperature annealing in a muffle furnace, and then take it out for water quenching.
[0011] Preferably, the titanium-molybdenum alloy is expressed as Ti-12Mo in terms of mass ratio (wt%), wherein the Mo element accounts for 12% (wt%) and the remaining component is Ti.
[0012] Preferably, in step 1, a vacuum arc melting method is used to prepare a Ti-12Mo alloy ingot, and the specific steps are as follows: according to the target alloy composition, the surface oxide scale of the configured high-purity raw materials is removed, and a certain mass is weighed, the raw materials are placed in a high vacuum arc melting furnace, and the alloy is homogenized by arc melting to obtain an alloy ingot, and finally the ingot is suction cast into a plate.
[0013] Preferably, in step 2, the ingot obtained in step 1 is placed in a quartz tube, the quartz tube is evacuated to a vacuum state and sealed, the ingot is placed in a muffle furnace, the temperature is raised to 1000° C. with the furnace, and the temperature is kept for 3 hours, followed by water quenching.
[0014] Preferably, in step 3, multiple hot rolling passes are performed, and the reduction amount of each rolling pass is 1%-4% of the original thickness, and the total reduction rate is reached after 20-80 passes of sample thickness accumulation.
[0015] Preferably, in step 4, the rolled alloy sheet is placed in a quartz tube, the quartz tube is evacuated to a vacuum state and sealed, the muffle furnace is heated to a target temperature, the alloy sheet is placed in the muffle furnace for heat preservation, and then water quenching is performed.
[0016] Preferably, in step 4, a metastable β titanium alloy having matching strength and plasticity is obtained.
[0017] Preferably, in step 4, the annealing temperature is 200° C. and the time is 5-20 min.
[0018] Compared with the prior art, the present invention has the following advantages:
[0019] 1. The present invention introduces hot rolling technology into the processing technology of metastable β titanium alloy for the first time. Through hot rolling, the stress-generated martensite phase is introduced on the basis of keeping the matrix in β phase. The hexagonal martensite can activate more slip systems at high temperature, such as cone slip and cylindrical slip, thereby generating FCC phase in the matrix, while maintaining high yield strength and tensile strength, increasing the plasticity of the material. Compared with the martensite phase introduced by solid solution and aging treatment, it has less effect on plasticity.
[0020] 2. Compared with other high-performance titanium alloys, the metastable β titanium alloy prepared by the present invention has only two alloying elements, which is convenient for early batching and smelting, and the cost of the alloy is greatly reduced. This method can also be used in other high-performance titanium alloy fields to further improve performance.
[0021] 3. The metastable β titanium alloy of the present invention can regulate the strength and plasticity of the material by controlling the annealing time: the metastable β titanium alloy of the present invention has a tensile yield strength of 892 MPa, a tensile strength of 1286 MPa, and a tensile shaping of 21% after annealing at 200°C for 5 minutes; the tensile yield strength is 907 MPa, the tensile strength is 1263 MPa, and the tensile shaping is 18% after annealing at 200°C for 10 minutes; the tensile yield strength is 976 MPa, the tensile strength is 1262 MPa, and the tensile shaping is 15% after annealing at 200°C for 20 minutes. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the true stress-strain curve and work hardening rate curve after hot rolling. After hot rolling, the yield strength of the material can reach 520MPa, the tensile strength is 1103MPa, and the elongation is 30%.
[0023] Figure 2 This is the true stress-strain curve after hot rolling and low-temperature tempering at 200°C. After annealing at 200°C for 5 minutes, the tensile yield strength is 892MPa, the tensile strength is 1286MPa, and the tensile shaping is 21%; after annealing at 200°C for 10 minutes, the tensile yield strength is 907MPa, the tensile strength is 1263MPa, and the tensile shaping is 18%; after annealing at 200°C for 20 minutes, the tensile yield strength is 976MPa, the tensile strength is 1262MPa, and the tensile shaping is 15%.
