System for preventing generation of passivation cross grains and use method
By adjusting and checking the parameters of each component of the strip chemical treatment system, combined with the use of a stable roller group, the problem of horizontal streaks in the strip chemical treatment was solved, and product quality and production stability were improved.
Patent Information
- Application Number
- CN202410768696.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-15
AI Technical Summary
Horizontal streaks are prone to appear during the chemical treatment of the plate and strip, which affects the appearance and quality of the product, especially when the coating chemical treatment of wide-width aluminum plates is more obvious.
By adjusting and checking the roughness, cylindricity, roller surface hardness, parallelism and balance quality of each component of the system, ensure that the parameters of the passivated steering roller, support roller, paint roller and drying and cooling device reach the preset values and the settings are stable The roller set stabilizes the strip and avoids horizontal lines.
It effectively avoids the occurrence of horizontal lines, improves the yield rate, ensures the stability of continuous product production, has strong practicability, good process repeatability, and easy maintenance.
Smart Images

Figure CN118773591A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of plate and strip finishing and processing, and in particular relates to a system for preventing the generation of passivation transverse lines and a use method thereof. Background Art
[0002] In the field of plate and strip finishing and processing equipment technology, such as continuous galvanizing units, continuous color coating units and continuous coating units, chemical treatment is performed on the surface of metal plates and strips to form an insoluble chemical passivation film on the surface, which prevents the atmosphere or other corrosive gases from corroding the substrate, while enhancing the adhesion between the substrate and the coating layer and improving the coating performance of the substrate. During the chemical treatment process, horizontal lines are likely to appear on the surface of the plate and strip, affecting the appearance and quality of the product, especially for wide aluminum plates with a width of 1800mm, which are more likely to produce the above defects during the chemical treatment of the coating.
[0003] No relevant literature has been found in the prior art to solve the above problem. Summary of the invention
[0004] The system and method for preventing the generation of passivation horizontal lines provided by the present invention aim to overcome the problem in the prior art that horizontal lines are easily generated on the surface of the plate and strip during the chemical treatment process, thus affecting the appearance and quality of the product.
[0005] To this end, the present invention provides a system for preventing the generation of passivation horizontal lines, including a plate strip, a passivation steering roller, a passivation front coating paint, a passivation front coating pick-up roller, a passivation front coating paint roller, a passivation back coating paint roller, a passivation back coating pick-up roller, a passivation back coating paint, a passivation drying furnace, a cooling device and a tension roller. The passivation steering roller, the passivation front coating paint roller, the passivation back coating paint roller, the passivation drying furnace, the cooling device and the tension roller are connected in sequence through the plate strip, the passivation steering roller and the passivation front coating paint roller are both connected to the front side of the plate strip, the passivation back coating paint roller is connected to the back side of the plate strip, the passivation front coating paint is connected to the passivation front coating paint roller via the passivation front coating pick-up roller, and the passivation back coating paint is connected to the passivation back coating paint roller via the passivation back coating pick-up roller. Preferably, a passivation support roller is arranged between the passivation front coating roller and the passivation back coating roller, and the back side of the plate strip is connected to the passivation support roller.
[0006] Preferably, a lifting roller is arranged between the passivation support roller and the passivation back coating roller, and the back side of the strip is connected to the lifting roller.
[0007] Preferably, the passivation drying furnace adopts a heating method of hot air circulation.
[0008] Preferably, the cooling device is an air cooling device.
[0009] Preferably, the plate strip between the passivation drying furnace and the cooling device is connected with a stabilizing roller group.
[0010] Preferably, the stabilizing roller set includes two sets of rollers, and the plate strip is connected between the two sets of rollers.
[0011] Preferably, the diameter of the roller is 85-120 mm.
[0012] Preferably, the roller is adjusted up and down within a range of ±15 mm based on the unit operation line.
