Antibacterial nylon toothbrush filament with high bending recovery rate and preparation method thereof
Preparing toughening fillers through modified titanium oxide and combining them with nylon powder and antibacterial fillers solves the problem of easy breeding of bacteria and poor interface bonding performance of toothbrush filament materials, improves the bending recovery and antibacterial performance of toothbrush filaments, and extends the service life.
Patent Information
- Application Number
- CN202410987851.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-15
AI Technical Summary
Existing toothbrush filament materials are prone to breed bacteria and affect oral health, and the addition of antibacterial and antioxidant components leads to poor interface bonding performance and affects bending performance.
Modified titanium oxide is used to prepare toughening filler, combined with nylon powder, coupling agent and antibacterial filler, and is mixed and formed by screw extruder and spinneret cooling to improve the flexibility and antibacterial performance of toothbrush filaments.
Significantly improves the bending recovery performance and antibacterial ability of toothbrush filaments, prolongs service life and maintains good cleaning effect.
Smart Images

Figure BDA0004957982170000071 
Figure BDA0004957982170000072 
Figure BDA0004957982170000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical fiber monofilaments, and in particular to an antibacterial nylon toothbrush filament with a high bending recovery rate and a preparation method thereof. Background Art
[0002] A toothbrush is a tool people use to clean teeth and maintain oral hygiene. People usually add toothpaste to the toothbrush when brushing their teeth for better cleaning. Therefore, the quality of the toothbrush is related to the oral hygiene and even physical health of the user. The mouth and teeth are one of the main portals for bacteria to invade the human body, and the toothbrush is in contact with the teeth and the internal environment of the mouth for a long time. Food residues and bacteria will inevitably enter the toothbrush wire. In addition, the toothbrush is placed in a relatively humid bathroom for a long time, which makes it easy for bacteria to grow in the toothbrush wire, which is not conducive to the long-term use of the toothbrush.
[0003] The commonly used toothbrush filaments in the prior art all use PA filaments or PBT filaments. Both materials are chemical fibers and do not have antibacterial function. They are easy to breed various bacteria on the surface and affect the oral health of users. In order to give the toothbrush filaments the antibacterial function when in use, the publication number CN108359236A provides an antibacterial toothbrush, in which the toothbrush bristles used use polyamide and polyethylene terephthalate as plastic substrates, and add 3-(methacryloyloxy)propyltrimethoxysilane modified magnesium powder, Eucalyptus globulus leaf extract, wax gourd seed extract and tea polyphenols to synergistically play an antibacterial role. In addition, pomegranate peel extract is added to play an antioxidant role. However, adding too much filler and antibacterial and antioxidant components in the toothbrush filaments easily leads to poor interface bonding performance of the toothbrush filaments, which will affect the anti-bending performance of the toothbrush filaments themselves. Therefore, it is urgent to provide a solution to improve the above problems. Summary of the invention
[0004] The object of the present invention is to provide an antibacterial nylon toothbrush filament with a high bending recovery rate and a preparation method thereof, and the bending recovery performance of the nylon toothbrush filament can be effectively improved by modifying the toughening filler.
[0005] In a first aspect, the present invention provides an antibacterial nylon toothbrush filament with high bending recovery rate, which comprises, by weight: 60-80 parts of nylon powder, 5-8 parts of coupling agent, 1-5 parts of antibacterial filler and 1-5 parts of toughening filler; wherein the preparation method of the toughening filler comprises: immersing modified titanium oxide in a polyphenol solution and stirring it, and then separating and drying it to obtain the toughening filler.
[0006] The toothbrush filaments provided by the present invention use common polyamide materials as raw materials, which have good wear resistance and chemical stability. After being formed into toothbrush filaments, they can effectively maintain the cleaning effect on teeth for a long time. The coupling agent can improve the interface bonding performance between the toughening filler and the antibacterial filler in the nylon, thereby improving the overall flexibility and structural stability of the toothbrush filaments. The antibacterial filler can effectively improve the antibacterial ability of the toothbrush filaments. In addition, after the toughening filler is modified with polyphenols, not only the bending recovery performance of the toothbrush filaments can be improved, but also the antibacterial performance of the antibacterial filler can be promoted.