[0024] Figure 3 These are the true stress-strain curves of cold-rolled, solution-treated and aged states. After cold-rolled, the yield strength can reach 1450MPa, with no plasticity; after solution-treated, the yield strength is 620MPa, the tensile strength is 1016MPa, and the elongation is 25%; after aging treatment, the yield strength is 1036MPa, with no plasticity.
[0025] Figure 4 This is the XRD spectrum after hot rolling and low-temperature tempering at 200℃. It can be seen that after tempering heat treatment, the main peak of the α″ phase inside the material gradually increases, and the main peak of the β phase slightly decreases, indicating that after tempering, the content of the α″ phase gradually increases, and the content of the β phase gradually decreases.
[0026] Specific implementation methods
[0027] The technical solution of the present invention is further described below with specific implementation methods. The following embodiments are all implemented under the premise of the technical solution of the present invention, and detailed implementation methods and specific operating processes are given, but the protection scope of the present invention is not limited to the following embodiments.
[0028] The present invention utilizes hot rolling and annealing treatment, and the alloy is mainly β phase. During the hot rolling deformation, α″ phase can be generated. The α″ phase with a hexagonal structure can activate more slip systems at high temperature, especially cylindrical and conical slip, thereby generating FCC phase inside the organization, so that the alloy obtains excellent performance of strong plasticity matching.
[0029] The high-strength and high-plasticity metastable β-titanium alloy (the alloy components are expressed as Ti-12Mo in mass percentage) described in the present invention innovatively adopts a hot rolling process on the β-titanium alloy, which improves the tensile strength of the alloy while maintaining good plasticity, thereby obtaining a metastable β-titanium alloy with excellent comprehensive mechanical properties.
[0030] Example 1
[0031] Step 1: Prepare raw materials according to the titanium alloy composition.
[0032] Ultrasonic cleaning: remove the surface oxide scale of Ti and Mo, then put them into a container and add alcohol cleaning solvent, clean them with ultrasound, take them out and blow off the residual cleaning solvent to obtain the required two metal raw materials.
[0033] Ingredients: Accurately weigh the Ti and Mo raw materials obtained in step (1) according to the mass percentage of the titanium alloy Ti-12Mo.
[0034] Step 2: Smelting to prepare alloy plates.
[0035] High vacuum arc melting: put the raw materials prepared in step 1 into a high vacuum arc melting furnace, evacuate the furnace, and then repeatedly fill and pump high-purity argon gas. Perform multiple gas washing to reduce the content of adverse gases in the furnace chamber. Set the working current to 190A, and perform homogenization melting on the raw materials. Turn the raw materials over after each melting. Repeat the melting six times to obtain an alloy ingot. Finally, perform suction casting on the alloy ingot according to the mold to obtain a plate.
[0036] Step 3, placing the alloy plate obtained in step 2 in a quartz tube, vacuumizing the quartz tube, then sealing the quartz tube, placing the quartz tube in a muffle furnace, heating the furnace to 1000° C., and keeping the temperature for 3 hours. After the insulation is completed, the quartz tube is quickly taken out of the muffle furnace for water quenching.
[0037] Step 4, take the plate obtained in step 3 and send it to the rolling mill for hot rolling. The sample is rolled in multiple passes, and the reduction amount of each rolling pass is 0.1mm. The sample is kept at 900℃ for 15min before the first rolling pass, and the sample is kept at 900℃ for 2min before each subsequent rolling pass, so that the rolling temperature of the sample is kept at about 900℃ during the rolling process. Finally, it is rolled into an alloy sheet with a thickness of 1.5mm, and the total hot rolling reduction rate is 80%. After the final rolling is completed, it is placed in the air to cool.
[0038] Step 5, take the alloy sheet obtained in step 4 and place it in a quartz tube, evacuate the quartz tube, then seal the quartz tube, heat the muffle furnace to 200°C, place the quartz tube in the muffle furnace and keep it warm for 5 minutes, quickly take it out of the muffle furnace after the insulation is completed, place it in water, and perform water quenching.
