Novel SERS-Apt sensor for detecting Tau protein and use method of novel SERS-Apt sensor

The SERS-Apt sensor constructed using Fe3O4@PEI/Ag nanoparticles and DNA hybridization indicator methylene blue solves the problems of complex and low sensitivity detection methods for Tau protein, achieving rapid and accurate detection, and is suitable for Alzheimer's disease. Early diagnosis.

CN118777280APending Publication Date: 2024-10-15GUANGXI UNIVERSITY OF TECHNOLOGY +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310360107.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing Tau protein detection methods have complex steps, are time-consuming, have low sensitivity, and lack fast and accurate detection methods.

Method used

Fe3O4@PEI/Ag nanoparticles were used as the SERS capture substrate, combined with the DNA hybridization indicator methylene blue (MB) as the probe, to construct a SERS-Apt sensor for Tau protein, which achieved detection through specific binding and release of signal molecules.

Benefits of technology

It achieves rapid, sensitive and accurate detection of Tau protein, with a detection limit of 0.18 pg/mL. It has the characteristics of simple preparation, strong specificity and good reproducibility, and is suitable for early diagnosis and screening of Alzheimer's disease.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118777280A_ABST
    Figure CN118777280A_ABST
Patent Text Reader

Abstract

The invention relates to a novel SERS-Apt sensor for detecting Tau protein and a use method of the novel SERS-Apt sensor, Fe3O4-coated PEI / Ag nanoparticles (Nc) are constructed to serve as an SERS capture substrate, a DNA hybridization indicator methylene blue (MB) serves as an SERS probe, and the SERS-Apt sensor for the Tau protein is successfully constructed. The Tau protein concentration and the SERS signal intensity of the sensor prepared by the invention have a good linear relationship, and the limit of detection (LOD) is 0.18 pg / mL. A labeling test is carried out on a human serum sample, and the recovery rate and the relative standard deviation (RSD) are 80%-107% and 1.4%-5.7% respectively. The novel sensor has the characteristics of simplicity in preparation, high specificity, rapidness in detection, sensitivity and the like, and has a certain application prospect in the aspect of early diagnosis and screening of the Alzheimer's disease.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of surface enhanced Raman detection technology, and in particular to a novel SERS-Apt sensor for detecting Tau protein and a use method thereof. Background Art

[0002] Alzheimer's disease (AD) is relatively common. Studies on neurodegenerative diseases have shown that Tau protein, as one of the biomarkers of AD, has important research significance in the clinical diagnosis and intervention treatment of the disease. Therefore, it is crucial to develop a highly sensitive, simple and rapid method for quantitatively detecting Tau protein. At present, the detection methods for Tau protein mainly include electrochemical method, immunoassay, fluorescence method, etc., but these methods have some shortcomings, such as complex steps, time-consuming, and low sensitivity. Therefore, it is necessary to develop a new method for rapid, sensitive and accurate Tau protein detection.

[0003] SERS technology has the characteristics of high sensitivity, rapidity, non-destructiveness, fingerprint recognition, and no interference from water molecules. The preparation of highly active and uniform signal SERS substrates is the key to SERS detection technology. Usually, rough surface precious metal nanostructures such as nano-gold and silver are used as Raman enhancement substrates. The effect can also be enhanced or the signal uniformity can be improved by regulating the structure and morphology. Magnetic precious metal nanoparticles have the characteristics of simple preparation, good dispersibility, high enhancement factor, etc., and can separate and enrich target substances from complex sample liquids. Therefore, they are widely used as SERS substrates.

[0004] Methylene blue (MB) is a commonly used DNA hybridization indicator in electrochemistry and can intercalate with double-stranded DNA (dsDNA). 3 O 4 @GO@Ag was used as the Raman substrate to quantitatively detect MB, and MB showed a good Raman effect. Aptamers are single-stranded fragments of DNA or RNA. Compared with traditional protein antibodies, they have the advantages of strong specificity, high stability, chemical synthesis, and easy modification. They are widely used in analytical chemistry, biosensors, and medical diagnosis. However, most SERS-Apt sensors require chemical labeling of Raman signal molecules, and this chemical labeling method is generally time-consuming. MB can be embedded in the double-stranded structure composed of the aptamer and its complementary chain. Based on this, a chemical labeling-free SERS-Apt sensor can be developed. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a novel SERS-Apt sensor for detecting Tau protein and a method for using the same, and to construct a Fe 3 O 4@PEI / Ag nanoparticles (Nc) were used as SERS capture substrates and DNA hybridization indicator methylene blue (MB) was used as SERS probe to successfully construct a SERS-Apt sensor for Tau protein. This new sensor has the characteristics of simple preparation, strong specificity, rapid and sensitive detection, etc.

