Prediction method for stable period of performance of hot mix plant recycled mixture

By determining the key parameters and testing methods in the recycled mixture and calculating the performance stability period, the problem of incomplete integration of new and old asphalt is solved, the accuracy of the mixture performance evaluation and construction quality are improved, and the risk of early disease is reduced.

CN118777580APending Publication Date: 2024-10-15TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410801604.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the design process of recycled asphalt mixture, the old and new asphalt cannot be completely integrated, causing the performance of the mixture to change with storage time and unable to accurately reflect the performance during actual service, affecting the scientific design and construction quality.

Method used

By determining the proportion of RAP material in the recycled mixture, the LMS value of asphalt and the curing temperature, using tetrahydrofuran solution immersion and gel permeation chromatography testing methods, the performance stability period is calculated, and the performance stability period of the recycled mixture is predicted using the formula.

Benefits of technology

It improves the accuracy of performance evaluation of recycled mixtures, reduces the possibility of early disease, guides construction and traffic organization, and reduces the variability of performance test results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118777580A_ABST
    Figure CN118777580A_ABST
Patent Text Reader

Abstract

The invention provides a method for predicting the performance stable period of a hot mix plant recycled mixture, and relates to the technical field of road engineering. The prediction method comprises the steps of determining the proportion of the RAP material in the recycled mixture, determining the LMS value of asphalt in the RAP material, determining the curing temperature of the recycled mixture, determining the performance stable period of the recycled mixture and the like, and specific calculation. The method provided by the invention can predict the performance stable period of the regenerated mixture, reduce the variability of the performance test result of the regenerated mixture, improve the accuracy of performance evaluation of the regenerated mixture, effectively guide the construction of the regenerated mixture pavement and open the traffic organization, and reduce the possibility of early diseases of the regenerated mixture pavement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road engineering, and in particular to a method for predicting the stable period of performance of factory-mixed hot recycled mixture. Background Art

[0002] During the hot regeneration process of recycled asphalt (RAP), the old asphalt in RAP can restore its performance to a certain extent under the action of new asphalt or regeneration agent, and play a bonding role with the new asphalt. In the design process of hot recycled asphalt mixture, the new and old asphalt are usually assumed to be completely fused. However, in reality, the new and old asphalt cannot reach a 100% fusion state, and even with the combined effects of high-temperature preheating and mechanical stirring during the mixing process, the new and old asphalt still cannot reach their ideal fusion state during mixing and molding and a short placement time.

[0003] The above phenomenon will cause the effective asphalt content and the properties of the effective asphalt to change with the placement time, resulting in differences in the evaluation results of the mixture performance at different placement times, which cannot accurately reflect the performance of the hot recycled asphalt mixture during service.

[0004] Therefore, how to accurately judge the time when the performance of recycled mixture reaches stability under different placement times is of great importance to improving the accuracy of recycled mixture performance evaluation, enhancing the scientific nature of recycled mixture design, effectively guiding the construction of recycled mixture pavements and open traffic organization, and reducing the possibility of early diseases on recycled mixture pavements. Summary of the invention

[0005] To solve the above problems, the present invention provides a method for predicting the stable period of performance of factory-mixed hot recycled mixture, which can accurately predict the stable period of performance of recycled mixture to improve the accuracy of performance evaluation of recycled mixture.

[0006] The method for predicting the stable period of performance of the factory-mixed hot recycled mixture of the present invention comprises the following steps:

[0007] S11, determining the proportion of RAP material in the recycled mixture;

[0008] S12, determining the LMS value of the asphalt in the RAP material;

[0009] S13, determining the curing temperature of the recycled mixture;

[0010] S14. Determine the stable period of performance of recycled mixture;

[0011] The calculation method of the stable period of the performance of the recycled mixture is shown in formula (1):

[0012]

[0013] Furthermore, the method for determining the LMS value of asphalt in the regenerated asphalt is as follows:

[0014] S21, taking the RAP material used in the regenerated mixture, and soaking it in a tetrahydrofuran solution;

[0015] S22, after the soaking is completed, 1 mL of the solution is extracted and filtered, and 0.5 μm of the filtered solution is injected into a gel permeation chromatography test instrument;

[0016] S23. After 40 min, the chromatogram of asphalt in RAP was collected. Based on the collected chromatogram, the LMS of asphalt was quantified according to formula (2).

[0017]

[0018] Furthermore, the material-liquid ratio of the RAP material and the tetrahydrofuran solution is 1 g:30 mL.

[0019] Furthermore, the soaking time is ≥ 2 days.

[0020] Further, the curing temperature of the recycled mixed material is 20°C-60°C. Preferably, the curing temperature of the recycled mixed material is 25°C-40°C.