[0007] Optionally, when the modified titanium oxide is immersed in a polyphenol solution, the preparation method of the modified titanium oxide includes the following steps: mixing titanium oxide and a modifier, dispersing them in an activation solution, stirring and mixing, and then separating and drying to obtain activated titanium oxide; stirring and mixing activated titanium oxide and polyethylene glycol, and then separating and drying to obtain modified titanium oxide.
[0008] Optionally, the mass ratio of titanium oxide to modifier is 1:(0.5-0.6).
[0009] Optionally, the modifier includes at least one of neopentyl glycol and pentaerythritol.
[0010] Optionally, the solute of the activation solution includes at least one of sodium dodecylbenzenesulfonate and hexadecyltrimethylammonium bromide.
[0011] Optionally, when the activated titanium oxide and the polyethylene glycol are stirred and mixed, the mass ratio of the activated titanium oxide to the polyethylene glycol is 1:(1-2).
[0012] Optionally, the coupling agent includes at least one of vinyl triethoxy silane, γ-aminopropyl triethoxy silane, and γ-glycidyl propoxy trimethoxy silane.
[0013] Optionally, the antibacterial filler includes at least one of nanosilver particles and graphene oxide, and the average particle size of the antibacterial filler is 10-50 nm.
[0014] Optionally, the nylon powder includes at least one of nylon 6, nylon 66, PA612, and PA12.
[0015] In a second aspect, the present invention also provides a method for preparing toothbrush filaments, comprising the following steps: mixing nylon powder, a coupling agent, a toughening filler and an antibacterial filler in a screw extruder, sequentially passing through extrusion zones of 240°C, 245°C, 255°C, 265°C and 270°C, and then spinning and cooling to form toothbrush filaments. DETAILED DESCRIPTION
[0016] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meanings understood by people with general skills in the field to which the present invention belongs.
[0017] The present invention provides an antibacterial nylon toothbrush filament with a high bending recovery rate, which comprises, by weight, 60-80 parts of nylon powder, 5-8 parts of coupling agent, 1-5 parts of antibacterial filler and 1-5 parts of toughening filler. Specifically, nylon, as the main material of the toothbrush filament, can provide the toothbrush filament with basic elasticity, flexibility and wear resistance. In addition, nylon also has good chemical stability. Therefore, when the toothbrush filament is used with toothpaste to clean the surface of teeth, the toothbrush filament can maintain its own structural stability for a long time. In addition, after the coupling agent is added, the interface bonding ability of each component in the toothbrush filament can be well balanced, thereby improving the structural stability of the toothbrush filament.
[0018] In fact, the addition of antibacterial fillers can give the toothbrush filaments antibacterial function, which can not only improve the toothbrush filaments' ability to inhibit or kill bacteria in the oral cavity, but also improve the surface antibacterial ability of the toothbrush filaments when stored in a humid environment, thereby preventing bacteria from multiplying on the surface or in the gaps of the toothbrush filaments, and improving the long-term performance and surface cleanliness of the toothbrush filaments.
[0019] Specifically, the preparation method of the toughened filler includes: immersing the modified titanium oxide in a polyphenol solution, stirring, separating and drying to obtain the toughened filler. In fact, immersing the modified titanium oxide in the polyphenol solution can graft polyphenol substances on the surface of the modified titanium oxide, which can not only improve the dispersion ability of titanium oxide in the toothbrush filaments, but also effectively improve the flexibility of the toothbrush filaments, thereby giving the toothbrush filaments higher bending recovery performance, so that the toothbrush filaments can clean the tooth surface at a larger angle when brushing teeth.
[0020] Specifically, the polyphenols dissolved in the polyphenol solution include at least one of tannic acid, tannic acid, and proanthocyanidins. In fact, when the modified titanium oxide is immersed in the polyphenol solution, the mass ratio of the modified titanium oxide to the polyphenol solute in the polyphenol solution is 1:(0.3-0.5).
[0021] In some embodiments, the preparation method of modified titanium oxide includes the following steps: mixing titanium oxide and a modifier in an activation solution, stirring and mixing, separating and drying to obtain activated titanium oxide; stirring and mixing activated titanium oxide and polyethylene glycol, separating and drying to obtain modified titanium oxide.
[0022] In some embodiments, when titanium oxide and a modifier are mixed and dispersed, the mass ratio of titanium oxide to the modifier is 1:(0.5-0.6). Specifically, the titanium oxide used is nano titanium oxide, and its average particle size ranges from 10 to 50 nm. Specifically, the modifier used includes at least one of neopentyl glycol and pentaerythritol.