[0006] The technical solution to the above technical problem is: a new SERS-Apt sensor for detecting Tau protein, which is prepared by the following method: (1) Preparation of Fe 3 O 4 @PEI / Ag magnetic SERS substrate: ①Fe 3 O 4 Preparation of @PEI: 8-12g of nano-Fe 3 O 4 The particles were dispersed in 10-25 mL ultrapure water, sonicated for 5-15 minutes, and then 8-12 mL of 5 mg / mL PEI solution was added. After sonication for 25-35 minutes, the particles were separated by magnetic separation and washed with ultrapure water to obtain Fe 3 O 4 @PEI particle suspension; ② Preparation of Au seeds: Take 1 mL of 1% HAuCl 4 The solution was added to 99 mL of water and stirred magnetically for 10 to 20 min. Then, 1 mL of 1% Na 3 Cit solution, continue stirring for 1 to 5 minutes, then add 1 mL of 0.075% NaBH dropwise 4 With 1 mL of 1% Na 3 The mixed solution of Cit was magnetically stirred for 25-35 min to obtain Auseeds; ③Fe 3 O 4 Preparation of @PEI-Au seeds: Add the negatively charged colloidal gold Au seeds prepared in step ② to the positively charged Fe 3 O 4 @PEI particle suspension, ultrasonic for 25-35 minutes, magnetic separation and ultrapure water washing to obtain Fe 3 O 4 @PEI-Au seed particles are dispersed in 50 mL ultrapure water for later use; ④Fe 3 O 4 Preparation of @PEI / Ag Nc: Take 10 mL of Fe prepared in step ③ 3 O 4@PEI-Au seeds were added to 100 mL ultrapure water and ultrasonicated for 5-15 min. 100 mg PVP and 1.5 mg AgNO were added. 3 , ultrasonically treated for 2-5 min, quickly added 150 μL formaldehyde and 150 μL ammonia water, ultrasonically reacted for 3-8 min, magnetically separated, washed with ultrapure water, and dissolved in 50 mL PBS buffer to obtain Fe 3 O 4 @PEI / Ag Nc suspension; (2) Preparation of SERS-Apt sensor: In 50 μL Fe 3 O 4 Add 5 μL of 50 μM SH-Apt solution and 5 μL of 50 μM cDNA solution to the PEI / Ag Nc suspension, mix well, incubate overnight at room temperature for 12-15 hours, and wash with PBS buffer after magnetic separation; add 20 μL of 1×10 -5 mol / L MB solution was incubated at room temperature for 5-7 h, washed with PBS buffer after magnetic separation, and dispersed in 50 μL PBS buffer to obtain Tau protein SERS-Apt sensor.

[0007] Furthermore, the nucleotide sequence of SH-Apt is: 3'-SH-GCG GAG CGA GGC AGG; and the nucleotide sequence of cDNA is: CGC CTC GCA CCG TCC.

[0008] Furthermore, nano-Fe 3 O 4 The particles were synthesized using the following method: ① Weigh 2.7g FeCl 3 6H 2 O was dissolved in 80 mL of ethylene glycol and stirred vigorously for 30 min to completely dissolve; ② Weigh 5.4g sodium acetate and 2g PEG6000 and add them to the above solution, continue stirring for 1 hour and mix well; ③ Transfer to a high-pressure reactor and place in a 210℃ forced air oven for reaction for 10 hours, then close the oven and wait for the product to cool to room temperature. The obtained black precipitate is washed with ultrapure water and ethanol respectively, and placed in a vacuum drying oven at 60℃ for drying. The obtained product is nano-Fe 3 O 4 Particles.

