Hydrogen production electrode and preparation method and application thereof

By spraying, then sandblasting and then spraying during the preparation process of the hydrogen production electrode, and using an alkaline solution in the dealumination activation, the problem of insufficient bonding force between the coating and the substrate was solved, and the mechanical and chemical stability of the electrode was significantly improved. .

CN118773598APending Publication Date: 2024-10-15三一氢能有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411028714.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing hydrogen production electrode's coating has insufficient bonding force with the substrate, causing the coating to easily crack and fall off, affecting its mechanical and chemical stability.

Method used

The first spraying treatment is carried out, then the sandblasting treatment is carried out, and finally the second spraying treatment is carried out, and KOH or NaOH solution is used in the dealumination activation process, and the two spraying formulas are controlled to be consistent to improve the bonding force between the coating and the substrate. .

Benefits of technology

The bonding force between the coating and the substrate of the hydrogen production electrode is significantly improved, its mechanical properties and electrochemical activity are enhanced, and the service life of the electrode is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of hydrogen production electrodes, in particular to a hydrogen production electrode and a preparation method and application thereof. The preparation method comprises the following steps: S1, carrying out first spraying treatment on a base material electrode, so that a first coating is arranged on the base material electrode to obtain a first electrode; s2, the first electrode is subjected to sand blasting treatment, and a second electrode is obtained; s3, the second electrode is subjected to second spraying treatment, so that a second coating is arranged on the second electrode, and the second electrode is obtained; and S4, carrying out dealumination activation treatment on the second electrode to obtain the hydrogen production electrode. Wherein the spraying powder in the first spraying treatment is the same as the spraying powder in the second spraying treatment. According to the method, the coating spraying process is optimized, meanwhile, the formula of two times of spraying is controlled to be consistent, and the binding force between the substrate electrode and the coating can be further improved on the premise that a third phase is not introduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogen production electrodes, and in particular to a hydrogen production electrode and a preparation method and application thereof. Background Art

[0002] In the context of the global advocacy of clean and low-carbon transformation, water electrolysis hydrogen production technology has become the key to achieving "carbon neutrality". At present, alkaline water electrolysis hydrogen production technology is the most mature and the lowest cost. In practical applications, alkaline water hydrogen production electrodes must have good mechanical and chemical stability in addition to high conductivity and high catalytic activity. The electrode stability is closely related to the bonding strength between the electrode coating and the substrate.

[0003] In the field of coating preparation, the bonding strength between the coating and the substrate is the most important indicator affecting the performance of the coating. Generally, the main forms of coating failure are cracking and shedding. The main reason for the above failure forms is the insufficient bonding strength between the film layer and the substrate.

[0004] Common hydrogen production electrodes use Raney nickel-coated electrodes prepared by thermal spraying. Although this type of electrode has the advantages of high specific surface area and high electrochemical activity, it has poor bonding force and mechanical strength and is easy to fall off from the substrate. Therefore, it is necessary to propose a preparation scheme for nickel-based electrocatalysts that have both mechanical properties and electrochemical activity. Summary of the invention

[0005] The present invention provides a hydrogen production electrode and a preparation method and application thereof, so as to solve the above-mentioned defects in the prior art and further improve the coating bonding strength of the hydrogen production electrode without introducing a third phase.

[0006] In a first aspect, the present invention provides a method for preparing a hydrogen production electrode, comprising: S1: performing a first spraying treatment on a substrate electrode so that a first coating is provided on the substrate electrode to obtain a first electrode; S2: sandblasting the first electrode to obtain a second electrode; S3: performing a second spraying treatment on the second electrode so that a second coating is provided on the second electrode to obtain a second electrode; S4: subjecting the second electrode to a dealumination activation treatment to obtain the hydrogen production electrode; wherein the spraying powder in the first spraying treatment is the same as the spraying powder in the second spraying treatment.

[0007] According to a method for preparing a hydrogen production electrode provided by the present invention, the thickness of the first coating is smaller than the thickness of the second coating.

[0008] According to a method for preparing a hydrogen-producing electrode provided by the present invention, in the first spraying treatment and the second spraying treatment, the spraying powder includes nickel-aluminum alloy powder and / or nickel-aluminum mixed powder; preferably, the spraying powder also includes one or more of nickel powder, aluminum powder, iron powder, molybdenum powder, nickel-molybdenum mixed powder, nickel-iron alloy powder, and nickel-molybdenum alloy powder.

[0009] According to a method for preparing a hydrogen production electrode provided by the present invention, the powder application amount of the first coating layer is 100-150 g / m2; and the powder application amount of the second coating layer is 200-250 g / m2.