[0013] A method for using a system for preventing the generation of passivation horizontal lines comprises the following steps: 1) Check and make the roughness, cylindricity and roller surface hardness of the passivated steering roller, passivated support roller, passivated front coating pick-up roller, passivated front coating roller, lifting roller, passivated back coating roller and passivated back coating pick-up roller reach the preset values; 2) Adjust the parallelism of each pair of rollers among the passivation steering roller, the passivation support roller, the passivation front coating pick-up roller, the passivation front coating roller, the lifting roller, the passivation back coating roller and the passivation back coating pick-up roller so that the parallelism tolerance value reaches the preset value; at the same time, adjust the cumulative tolerance value of the parallelism between the control rollers so that the cumulative tolerance value reaches the preset value; 3) Check the balance quality level of the passivation steering roller, passivation support roller, passivation front coating pick-up roller, passivation front coating roller, lifting roller, passivation back coating roller, passivation back coating pick-up roller and tension roller, so that the balance quality level value reaches the preset value; 4) Adjust the rotation speed of the passivation front coating pick-up roller, the passivation front coating roller, the passivation back coating roller and the passivation back coating pick-up roller so that the rotation speed value reaches the preset value; 5) Adjust the viscosity of the passivation front coating and the passivation back coating to the preset value; 6) Adjust the air volume, air pressure and wind speed of the passivation drying furnace and cooling device to the preset values; 7) Adjust the tension value of the passivation section to the preset value.
[0014] Beneficial effects of the present invention: 1. The system and method for using the present invention for preventing the generation of passivation transverse lines, by adjusting and inspecting the components in the system for preventing the generation of passivation transverse lines and making them reach preset values, ensures that the roughness, cylindricity and roller surface hardness between the rollers of the passivation steering roller, the passivation support roller, the passivation front coating pick-up roller, the passivation front coating roller, the lifting roller, the passivation back coating roller and the passivation back coating pick-up roller reach the accuracy requirements of the preset values, and at the same time reduces the cumulative tolerance value of the parallelism between the rollers; ensures that the viscosity of the coating reaches the preset value requirements, so that the roller speed configuration matches the unit speed, and the tension of the passivation section reaches the preset value, avoiding the influence of the passivation drying furnace and the cooling device on the vibration of the plate and strip, and meeting the requirements for continuous production of the product. The generation of transverse lines is avoided by inspection and adjustment, and the yield rate is improved. It has strong practicality, good process repeatability, convenient maintenance and easy implementation.
[0015] 2. The system and method for preventing the generation of passivation horizontal lines provided by the present invention play a role in stabilizing the plate and strip by providing a stabilizing roller group connected to the plate and strip between the passivation drying furnace and the cooling device.
[0016] 3. The system and method for preventing the generation of passivation horizontal lines provided by the present invention has a roller diameter of 85-120 mm in the stabilizing roller group, which has good stability and will not scratch the surface of the plate or strip. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The present invention will be further described in detail below with reference to the accompanying drawings.
[0018] Figure 1 It is a schematic diagram of the structure of the system for preventing the generation of passivation striations; Figure 2 The present invention is a flow chart of a method for using a system for preventing the occurrence of passivation horizontal lines.
[0019] Explanation of the reference numerals: 1. Plate and strip; 2. Passivated steering roller; 3. Passivated front coating; 4. Passivated front coating pick-up roller; 5. Passivated front coating roller; 6. Passivated support roller; 7. Lifting roller; 8. Passivated back coating roller; 9. Passivated back coating pick-up roller; 10. Passivated back coating; 11. Cooling device; 12. Passivated drying furnace; 13. Stabilizing roller group; 14. Tension roller. DETAILED DESCRIPTION
[0020] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific conditions are specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer.