[0009] Another technical solution of the present invention is: a method for using the novel SERS-Apt sensor for detecting Tau protein prepared by the above method, comprising the following steps: (1) Drawing a working curve: 10 μL of Tau protein standard solution of different concentrations was added to multiple SERS-Apt sensors respectively. After incubation at room temperature for 45 min, the sensors were fully washed with PBS buffer and dried naturally. The Raman spectra were collected and the Tau protein working curve was drawn. (2) Add 10 μL of the Tau protein sample to be tested onto the SERS-Apt sensor, incubate for 45 min, wash thoroughly with PBS buffer and dry naturally, and collect its Raman spectrum; calculate the Tau protein concentration using the Tau protein working curve.

[0010] Furthermore, the working curve in step (1) is: y=-95.5x+10523.7, R 2 =0.993, y represents 1624cm -1 The SERS signal intensity is shown in Figure 2, and x represents the Tau protein concentration.

[0011] The present invention prepares Fe 3 O 4 @PEI / Ag Nc, and modified the thiol-modified Tau protein aptamer (SH-Apt), the complementary chain (cDNA) and SH-Apt formed dsDNA, and the signal probe MB was embedded in dsDNA. When Tau protein was present in the system, Tau protein specifically bound to SH-Apt, resulting in the dissociation of the dsDNA structure, the release of the signal molecule MB, and the weakening of the Raman signal intensity; as the concentration of Tau protein increased, the Raman signal intensity further decreased. Based on this, the SERS-Apt sensor of Tau protein was successfully constructed. Its principle is as follows Figure 1 The experimental results show that the SERS-Apt sensor has the advantages of high sensitivity, good reproducibility and stability, and has good application prospects in the detection of Tau protein.

[0012] The present invention constructs Fe 3 O 4 @PEI / Ag nanoparticles (Nc) were used as SERS capture substrates and DNA hybridization indicator methylene blue (MB) was used as SERS probe to successfully construct a SERS-Apt sensor for Tau protein. -1 There is a good linear relationship between the SERS intensity at 1 pg / mL and the Tau protein concentration (1 pg / mL-70 pg / mL) (R 2 =0.993), with a limit of detection (LOD) of 0.18 pg / mL. The recovery rate and relative standard deviation (RSD) of spiked human serum samples were 80%-107% and 1.4%-5.7%, respectively. This new sensor has the characteristics of simple preparation, strong specificity, rapid detection and sensitivity, and has certain application prospects in the early diagnosis and screening of Alzheimer's disease.

[0013] The technical features of a novel SERS-Apt sensor for detecting Tau protein according to the present invention are further described below in conjunction with the accompanying drawings and examples. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 : Schematic diagram of the detection principle of the present invention.

[0015] Figure 2 :Use TEM and SEM to analyze Fe 3 O 4 @PEI / Ag Nc SERS substrate characterization pictures. A is Fe 3 O 4 TEM image of nanoparticles; B is Fe 3 O 4 TEM image of @PEI; C is Fe 3 O 4 TEM image of @PEI-Au seed; D is Fe 3 O 4 SEM image of @PEI / Ag Nc.

[0016] Figure 3 :Fe 3 O 4 XRD characterization diagram of @PEI / Ag Nc.

[0017] Figure 4 : Working curve of the sensor of the present invention for detecting Tau protein standard solutions with different concentrations.

[0018] Figure 5 : SERS spectra of the sensor of the present invention detecting Tau protein standard solutions with different concentrations.

[0019] Figure 6 : The detection result diagram of the sensor of the present invention detecting different types of proteins respectively.

[0020] Figure 7 : Graph showing the uniformity test results of the Tau protein SERS-Apt sensor of the present invention.

[0021] Figure 8 : Graph showing the reproducibility test results of the Tau protein-SERS aptamer sensor of the present invention.

[0022] Fig. 9 : Graph showing the stability test results of the Tau protein SERS-Apt sensor of the present invention. DETAILED DESCRIPTION

[0023] The reagents used in the present invention are as follows: Ferric chloride (FeCI3·6H 2 O) (AR, Tianjin Komiou Chemical Reagent Co., Ltd.); silver nitrate (AgNO3) (AR, Sinopharm Chemical Reagent Co., Ltd.); ethylene glycol (AR, Guangdong Guanghua Science and Technology Co., Ltd.), polyethylene glycol 6000 (CP, Xilong Chemical Co., Ltd.); ammonia 28% (AR, Xilong Science Co., Ltd.); polyvinyl pyrrolidone (PVP) (CR, Sinopharm Chemical Reagent Co., Ltd.); methylene blue (MB, Chengdu Kelong Chemical Co., Ltd.); phosphate buffer solution (PBS, PH 7.2 Guangdong Huankai Microbiology Technology Co., Ltd.); human serum (Shanghai Jinghang Biological).