[0039] The hot-rolled alloy sheet obtained in step 4 was cut and subjected to tensile test. The mechanical properties were as follows: Figure 1 shown.
[0040] The hot-rolled alloy sheet obtained in step 5 was cut and subjected to tensile test. The mechanical properties were as follows: Figure 2 shown.
[0041] Example 2
[0042] Steps 1-2 are as described in Example 1.
[0043] Step 3, placing the alloy plate obtained in step 2 in a quartz tube, vacuumizing the quartz tube, then sealing the quartz tube, placing the quartz tube in a muffle furnace, heating the furnace to 1000° C., and keeping the temperature for 3 hours. After the insulation is completed, the quartz tube is quickly taken out of the muffle furnace for water quenching.
[0044] Step 4, take the plate obtained in step 3 and send it to the rolling mill for hot rolling. The sample is rolled in multiple passes, and the reduction amount of each rolling pass is 0.1mm. The sample is kept at 900℃ for 15min before the first rolling pass, and the sample is kept at 900℃ for 2min before each subsequent rolling pass, so that the rolling temperature of the sample is kept at about 900℃ during the rolling process. Finally, it is rolled into an alloy sheet with a thickness of 1.5mm, and the total hot rolling reduction rate is 80%. After the final rolling is completed, it is placed in the air to cool.
[0045] Step 5, take the alloy sheet obtained in step 4 and place it in a quartz tube, evacuate the quartz tube, then seal the quartz tube, heat the muffle furnace to 200°C, place the quartz tube in the muffle furnace and keep it warm for 10 minutes, quickly take it out of the muffle furnace after the insulation is completed, place it in water, and perform water quenching.
[0046] The annealed alloy sheet sample obtained in step 5 is subjected to electric spark cutting and mechanical property testing. The mechanical properties are as follows: Figure 2 shown.
[0047] Example 3
[0048] Steps 1-2 are as described in Example 1.
[0049] Step 3, placing the alloy plate obtained in step 2 in a quartz tube, vacuumizing the quartz tube, then sealing the quartz tube, placing the quartz tube in a muffle furnace, heating the furnace to 1000° C., and keeping the temperature for 3 hours. After the insulation is completed, the quartz tube is quickly taken out of the muffle furnace for water quenching.
[0050] Step 4, take the plate obtained in step 3 and send it to the rolling mill for hot rolling. The sample is rolled in multiple passes, and the reduction amount of each rolling pass is 0.1mm. The sample is kept at 900℃ for 15min before the first rolling pass, and the sample is kept at 900℃ for 2min before each subsequent rolling pass, so that the rolling temperature of the sample is kept at about 900℃ during the rolling process. Finally, it is rolled into an alloy sheet with a thickness of 1.5mm, and the total hot rolling reduction rate is 80%. After the final rolling is completed, it is placed in the air to cool.
[0051] Step 5, take the alloy sheet obtained in step 4 and place it in a quartz tube, evacuate the quartz tube, then seal the quartz tube, heat the muffle furnace to 200°C, place the quartz tube in the muffle furnace and keep it warm for 20 minutes, quickly take it out of the muffle furnace after the insulation is completed, place it in water, and perform water quenching.
[0052] The annealed alloy sheet sample obtained in step 5 is subjected to electric spark cutting and mechanical property testing. The mechanical properties are as follows: Figure 2 shown.
[0053] Comparative Example 1
[0054] Steps 1-3 are as described in Example 1.
[0055] Step 4, taking the homogenized plate obtained in step 3, cold rolling the alloy on a rolling mill, with a reduction of 0.1 mm in each rolling pass, and finally rolling it into an alloy sheet with a thickness of 1.5 mm, with a total hot rolling reduction rate of 80%.