[0023] In some embodiments, when titanium oxide and a modifier are mixed and dispersed in an activation solution, the solute of the activation solution used includes at least one of sodium dodecylbenzene sulfonate and hexadecyltrimethylammonium bromide. In fact, the solvent in the activation solution can be any organic solvent that can dissolve sodium dodecylbenzene sulfonate and hexadecyltrimethylammonium bromide.
[0024] In some embodiments, when the activated titanium oxide and the polyethylene glycol are stirred and mixed, the mass ratio of the activated titanium oxide to the polyethylene glycol is 1:(1-2). In fact, the weight average molecular weight of the polyethylene glycol used is 2000.
[0025] In some embodiments, the coupling agent includes at least one of vinyl triethoxysilane, γ-aminopropyl triethoxysilane, and γ-glycidyl propoxy trimethoxy silane, the antibacterial filler includes nanosilver particles or graphene oxide with an average particle size of 10-50 nm, and the nylon raw material includes at least one of nylon 6, nylon 66, nylon 612 and nylon 610.
[0026] In fact, the present invention also provides a method for preparing toothbrush filaments, comprising the following steps: mixing nylon raw materials, coupling agents, toughening fillers and antibacterial fillers in a screw extruder, passing through extrusion zones of 240°C, 245°C, 255°C, 265°C and 270°C in sequence, and then spinning and cooling to form toothbrush filaments.
[0027] Example 1 to Example 3
[0028] Embodiments 1 to 3 of the present invention respectively provide an antibacterial nylon toothbrush filament with a high bending recovery rate, and the specific components and amounts thereof are shown in Table 1 below.
[0029] Table 1 Components and dosages of Examples 1 to 3
[0030] Example 1 Example 2 Example 3 nylon 60 70 80 Coupling agent 5 7 8 Antibacterial filler 1 3 5 Toughening filler 1 2 5
[0031] The nylon raw material used in Examples 1 to 3 is selected from Arkema PA12, the coupling agent used is vinyl triethoxysilane (purchased from Maclean Reagent with item number T818810), and the antibacterial filler used is nano silver particles (purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.).
[0032] The preparation method of the toughening filler used in Examples 1 to 3 comprises the following steps:
[0033] S1. Titanium oxide (purchased from Brofos Nanotechnology (Ningbo) Co., Ltd., model Brofos-TiO2) and neopentyl glycol (CAS: 126-30-7) were mixed at a mass ratio of 1:0.5, and then put into an activation solution (mass ratio of titanium oxide to sodium dodecylbenzene sulfonate is 1:0.2) dissolved with sodium dodecylbenzene sulfonate (Shanghai Shengzhong Fine Chemical Co., Ltd.), and ultrasonically mixed at a frequency of 20 kHz, filtered and separated, washed with deionized water and anhydrous ethanol, and then transferred to a vacuum drying oven at 80°C for drying to obtain activated titanium oxide;
[0034] S2, after the activated titanium oxide and polyethylene glycol 2000 (PEG2000 of Hai'an Petrochemical Plant, Jiangsu Province) were mixed at a mass ratio of 1:1.5, the mixture was stirred at 50°C for 12 hours, and then filtered and separated, and the mixture was transferred to 40°C and dried to constant weight to obtain modified titanium oxide;
[0035] S3. Immerse the modified titanium oxide in the proanthocyanidin solution (the mass ratio of modified titanium oxide to proanthocyanidin is 1:0.4), and disperse it ultrasonically at 45°C for 30 minutes, filter it out and wash it with anhydrous ethanol, then transfer it to a 50°C vacuum drying oven and dry it to constant weight to obtain a toughened filler.
[0036] The preparation method of antibacterial nylon toothbrush filaments with high bending recovery rate in Examples 1 to 3 comprises the following steps: loading nylon raw material, coupling agent, antibacterial filler and toughening filler into the feeding system of the screw extruder, and pre-mixing the raw materials in the metering mixing system, and then passing through the extrusion zones of 240°C, 245°C, 255°C, 265°C and 270°C in sequence, and then spinning and cooling to form the toothbrush filaments.
[0037] Comparative Example 1
[0038] This comparative example 1 provides a nylon toothbrush filament, which is different from Example 2 in that no toughening filler is added in comparative example 1.