[0024] The thiolated Tau protein aptamer (SH-Apt) (3'-SH-GCG GAG CGA GGC AGG), complementary chain (cDNA) (CGC CTC GCA CCG TCC), and Tau protein standard were purchased from Sangon Biotech Co., Ltd. (Shanghai, China). The DNA solution was prepared with PBS buffer at a concentration of 50 μM and stored frozen before use. Example 1

[0025] A novel SERS-Apt sensor for detecting Tau protein is prepared by the following method: (1) Preparation of Fe 3 O 4 @PEI / Ag magnetic SERS substrate: ①Nano-Fe 3 O 4 Synthesis method: A. Weigh 2.7 g FeCl 3 6H 2 O was dissolved in 80 mL of ethylene glycol and stirred vigorously for 30 min to allow it to dissolve completely.

[0026] B. Weigh 5.4g sodium acetate and 2g PEG6000 and add them to the above solution. Continue stirring for 1 hour to mix well.

[0027] C, transferred to a high-pressure reactor (polytetrafluoroethylene liner), and placed in a 210°C forced air oven for reaction for 10 hours, then the oven was closed, and the product was cooled to room temperature. The obtained black precipitate was washed with ultrapure water and ethanol for 3 times respectively, and placed in a vacuum drying oven at 60°C for drying. The obtained product was nano-Fe 3 O 4 Particles.

[0028] ②Fe 3 O 4Preparation of @PEI: The above nano-Fe 3 O 4 The particles were dispersed in 20 mL ultrapure water, sonicated for 10 minutes, and 10 mL of 5 mg / mL PEI solution was added. After sonication for 30 minutes, the particles were magnetically separated and washed with ultrapure water for 5 times to obtain Fe 3 O 4 @PEI particle suspension.

[0029] ③ Preparation of Au seeds: Take 1 mL HAuCl 4 The solution (1%) was added to 99 mL of water and stirred magnetically for 15 min before adding 1 mL of Na 3 Cit solution (1%), continue stirring for 2 min, and then add 1 mL of NaBH 4 (0.075%) with 1 mLNa 3 The mixed solution of Cit (1%) was magnetically stirred for 30 min to obtain Au seeds.

[0030] ④Fe 3 O 4 Preparation of @PEI-Au seeds: Add the negatively charged colloidal gold Au seeds prepared above to the positively charged Fe 3 O 4 @PEI particle suspension, ultrasonic for 30 minutes, magnetic separation and washing with ultrapure water for 3 times to obtain Fe 3 O 4 @PEI-Au seed particles are dispersed in 50 mL ultrapure water for later use.

[0031] ⑤Fe 3 O 4 Preparation of @PEI / Ag Nc: Take 10 mL of Fe 3 O 4 @PEI-Au seeds were added to 100 mL ultrapure water and sonicated for 10 min. 100 mg PVP and 1.5 mg AgNO 3 , ultrasonic for 5 min, quickly add 150 μL formaldehyde and 150 μL ammonia water, ultrasonically react for 5 min, magnetically separate, wash with ultrapure water 3 times, and dissolve in 50 mL PBS buffer to obtain Fe 3 O 4 @PEI / Ag Nc suspension.

[0032] (2) Preparation of Tau protein SERS-Apt sensor: In 50 μL Fe 3 O 45 μL of 50 μM SH-Apt solution and 5 μL of 50 μM cDNA solution were added to the PEI / Ag Nc suspension, mixed evenly, incubated at room temperature for 12 h, and washed three times with PBS buffer after magnetic separation; 20 μL of 1×10 -5 mol / L MB solution was incubated at room temperature for 6 h, washed three times with PBS buffer after magnetic separation, and dispersed in 50 μL PBS buffer to obtain the Tau protein SERS-Apt sensor. Example 2

[0033] The method for using the novel SERS-Apt sensor for detecting Tau protein prepared in Example 1 comprises the following steps: (1) Drawing the working curve: 10 μL of Tau protein standard solution of different concentrations was added to multiple SERS-Apt sensors respectively. After incubation for 45 min, the sensors were fully washed with PBS buffer and dried naturally. The Raman spectra were collected and the Tau protein working curve was drawn. The Tau protein working curve is: y=-95.5x+10523.7, R 2 =0.993, y represents 1624cm -1 The SERS signal intensity is shown in Figure 2, and x represents the Tau protein concentration.