[0021] Embodiment 1: like Figure 1As shown, a system for preventing the generation of passivation horizontal lines includes a plate strip 1, a passivation steering roller 2, a passivation front coating roller 3, a passivation front coating pick-up roller 4, a passivation front coating roller 5, a passivation back coating roller 8, a passivation back coating pick-up roller 9, a passivation back coating roller 10, a passivation drying furnace 12, a cooling device 11 and a tension roller 14. The passivation steering roller 2, the passivation front coating roller 5, the passivation back coating roller 8, the passivation drying furnace 12, the cooling device 11 and the tension roller 14 are connected in sequence through the plate strip 1, the passivation steering roller 2 and the passivation front coating roller 5 are both connected to the front side of the plate strip 1, the passivation back coating roller 8 is connected to the back side of the plate strip 1, the passivation front coating 3 is connected to the passivation front coating roller 5 through the passivation front coating pick-up roller 4, and the passivation back coating 10 is connected to the passivation back coating roller 8 through the passivation back coating pick-up roller 9. Specifically, the plate strip 1 loaded with the passivation section tension runs at a certain speed, and passes through the passivation steering roller 2, the passivation front coating roller 5, the passivation support roller 6, the passivation back coating roller 8, the passivation drying furnace 12, the cooling device 11 and the tension roller 14 in sequence; the passivation steering roller 2 changes the running direction of the plate strip 1, so that the plate strip 1 runs in the direction of the coating roller; the passivation front coating pick-up roller 4 picks up the passivation front coating 3 and transfers it to the passivation front coating roller 5, and the passivation front coating roller 5 then applies the passivation front coating 3 on the front side of the plate strip 1, and the passivation back coating pick-up roller 9 picks up the passivation back coating 10 and transfers it to the passivation back coating roller 8, and the passivation back coating roller 8 then applies the passivation back coating 10 on the back side of the plate strip 1; the tension roller 14 can establish and adjust the passivation section tension.
[0022] By adjusting and checking the components in the system to prevent the generation of passivation horizontal lines and making them reach the preset values, it is ensured that the roughness, cylindricity and roller surface hardness between the passivation steering roller 2, the passivation support roller 6, the passivation positive coating pick-up roller 4, the passivation positive coating roller 5, the lifting roller 7, the passivation back coating roller 8 and the passivation back coating pick-up roller 9 reach the accuracy requirements of the preset values, and at the same time reduce the cumulative tolerance value of the parallelism between the rollers; it is ensured that the viscosity of the coating reaches the preset value requirements, so that the roller speed configuration matches the unit speed, and the tension of the passivation section reaches the preset value, avoiding the influence of the passivation drying furnace 12 and the cooling device 11 on the vibration of the plate strip 1, and meeting the continuous production requirements of the product. Through inspection and adjustment, the generation of horizontal lines is avoided and the yield rate is improved. It has strong practicality, good process repeatability, convenient maintenance and easy implementation.
[0023] Preferably, a passivation support roller 6 is provided between the passivation front coating roller 5 and the passivation back coating roller 8 , and the back side of the plate strip 1 is connected to the passivation support roller 6 .
[0024] Specifically, when the passivation coating roller 5 is coating, the passivation support roller 6 supports the strip 1 .
[0025] Preferably, a lifting roller 7 is provided between the passivation support roller 6 and the passivation back coating roller 8 , and the back side of the plate strip 1 is connected to the lifting roller 7 .
[0026] Specifically, when the passivation back coating roller 8 is coating, the lifting roller 7 supports the strip 1 .
[0027] Preferably, the passivation drying furnace 12 adopts a heating method of hot air circulation.
[0028] Specifically, the passivation drying furnace 12 adopts a hot air circulation heating method, and uses high-temperature hot air to dry the passivation coating, which can easily form a passivation film on the surface of the plate strip 1 and has a good drying effect.
[0029] Preferably, the cooling device 11 is an air cooling device.
[0030] Specifically, the main function of the air cooling device is to blow air on the surface of the plate strip 1 after passivation and drying, so as to achieve the purpose of cooling the aluminum plate, and the cooling effect is good.
[0031] Preferably, a stabilizing roller group 13 is provided and connected to the strip 1 between the passivation drying furnace 12 and the cooling device 11 .
[0032] Specifically, a stabilizing roller group 13 is provided on the strip 1 between the passivation drying furnace 12 and the cooling device 11 to stabilize the strip.
[0033] Preferably, the stabilizing roller set 13 includes two sets of rollers, and the plate strip 1 is connected between the two sets of rollers.
[0034] Specifically, in actual applications, the stabilizing roller group 13 arranged between the passivation drying furnace 12 and the cooling device 11 blocks the cross-influence of hot air and cold air, reduces the vibration of the plate strip 1, makes the plate strip run stably, effectively prevents the generation of transverse lines, and indirectly improves the yield rate.
[0035] Preferably, the diameter of the roller is 85-120 mm.