[0010] According to a method for preparing a hydrogen production electrode provided by the present invention, during the sandblasting process, the spraying gas pressure is controlled to be 0.4-0.5 MPa.

[0011] According to a method for preparing a hydrogen production electrode provided by the present invention, in the sandblasting process, the particle size of the sandblasting is controlled to be 80-150 meshes.

[0012] According to a method for preparing a hydrogen production electrode provided by the present invention, in the sandblasting process, the sandblasting time is 10 to 1200 seconds.

[0013] According to a method for preparing a hydrogen production electrode provided by the present invention, the dealumination activation comprises: soaking in a 10-30wt% KOH or NaOH solution for 1-24 hours.

[0014] In a second aspect, the present invention provides a hydrogen production electrode, which is prepared by the above-mentioned method for preparing a hydrogen production electrode.

[0015] In a third aspect, the present invention provides application of the above-mentioned hydrogen production electrode in hydrogen evolution reaction.

[0016] The hydrogen production electrode and its preparation method and application provided by the present invention can further improve the bonding strength between the substrate electrode and the coating without introducing a third phase by optimizing the coating spraying process and controlling the formulation of the two sprayings to be consistent. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] At present, in the existing technology, when improving the bonding strength of the hydrogen production electrode coating, the optimization direction is mainly the coating formula and the optimization process. The main methods to improve the bonding strength of the coating are: 1) Increasing the contact area of ​​the substrate before spraying, using chemical or physical treatment methods to increase the surface roughness of the metal substrate, such as sandblasting, pickling, electrochemical etching, etc., can also improve the bonding strength; 2) The gradient growth of the coating can effectively improve the stress changes caused by the sudden change of the coating composition, greatly reduce the residual stress of the coating, and help improve the bonding strength between the coating and the substrate; 3) Introducing an intermediate layer. The electrode consists of a coating and a substrate. When the characteristics of the two do not match, the sudden change in the material properties between the substrate and the coating leads to a significant reduction in the bonding strength between the coating and the substrate. The introduction of a transition layer (intermediate layer) can reduce the stress changes caused by the material mutation and improve the bonding strength. However, there is still room for further improvement in the above methods in terms of coating bonding strength.

[0019] The present invention finds that before sandblasting the substrate electrode, a spraying treatment is first performed, and then the spraying treatment is performed again after sandblasting. By controlling the spraying formula during the two spraying treatments to be consistent, the bonding strength between the substrate electrode and the coating can be significantly improved.

[0020] Based on this, the present invention has the following technical solutions: In a first aspect, the present invention provides a method for preparing a hydrogen production electrode, comprising: S1: performing a first spraying treatment on a substrate electrode so that a first coating is provided on the substrate electrode to obtain a first electrode; S2: sandblasting the first electrode to obtain a second electrode; S3: performing a second spraying treatment on the second electrode so that a second coating is provided on the second electrode to obtain a second electrode; S4: subjecting the second electrode to a dealumination activation treatment to obtain the hydrogen production electrode; wherein the spraying powder in the first spraying treatment is the same as the spraying powder in the second spraying treatment.

[0021] The present invention finds that before sandblasting the substrate electrode, a spraying treatment is first performed to obtain a first electrode with a thinner coating. The substrate electrode with the first coating is sandblasted. Under the impact of high-pressure sand, a roughening layer is formed on the surface of the substrate, and part of the material of the first coating is flushed into the depression on the surface of the substrate and embedded therein. Then, after sandblasting, the spraying treatment is performed again. By controlling the spraying formulas during the two spraying treatments to be the same, the properties of the obtained second coating are consistent with those of the first coating, which can reduce the stress changes caused by material mutations during the spraying process, so that the two coatings can be more firmly combined.

[0022] In the present invention, between S3 and S4, other formulations of spraying treatment can also be performed with reference to the existing disclosed technical solutions in the prior art, as long as the spraying formulas in S1 and S3 are consistent, and no specific limitation is made here.

[0023] According to a preferred embodiment provided by the present invention, the amount of powder applied to the first coating layer is less than the amount of powder applied to the second coating layer.

[0024] In the present invention, those skilled in the art can use known and disclosed technologies such as plasma spraying to perform spraying treatment according to actual conditions. The parameters of the spraying treatment in S1 and S3 can be the same, and the amount of powder applied can be regulated by controlling the speed of the spray gun.

[0025] The present invention finds that the amount of powder applied to the first coating should not be too high, otherwise excessive coating waste will be caused during the sandblasting process.

[0026] In the present invention, the amount of powder applied here refers to the deposition mass of the coating material per unit area under the condition of uniform spraying.