[0034] (2) 10 μL of the Tau protein sample to be tested was added to the SERS-Apt sensor. After incubation for 45 min, the sensor was washed thoroughly with PBS buffer and dried naturally. The Raman spectrum was collected (Raman instrument parameters: Grating 600 gr / mm, wavelength 638 nm, power 37.5 mW, integration time 10 s, Filter: 10%). The Tau protein concentration was calculated using the Tau protein working curve.

[0035] The following is a description of the development process of this invention: 1. Fe 3 O 4 Characterization of @PEI / AgNc SERS substrate.

[0036] Fe 3 O 4 @PEI / Ag Nc SERS substrate was characterized, and the results are as follows Figure 2 shown. Figure 2 A is Fe 3 O 4 TEM image of nanoparticles shows that Fe 3 O 4 The nanoparticles are uniformly spherical. Figure 2 B is Fe 3 O4 TEM image of @PEI, where Fe 3 O 4 @PEI nanoparticles have a transparent PEI layer on their surface with a thickness of approximately 2.5 nm. Figure 2 C is Fe 3 O 4 @The TEM image of PEI-Au seed shows that a layer of gold nanoparticles was adsorbed on the surface of the previous PEI layer, making it opaque. Figure 2 D is Fe 3 O 4 SEM image of @PEI / Ag Nc shows that abundant nano-Ag is deposited on the Fe 3 O 4 @PEI outer layer, forming a uniform Fe 3 O 4 @PEI / Ag Nc. The above results show that Fe 3 O 4 @PEI / Ag Nc was successfully prepared and the distribution was relatively uniform.

[0037] 2. Fe 3 O 4 XRD characterization of @PEI / AgNc.

[0038] Figure 3 Fe 3 O 4 XRD spectrum of @PEI / Ag Nc. Figure 3 It can be seen that there are significant Fe 3 O 4 Characteristic peaks, according to the standard card (PDF 65-3107), are Fe 3 O 4 (112), (221), (220), (303), (224) crystal planes. Four new significant characteristic peaks appeared at 2θ of 38.2°, 44.3°, 64.5°, and 77.5°. According to the standard card (PDF 04-0783), they are the (111), (200), (220), and (311) crystal planes of Ag. The XRD characteristic peaks further prove that Fe 3 O 4 Successful preparation of @PEI / Ag Nc substrate.

[0039] 3. Fe 3 O 4 Raman enhancement factor (EF) of @PEI / AgNc SERS substrate.

[0040] MB at 1624cm-1 The SERS signal intensity at the substrate Fe 3 O 4 @PEI / Ag Nc Raman enhancement effect, according to the formula

[0041] Calculate the enhancement factor (EF), where I SERS ——MB Raman intensity on the substrate material; I bare ——MB Raman intensity on bare glass slide; C SERS ——MB concentration on the substrate material; C bare ——MB concentration on bare glass slide.

[0042] The experimental results show that Fe 3 O 4 @PEI / AgNc substrate detection MB concentration and its SERS signal intensity are C SERS =1×10 -7 mol / L,I SERS =6089.6; MB concentration and SERS signal intensity detected on bare glass slide are C bare =1.0 mol / L, I bare =275. Substituting into the above formula, EF is 2.2×10 8 , indicating that the Fe prepared by the present invention 3 O 4 @PEI / Ag Nc has a good SERS enhancement effect, which provides the possibility for the subsequent high-sensitivity detection of Tau protein-SERS aptamer sensors.

[0043] 4. Working curve of SERS-Apt sensor detecting Tau protein standard solution.