[0036] Specifically, a roller with a diameter that is too small is light and cannot suppress the vibration of the plate strip 1, and has poor stability; a roller with a diameter that is too large requires a motor to drive it to roll, and a large-diameter roller, if not driven, is prone to scratching the surface of the plate strip, and if driven, consumes electricity; the present invention adopts a roller with a diameter of 85-120mm, which overcomes the problems of rollers with too large or too small diameters, has good stability, simple structure, and avoids scratches on the surface of the plate strip.
[0037] Preferably, the diameter of the roller is 100 mm.
[0038] Specifically, rollers with a diameter of 100 mm have the best stability and will not scratch the surface of the strip.
[0039] Preferably, the roller is adjusted up and down within a range of ±15 mm based on the unit operation line.
[0040] Specifically, the position of the roller can be adjusted up and down according to demand, and has good adaptability.
[0041] Embodiment 2: like Figure 2 As shown, based on Example 1, a method for using a system for preventing the generation of passivation horizontal lines includes the following steps: 1) Check and make the roughness, cylindricity and roller surface hardness of the passivation steering roller 2, the passivation support roller 6, the passivation front coating pick-up roller 4, the passivation front coating roller 5, the lifting roller 7, the passivation back coating roller 8 and the passivation back coating pick-up roller 9 reach the preset values; 2) Adjust the parallelism of each pair of rollers among the passivation steering roller 2, the passivation support roller 6, the passivation front coating pick-up roller 4, the passivation front coating roller 5, the lifting roller 7, the passivation back coating roller 8 and the passivation back coating pick-up roller 9, so that the parallelism tolerance value reaches the preset value; at the same time, adjust the cumulative tolerance value of the parallelism between the control rollers so that the cumulative tolerance value reaches the preset value; 3) Check the balance quality level of the passivation steering roller 2, the passivation support roller 6, the passivation front coating pick-up roller 4, the passivation front coating roller 5, the lifting roller 7, the passivation back coating roller 8, the passivation back coating pick-up roller 9 and the tension roller 14, so that the balance quality level value reaches the preset value; 4) adjusting the rotation speeds of the passivation front coating pick-up roller 4, the passivation front coating roller 5, the passivation back coating roller 8 and the passivation back coating pick-up roller 9 so that the rotation speeds reach the preset values; 5) Adjust the viscosity of the passivation front coating 3 and the passivation back coating 10 to a preset value; 6) Adjust the air volume, air pressure and air speed of the passivation drying furnace 12 and the cooling device 11 to the preset values; 7) Adjust the tension value of the passivation section to the preset value.
[0042] In engineering, the tension of the strip between the passivation steering roller 2 and the tension roller 14 is called the passivation section tension. By adjusting and checking the components in the system to prevent the generation of passivation horizontal lines and making them reach the preset values, it is ensured that the roughness, cylindricity and roller surface hardness between the passivation steering roller 2, the passivation support roller 6, the passivation positive coating pick-up roller 4, the passivation positive coating roller 5, the lifting roller 7, the passivation back coating roller 8 and the passivation back coating pick-up roller 9 meet the accuracy requirements of the preset values, and at the same time reduce the cumulative tolerance value of the parallelism between the rollers; ensure that the viscosity of the coating meets the preset value requirements, so that the roller speed configuration matches the unit speed, and the passivation section tension reaches the preset value, avoiding the influence of the passivation drying furnace 12 and the cooling device 11 on the vibration of the strip 1, and meeting the continuous production requirements of the product. Through inspection and adjustment, the generation of horizontal lines is avoided and the yield rate is improved. It has strong practicality, good process repeatability, convenient maintenance and easy implementation.
[0043] In the description of the present invention, it should be understood that the terms "front" and "back" etc. indicating orientation or positional relationship are based on the orientation or positional relationship shown in the drawings, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, the terms describing the positional relationship in the drawings are only used for illustrative purposes and are not to be construed as limitations on the present invention.
[0044] The above examples are merely illustrative of the present invention and do not constitute a limitation on the protection scope of the present invention. All designs that are the same or similar to the present invention fall within the protection scope of the present invention.