[0027] According to a preferred embodiment provided by the present invention, in the first spraying process and the second spraying process, the spraying powder includes nickel-aluminum alloy powder and / or nickel-aluminum mixed powder.

[0028] Further preferably, the mass ratio of nickel to aluminum in the nickel-aluminum mixed powder or nickel-aluminum alloy powder is (6-9): (1-4).

[0029] In the present invention, the spraying powder may also include one or more of nickel powder, aluminum powder, iron powder, molybdenum powder, nickel-molybdenum mixed powder, nickel-iron alloy powder, and nickel-molybdenum alloy powder.

[0030] More preferably, the spraying powder is a nickel-aluminum mixed powder.

[0031] Further preferably, the mass ratio of nickel to aluminum in the nickel-aluminum mixed powder is (6-9): (1-4).

[0032] According to a preferred embodiment provided by the present invention, the amount of powder applied to the first coating layer is 100-150 g / m2; the amount of powder applied to the second coating layer is 200-250 g / m2. Specifically, the amount of powder applied to the first coating layer is 100 g / m2, 110 g / m2, 120 g / m2, 130 g / m2, 140 g / m2 or 150 g / m2; the amount of powder applied to the second coating layer is 200 g / m2, 210 g / m2, 220 g / m2, 230 g / m2, 240 g / m2 or 250 g / m2.

[0033] According to a preferred embodiment provided by the present invention, during the sandblasting process, the spraying gas pressure is controlled to be 0.4-0.5 MPa.

[0034] According to a preferred embodiment provided by the present invention, in the sandblasting process, the particle size of the sandblasting is controlled to be 80-150 meshes.

[0035] According to a preferred embodiment provided by the present invention, in the sandblasting process, the sandblasting time is 10 to 1200 seconds.

[0036] According to a preferred embodiment provided by the present invention, the dealumination activation comprises: soaking in a 10-30wt% KOH or NaOH solution for 1-24 hours.

[0037] In a second aspect, the present invention provides a hydrogen production electrode, which is prepared by the above-mentioned method for preparing a hydrogen production electrode.

[0038] In a third aspect, the present invention provides application of the above-mentioned hydrogen production electrode in hydrogen evolution reaction.

[0039] In order to further illustrate the technical solution of the present invention, the present invention provides the following specific embodiments and comparative examples.

[0040] Unless otherwise specified, the various raw materials used in the examples and comparative examples are commercially available conventional raw materials, and the technical means used are conventional means well known to those skilled in the art.

[0041] In the following examples, the mass ratio of nickel to aluminum in the nickel-aluminum alloy powder used is 8:2; the mass ratio of the nickel-aluminum mixed powder is 8:2.

[0042] Example 1

[0043] This embodiment provides a hydrogen production electrode, and the preparation method thereof includes: S1: Clean the surface of the nickel substrate with ethanol, acetone, etc., and after drying, plasma spray metal powder on the nickel substrate in an inert gas atmosphere. The metal powder is nickel-aluminum alloy powder, and the powder amount is regulated to 100 g / m2 by adjusting the speed of the spray gun.

[0044] S2: The pre-sprayed nickel substrate is cleaned with ethanol, acetone, etc., and then sandblasted and roughened with a sandblasting machine after drying. The sandblasting process parameters are: air pressure 0.4 MPa, sandblasting time 3 minutes, and the particle size of the corundum sand used for sandblasting is 120 mesh.

[0045] S3: In an inert gas atmosphere, the nickel-aluminum alloy powder in S1 is sprayed on the surface of the treated nickel substrate, with a powder amount of 250 g / m2.

[0046] S4: After dealumination activation in a 30 wt % KOH solution, the hydrogen production electrode is obtained.

[0047] Example 2

[0048] This embodiment provides a hydrogen production electrode, and the preparation method thereof is different from that of Embodiment 1 only in that the metal powders in S1 and S3 are replaced with nickel-aluminum mixed powders.

[0049] Example 3

[0050] This embodiment provides a hydrogen production electrode, and the preparation method thereof is different from that of Embodiment 1 only in that the sandblasting process parameters are: air pressure 0.5 MPa, sandblasting time 3 minutes, and corundum sand with a particle size of 150 mesh.

[0051] Example 4

[0052] This embodiment provides a hydrogen production electrode, and the preparation method thereof is different from that of Embodiment 1 only in that the metal powder in S1 and the metal powder in S3 are replaced with a mixed powder of nickel, aluminum and molybdenum, and the mass ratio of nickel, aluminum and molybdenum is 6:2:2.

[0053] Example 5

[0054] This embodiment provides a hydrogen production electrode, and the preparation method thereof is different from that of Embodiment 1 only in that the amount of powder applied in S1 is 150 g / m2, and the amount of powder applied in S3 is 200 g / m2.