[0044] The SERS-Apt sensor prepared by the present invention was used to detect Tau protein standard solutions of different concentrations. The working curve is shown in FIG. Figure 4 As shown, the linear fitting equation is: y=-95.5x+10523.7, R 2 =0.993 (y represents 1624cm -1 The SERS signal intensity of the Tau protein standard is shown in Figure 2, where x represents the Tau protein concentration. According to the 3σ / m standard proposed by IUPAC, the detection limit is estimated to be 0.18 pg / mL. The SERS spectra of the Tau protein standard solutions with different concentrations are shown in Figure 2. Figure 5 As shown in the figure, in the range of 1-70 pg / mL, as the concentration of Tau protein standard solution increases, the sensor-1 The SERS signal intensity gradually decreases. Compared with the conventional Tau protein detection method ELISA, the SERS-Apt sensor prepared by the present invention has a lower detection limit.

[0045] 5. Selectivity of Tau protein SERS-Apt sensor.

[0046] The sensor was used to detect 10 μL 1 pg / mL AchE, BsA, HsA, LpL, IgG, standard solution, and PBS as a blank control. The results are shown in Figure 6 As shown, except for the target protein Tau protein, the detection results of other proteins are similar to those of the blank sample, which proves that the sensor has specific recognition function for the target protein Tau protein and has good selectivity.

[0047] 6. Uniformity of Tau protein SERS-Apt sensor.

[0048] 10 μL of 30 pg / mL Tau protein standard solution was tested, and 15 different sample points were collected. The results are summarized as follows: Figure 7 As shown, the relative standard deviation (RSD) is 1.7%, which proves that the sensor has good uniformity.

[0049] 7. Reproducibility of SERS-Apt sensor in detecting Tau protein standard solution.

[0050] The present invention conducted the following two reproducibility experiments. Experiment 1: Five parallel experiments were conducted on 10 μL of 10 pg / mL Tau protein standard solution. The test results are as follows: Figure 8 As shown in Figure A, the relative standard deviation (RSD) is 2%. In Experiment 2, 10 μL of 70 pg / mL Tau protein standard solution was measured 15 times at the same sample point. The test results are shown in Figure 3. Figure 8 As shown in Figure B, the relative standard deviation (RSD) is 4.7%. The results of the two experiments show that the sensor has good reproducibility.

[0051] 8. SERS-Apt sensor detects the stability of Tau protein standard solution.

[0052] 10 μL of 50 pg / mL Tau protein standard solution was tested regularly. The samples to be tested were placed at 4°C and tested after 0, 3, 5, 10, and 15 days. The test results were as follows: Fig. 9 As shown, with the increase of interval time, the SERS signal intensity decreased slightly compared with the first set of data, and the relative deviation RSD of the five sets of data was 4.95%, indicating that the sensor had good stability within 15 days.

[0053] 9. Detection of Tau protein in human serum.

[0054] The SERS-Apt sensor prepared by the present invention was used to detect the content of Tau protein in human serum, and a spike experiment was performed. The detection results are shown in Table 1. The recovery rate was between 80-107%, and the RSD was between 1.4-5.7%, indicating that the sensor has good accuracy and can be used for quantitative detection of Tau protein in actual serum samples.

[0055] Table 1 Summary of the results of the detection and spike test of Tau protein in human serum

[0056] 10. Conclusion.

[0057] The present invention uses Fe 3 O 4 @PEI / Ag Nc was used as the SERS substrate and DNA hybridization indicator MB was used as the Raman signal probe to successfully construct a new SERS-Apt sensor for detecting Tau protein. There is a good linear relationship between the Tau protein concentration (1 pg / mL-70 pg / mL) and the SERS signal intensity of the sensor (R 2 =0.993), the limit of detection (LOD) reached 0.18 pg / mL. It can be successfully applied to the detection of Tau protein in human serum samples. The sensor has the advantages of simple preparation, high sensitivity, strong specificity, and rapid detection, and is expected to be used for early diagnosis and screening of Alzheimer's disease.