Claims
1. A system for preventing the generation of passivation stripes, characterized in that: It comprises a plate strip (1), a passivation steering roller (2), a passivation front coating paint (3), a passivation front coating pick-up roller (4), a passivation front coating paint roller (5), a passivation back coating paint roller (8), a passivation back coating paint pick-up roller (9), a passivation back coating paint (10), a passivation drying furnace (12), a cooling device (11) and a tension roller (14), a passivation steering roller (2), a passivation front coating paint roller (5), a passivation back coating paint roller (8), and a passivation drying furnace (12) , a cooling device (11) and a tension roller (14) are connected in sequence through the plate strip (1); the passivation steering roller (2) and the passivation front coating roller (5) are both connected to the front side of the plate strip (1); the passivation back coating roller (8) is connected to the back side of the plate strip (1); the passivation front coating (3) is connected to the passivation front coating roller (5) through the passivation front coating pick-up roller (4); and the passivation back coating (10) is connected to the passivation back coating roller (8) through the passivation back coating pick-up roller (9).
2. The system for preventing the generation of passivation horizontal lines as claimed in claim 1, characterized in that: A passivation support roller (6) is arranged between the passivation front coating roller (5) and the passivation back coating roller (8), and the back side of the plate strip (1) is connected to the passivation support roller (6).
3. The system for preventing the generation of passivation horizontal lines as claimed in claim 1, characterized in that: A lifting roller (7) is arranged between the passivation support roller (6) and the passivation back coating roller (8), and the back side of the plate strip (1) is connected to the lifting roller (7).
4. The system for preventing the generation of passivation horizontal lines as claimed in claim 1, characterized in that: The passivation drying furnace (12) adopts a heating method of hot air circulation.
5. The system for preventing the generation of passivation horizontal lines as claimed in claim 1, characterized in that: The cooling device (11) is an air cooling device.
6. The system for preventing the generation of passivation horizontal lines as claimed in claim 1, characterized in that: A stabilizing roller group (13) is provided and connected to the plate strip (1) between the passivation drying furnace (12) and the cooling device (11).
7. The system for preventing the generation of passivation horizontal lines as claimed in claim 6, characterized in that: The stabilizing roller group (13) comprises two groups of rollers, and the plate strip (1) is connected between the two groups of rollers.
8. The system for preventing the generation of passivation horizontal lines as claimed in claim 7, characterized in that: The diameter of the roller is 85-120 mm.
9. The system for preventing the generation of passivation horizontal lines as claimed in claim 7, characterized in that: The roller can be adjusted up and down within a range of ±15 mm based on the unit operation line.
10. A method for using a system for preventing the generation of passivation horizontal lines, characterized in that: The steps include: 1) Check and ensure that the roughness, cylindricity and roller surface hardness values of the passivated steering roller (2), the passivated support roller (6), the passivated front coating pick-up roller (4), the passivated front coating roller (5), the lifting roller (7), the passivated back coating roller (8) and the passivated back coating pick-up roller (9) reach preset values; 2) adjusting the parallelism of each pair of rollers among the passivation steering roller (2), the passivation support roller (6), the passivation front coating pick-up roller (4), the passivation front coating roller (5), the lifting roller (7), the passivation back coating roller (8) and the passivation back coating pick-up roller (9) so that the parallelism tolerance value thereof reaches a preset value; and at the same time adjusting the cumulative tolerance value of the parallelism between the control rollers so that the cumulative tolerance value reaches a preset value; 3) Check the balance quality level of the passivated steering roller (2), the passivated support roller (6), the passivated front coating pick-up roller (4), the passivated front coating roller (5), the lifting roller (7), the passivated back coating roller (8), the passivated back coating pick-up roller (9) and the tension roller (14), so that the balance quality level value reaches the preset value; 4) adjusting the rotation speeds of the passivation front coating pick-up roller (4), the passivation front coating roller (5), the passivation back coating roller (8) and the passivation back coating pick-up roller (9) so that the rotation speeds reach preset values; 5) adjusting the viscosity of the passivation front coating (3) and the passivation back coating (10) to a preset value; 6) adjusting the air volume, air pressure and air speed of the passivation drying furnace (12) and the cooling device (11) to preset values; 7) Adjust the tension value of the passivation section to the preset value.