[0056] The cold-rolled alloy sheet obtained in step 4 was subjected to electrospark cutting and then to mechanical property testing. The test results are as follows: Figure 3 shown.
[0057] Comparative Example 2
[0058] Steps 1-3 are as described in Example 1.
[0059] Step 4, taking the homogenized plate obtained in step 3, cold rolling the alloy on a rolling mill, with a reduction of 0.1 mm in each rolling pass, and finally rolling it into an alloy sheet with a thickness of 1.5 mm, with a total hot rolling reduction rate of 80%.
[0060] Step 5, take the alloy sheet obtained by rolling in step 4 and place it in a quartz tube, evacuate the quartz tube, seal the quartz tube, place the quartz tube in a muffle furnace, heat it to 900° C., and keep it warm for 1 hour. After the end of the insulation, quickly perform water quenching.
[0061] The alloy sheet obtained in step 5 was subjected to electrospark cutting and then to mechanical property testing. The test results are as follows: Figure 3 shown.
[0062] Comparative Example 2
[0063] Steps 1-3 are as described in Example 1.
[0064] Step 4, taking the homogenized plate obtained in step 3, cold rolling the alloy on a rolling mill, with a reduction of 0.1 mm in each rolling pass, and finally rolling it into an alloy sheet with a thickness of 1.5 mm, with a total hot rolling reduction rate of 80%.
[0065] Step 5, take the alloy sheet obtained by rolling in step 4 and place it in a quartz tube, evacuate the quartz tube, seal the quartz tube, place the quartz tube in a muffle furnace, heat it to 900° C., and keep it warm for 1 hour. After the end of the insulation, quickly perform water quenching.
[0066] Step 6, placing the alloy sheet in a solid solution state in a quartz tube, evacuating the quartz tube, and then sealing the quartz tube, placing the quartz tube in a muffle furnace, heating the furnace to 500° C., keeping the temperature for 30 minutes, and then water quenching.
[0067] The aged alloy sheet obtained in step 6 was subjected to electrospark cutting and then to mechanical property testing. The test results are as follows: Figure 3 shown.
Claims
1. A method for preparing a metastable β titanium alloy with high strength and plasticity matching, characterized in that: The titanium alloy is a Ti-12Mo alloy, comprising the following steps: Step 1, preparing a Ti-12Mo alloy ingot by arc melting method, and suction casting it into a plate with a thickness of 5.8 mm; Step 2, placing the ingot from step 1 in a muffle furnace, heating it to 1000° C. and keeping it at that temperature for 3 hours, and then quickly water quenching it; Step 3, hot rolling the ingot obtained in step 2, the rolling temperature is 900° C., and the total hot rolling reduction rate is 80%; Step 4, take the alloy sheet obtained in step 3, perform low-temperature annealing in a muffle furnace, and then take it out for water quenching.
2. The method according to claim 1, characterized in that In step 1, an arc melting method is used to prepare a titanium-molybdenum alloy ingot, and the steps are as follows: according to the target alloy composition, the configured high-purity raw materials are placed in a high-vacuum arc melting furnace, the alloy is arc-melted for homogenization to obtain an alloy ingot, and suction casting is performed. The thickness of the suction-cast plate is 5.8 mm.
3. The method according to claim 1, characterized in that In step 3, multiple hot rolling passes are performed, and the reduction amount of each rolling pass is 1%-4% of the original thickness.
4. The method according to claim 1, characterized in that In step 4, the alloy is placed in a muffle furnace for low temperature annealing, the temperature is set to 200° C., and the time is controlled within 5-20 minutes.
5. The method according to claim 1, characterized in that The Mo element accounts for 12% (wt%), and the rest is Ti.
6. A metastable β titanium alloy having good matching of strength and plasticity prepared by the method according to any one of claims 1 to 6.
Citation Information
Cited By
Preparation method and application of titanium alloy with high electron emission threshold
CN119843088A
Preparation method and application of high electron emission threshold titanium alloy
CN119843088B