Claims

1. A novel SERS-Apt sensor for detecting Tau protein, characterized in that: The sensor was prepared by the following method: (1) Preparation of Fe3O4@PEI / Ag magnetic SERS substrate: ① Preparation of Fe3O4@PEI: 8-12 g of nano-Fe3O4 particles were dispersed in 10-25 mL of ultrapure water, ultrasonicated for 5-15 minutes, and 8-12 mL of 5 mg / mL PEI solution was added. After ultrasonication for 25-35 minutes, magnetic separation was performed and washed with ultrapure water to obtain a Fe3O4@PEI particle suspension; ② Preparation of Au seeds: Take 1 mL of 1% HAuCl4 solution and add it to 99 mL of water. After magnetic stirring for 10-20 min, add 1 mL of 1% Na3Cit solution and continue stirring for 1-5 min. Then, add dropwise 1 mL of a mixed solution of 0.075% NaBH4 and 1 mL of 1% Na3Cit and magnetic stirring for 25-35 min to obtain Au seeds. ③ Preparation of Fe3O4@PEI-Au seeds: Add the negatively charged colloidal gold Au seeds prepared in step ② to the positively charged Fe3O4@PEI particle suspension prepared in step ①, ultrasonicate for 25 to 35 minutes, and wash with ultrapure water by magnetic separation to obtain Fe3O4@PEI-Au seed particles, which are dispersed in 50 mL ultrapure water for later use; ④ Preparation of Fe3O4@PEI / Ag Nc: Take 10 mL of Fe3O4@PEI-Au seeds prepared in step ③ and add them to 100 mL of ultrapure water for 5-15 min, add 100 mg of PVP and 1.5 mg of AgNO3, and ultrasonicate for 2-5 min. Quickly add 150 μL of formaldehyde and 150 μL of ammonia water and ultrasonicate for 3-8 min. After magnetic separation, wash with ultrapure water and dissolve in 50 mL of PBS buffer to obtain Fe3O4@PEI / Ag Nc suspension. (2) Preparation of SERS-Apt sensor: In 50 μL of Fe3O4@PEI / Ag Nc suspension, add 5 μL of 50 μM SH-Apt solution and 5 μL of 50 μM cDNA solution, mix well, incubate at room temperature overnight for 12-15 h, and wash with PBS buffer after magnetic separation; Add 20 μL 1×10 -5 mol / L MB solution was incubated at room temperature for 5-7 h, washed with PBS buffer after magnetic separation, and dispersed in 50 μL PBS buffer to obtain Tau protein SERS-Apt sensor.

2. A novel SERS-Apt sensor for detecting Tau protein according to claim 1, characterized in that: The nucleotide sequence of SH-Apt is: 3'-SH-GCG GAG CGA GGC AGG; the nucleotide sequence of cDNA is: CGC CTC GCACCG TCC.

3. A novel SERS-Apt sensor for detecting Tau protein according to claim 2, characterized in that: Nano-Fe3O4 particles were synthesized by the following method: ① Weigh 2.7g FeCl3·6H2O and dissolve it in 80mL ethylene glycol. Stir vigorously for 30 minutes to completely dissolve it. ② Weigh 5.4g sodium acetate and 2g PEG6000 and add them to the above solution, continue stirring for 1 hour and mix well; ③ Transfer to a high-pressure reactor and place it in a 210℃ forced air oven for reaction for 10 hours, then turn off the oven and wait for the product to cool to room temperature. The obtained black precipitate is washed with ultrapure water and ethanol respectively, and placed in a vacuum drying oven at 60℃ for drying. The obtained product is nano-Fe3O4 particles.

4. A method for using the novel SERS-Apt sensor for detecting Tau protein prepared according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Drawing a working curve: 10 μL of Tau protein standard solution of different concentrations was added to multiple SERS-Apt sensors respectively. After incubation at room temperature for 45 min, the sensors were fully washed with PBS buffer and dried naturally. The Raman spectra were collected and the Tau protein working curve was drawn. (2) Add 10 μL of the Tau protein sample to be tested onto the SERS-Apt sensor, incubate for 45 min, wash thoroughly with PBS buffer, dry naturally, and collect its Raman spectrum; The Tau protein concentration was calculated using the Tau protein working curve.

5. The method for using the novel SERS-Apt sensor for detecting Tau protein according to claim 4, characterized in that: The working curve in step (1) is: y=-95.5x+10523.7, R 2 =0.993, y represents 1624cm -1 The SERS signal intensity is shown in Figure 2, and x represents the Tau protein concentration.

Citation Information

Cited By

  • Label-free magnetic self-assembly nano-probe, construction method thereof and application of label-free magnetic self-assembly nano-probe in detection of PrPC protein

    CN119438346A