[0055] Example 6

[0056] This embodiment provides a hydrogen production electrode, and the preparation method thereof is different from that of Embodiment 1 only in that the sandblasting process parameters are: air pressure 0.2 MPa, sandblasting time 3 minutes, and the particle size of the corundum sand used for sandblasting is 400 mesh.

[0057] Comparative Example 1

[0058] This comparative example provides a hydrogen production electrode, and the preparation method thereof is different from that of Example 1 only in that the metal powder in S3 is replaced by a mixed powder of nickel, aluminum and molybdenum in a mass ratio of 6:2:2.

[0059] Comparative Example 2

[0060] This comparative example provides a hydrogen production electrode, and its preparation method is different from that of Example 1 only in that: S1 is not included, that is, the sandblasted nickel mesh is directly used as the substrate, the nickel-aluminum alloy powder is sprayed by a plasma spraying device, and the hydrogen production electrode is obtained after dealumination and activation.

[0061] Test Example 1

[0062] The present invention further tests the bonding strength between the substrate electrode and the coating of the hydrogen production electrode prepared in the embodiment and the comparative example. The test results are shown in Table 1: Table 1

[0063] Among them, the electrode weight loss test method includes the following steps: 1. Weigh the weight of the electrode to be tested before the test; 2. Soak the electrode to be tested in a beaker filled with water, place the beaker in an ultrasonic machine, continue ultrasonication for 3 hours, and weigh the weight of the electrode after cleaning and drying; 3. Calculate the difference in electrode weight before and after the test, and further calculate to obtain the electrode weight loss percentage.

[0064] The results show that by optimizing the coating spraying process and controlling the consistency of the formula of the two sprayings, the hydrogen evolution performance of the electrode can be effectively guaranteed while further improving the bonding strength between the substrate electrode and the coating. Among them, compared with Example 4, since the amount of powder applied to the first coating (150 g / m2) and the amount of powder applied to the second coating (200 g / m2) in Example 4 are closer to 1:1 than in Example 1, the coating bonding strength is slightly worse than that in Example 1. Although Example 6 adopts the spraying process of this application, the sandblasting parameters adopt the conventional conditions of the prior art, and its coating bonding strength is worse than that in Example 1.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a hydrogen production electrode, It is characterized in that include: S1: performing a first spraying treatment on a substrate electrode so that a first coating is provided on the substrate electrode to obtain a first electrode; S2: sandblasting the first electrode to obtain a second electrode; S3: performing a second spraying treatment on the second electrode so that a second coating is provided on the second electrode to obtain a second electrode; S4: performing a dealumination activation treatment on the second electrode to obtain the hydrogen production electrode; The spraying powder in the first spraying process is the same as the spraying powder in the second spraying process.

2. The method for preparing the hydrogen production electrode according to claim 1, It is characterized in that The powder amount of the first coating layer is less than the powder amount of the second coating layer.

3. The method for preparing the hydrogen production electrode according to claim 1 or 2, It is characterized in that In the first spraying process and the second spraying process, the spraying powder includes nickel-aluminum alloy powder and / or nickel-aluminum mixed powder; preferably, the spraying powder also includes one or more of nickel powder, aluminum powder, iron powder, molybdenum powder, nickel-molybdenum mixed powder, nickel-iron alloy powder, and nickel-molybdenum alloy powder.

4. The method for preparing a hydrogen production electrode according to any one of claims 1 to 3, It is characterized in that The powder application amount of the first coating is 100-150 g / m2; the powder application amount of the second coating is 200-250 g / m2.

5. The method for preparing the hydrogen production electrode according to any one of claims 1 to 4, It is characterized in that During the sandblasting process, the spraying air pressure is controlled to be 0.4-0.5 MPa.

6. The method for preparing a hydrogen production electrode according to any one of claims 1 to 5, It is characterized in that In the sandblasting process, the particle size of the sandblasting is controlled to be 80-150 meshes.

7. The method for preparing a hydrogen production electrode according to any one of claims 1 to 6, It is characterized in that In the sandblasting process, the sandblasting time is 10 to 1200 seconds.

8. The method for preparing a hydrogen production electrode according to any one of claims 1 to 7, It is characterized in that The dealumination activation comprises: soaking in a 10-30wt% KOH or NaOH solution for 1-24 hours.

9. A hydrogen production electrode, It is characterized in that It is prepared by the preparation method of the hydrogen production electrode according to any one of claims 1 to 8.

10. Use of the hydrogen production electrode according to claim 9 in hydrogen evolution reaction.