[0039] Comparative Example 2
[0040] This comparative example 2 provides a nylon toothbrush filament, which is different from Example 2 in that no antibacterial filler is added in comparative example 2.
[0041] Comparative Example 3
[0042] This comparative example 3 provides a nylon toothbrush filament, which is different from Example 2 in that, when preparing the toughening filler, the comparative example 3 does not perform step S3, and the modified titanium oxide prepared in step S2 is used as the toughening filler.
[0043] Performance Testing
[0044] After the nylon toothbrush filaments prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were sterilized at 150°C under high pressure, 100 cfu / mL of Escherichia coli and Staphylococcus aureus were added respectively, and treated at 25°C for 10 hours. The liquid was aspirated for pouring culture to count the live bacteria and calculate the sterilization rate. The nylon toothbrush filaments were then immersed in a saturated sucrose solution at 40°C for 12 hours, and the above sterilization rate test was repeated. The results are shown in Table 2 below.
[0045] The nylon toothbrush filaments prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were respectively made into standard toothbrushes of the same specifications, and a lodging ratio test was performed at a speed of 13 mm / s using a weight of 335 g on the toothbrush filaments. The test time was 24 hours, and the test was repeated five times to take the average value. The lodging ratios are shown in Table 3 below. After the nylon toothbrush filaments were aged in an oxygen atmosphere at 50°C for 48 hours, the lodging test was repeated, and the results are shown in Table 3 below.
[0046] Table 2 Sterilization rate test
[0047]
[0048] Table 3 Rebound rate test
[0049]
[0050]
[0051] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. An antibacterial nylon toothbrush filament with high bending recovery rate, It is characterized in that The composition comprises, by weight, 60-80 parts of nylon powder, 5-8 parts of coupling agent, 1-5 parts of antibacterial filler and 1-5 parts of toughening filler. The preparation method of the toughening filler comprises: immersing the modified titanium oxide in a polyphenol solution, stirring the solution, and then separating and drying the solution to obtain the toughening filler.
2. The toothbrush filament according to claim 1, It is characterized in that When the modified titanium oxide is immersed in a polyphenol solution, the preparation method of the modified titanium oxide comprises the following steps: mixing titanium oxide and a modifier in an activation solution, stirring and mixing, separating and drying to obtain activated titanium oxide; stirring and mixing activated titanium oxide and polyethylene glycol, separating and drying to obtain modified titanium oxide.
3. The toothbrush filament according to claim 2, It is characterized in that The mass ratio of the titanium oxide to the modifier is 1:(0.5-0.6).
4. The toothbrush filament according to claim 2, It is characterized in that The modifier includes at least one of neopentyl glycol and pentaerythritol.
5. The toothbrush filament according to claim 2, It is characterized in that The solute of the activation solution includes at least one of sodium dodecylbenzenesulfonate and hexadecyltrimethylammonium bromide.
6. The toothbrush filament according to claim 2, It is characterized in that When the activated titanium oxide and the polyethylene glycol are stirred and mixed, the mass ratio of the activated titanium oxide to the polyethylene glycol is 1:(1-2).
7. The toothbrush filament according to claim 1, It is characterized in that The coupling agent includes at least one of vinyl triethoxysilane, γ-aminopropyl triethoxysilane, and γ-glycidyl propoxy trimethoxysilane.
8. The toothbrush filament according to claim 1, It is characterized in that The antibacterial filler comprises at least one of nano silver particles and graphene oxide, and the average particle size of the antibacterial filler is 10-50 nm.
9. The toothbrush filament according to claim 1, It is characterized in that The nylon powder includes at least one of nylon 6, nylon 66, PA612 and nylon 610.
10. A method for preparing toothbrush filaments according to any one of claims 1 to 9, It is characterized in that The following steps are involved: Nylon powder, coupling agent, toughening filler and antibacterial filler are mixed in a screw extruder, and then passed through extrusion zones of 240° C., 245° C., 255° C., 265° C. and 270° C., and then spun, cooled and formed into toothbrush filaments.
Citation Information
Patent Citations
Antibacterial nylon stretch yarn
CN106637474A
Preparation method for self-cleaning antibacterial paint based on modification of nanometer titanium dioxide
CN106939135A
Method for preparing graphene-containing antibacterial reinforced and toughened nylon toothbrush filament
CN108113200A
Cited By
Antibacterial and deodorant nylon fabric and preparation method thereof
CN120592042A