[0021] Compared with the prior art, the beneficial technical effects of the present invention are:

[0022] The method of the present invention can predict the performance stability period of recycled mixture, reduce the variability of recycled mixture performance test results, and improve the accuracy of recycled mixture performance evaluation;

[0023] The method of the present invention can effectively guide the construction of recycled mixture pavement and the organization of open traffic, and reduce the possibility of early disease occurrence on the recycled mixture pavement. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention will be further described below in conjunction with the accompanying drawings.

[0025] Figure 1 The design gradation of the factory-mixed hot recycled mixture of Example 2 of the present invention;

[0026] Figure 2 This is the Marshall test result of Example 2 of the present invention;

[0027] Where: (a) is Marshall stability; (b) is void ratio VV; (c) is mineral interstitial ratio VMA; (d) is asphalt saturation VFA; (e) is bulk volume relative density;

[0028] Figure 3The design gradation of the factory-mixed hot recycled mixture of Example 3 of the present invention;

[0029] Figure 4 This is the designed gradation of the factory-mixed hot recycled mixture in Example 4 of the present invention. DETAILED DESCRIPTION

[0030] The technical solution provided by the present invention is further described below in conjunction with embodiments.

[0031] Example 1

[0032] Design 8 groups of recycled mixtures under different working conditions. The gradation of the mixture is AC-20. The gradation curve is as follows: Figure 1 The specific working conditions of the 8 groups of recycled mixtures are shown in Table 1. The recycled mixtures under the above working conditions cover the types of mixtures commonly used in this field. The performance stability period of the 8 groups of recycled mixtures is tested and substituted into formula (3) to fit a, b, c, d, so that the above parameters can be used to predict the stability period of most samples.

[0033]

[0034] Among them, D stab is the stable period, days; RAP perc is the dosage of RAP material, %; T is the placement temperature, ℃; LMS is the macromolecular content based on GPC test; a, b, c, d are different fitting parameters respectively.

[0035] After calculation, a is 143.079, b is 0.058, c is -1.095, and d is 2.177.

[0036] Table 18 Specific working conditions of recycled mixture

[0037] Working condition number LMS / % RAP dosage / % Health temperature / ℃ Performance stability period / day 1 10.7 25 25 4 2 15 25 25 10 3 15.7 25 25 10 4 10.7 30 25 4 5 10.7 40 25 14 6 10.7 40 25 14 7 10.7 40 40 10 8 10.7 40 60 7

[0038] Example 2

[0039] A method for predicting the stable period of performance of factory-mixed hot recycled mixture, the steps are as follows:

[0040] 70# matrix asphalt, limestone and RAP material obtained from actual engineering milling are used to prepare recycled asphalt mixture. The target gradation is AC-20, the RAP material dosage is 25%, and the designed gradation curve is as follows: Figure 1 The relevant indicators of RAP and asphalt used are shown in Table 2-4.

[0041] Table 2 RAP old asphalt content test results

[0042] Binning 0-5mm 5-10mm 10-30mm Test Method RAP material old asphalt content / % 6.73 4.97 3.74 T0735-2011

[0043] Table 3 Test results of basic performance indicators of RAP old asphalt

[0044] Technical indicators Needle penetration / 0.1mm Softening point / ℃ Ductility / mm Test Results 34.8 58.2 5.7

[0045] Table 470# Asphalt Main Technical Indicators

[0046]

[0047] Conventional mix design method:

[0048] According to the provisions of the Technical Specifications for Highway Asphalt Pavement Regeneration, four total asphalt-to-stone ratios of 3.3%, 3.8%, 4.3% and 4.8% were selected. According to the Marshall design method in the Technical Specifications for Highway Asphalt Pavement Construction, the Marshall time was formed and the Marshall stability, void ratio and other indicators were measured and calculated. The test results are as follows: Figure 2 According to the calculation method of the best asphalt-stone ratio given in the specification, the best asphalt-stone ratio under 25% RAP dosage is determined to be 4.10%.

[0049] Prediction method of stable period of recycled mixture performance:

[0050] Determination of specific working conditions and stability period of recycled mixture:

[0051] The recycled mixture was prepared using 25% RAP admixture, three curing temperatures and two RAP materials with different aging degrees. The specific working conditions are shown in Table 5:

[0052] Table 5 Working conditions of different recycled mixtures

[0053] Working condition number LMS / % RAP dosage / % Health temperature / ℃ 1 10.7 25 25 2 15 25 25 3 15.7 25 25

[0054] The high temperature performance, low temperature performance and water stability performance of the mixtures under different working conditions were tested at different placement times. The performance stabilization period was determined based on the test results. It was found that the performance stabilization period of the recycled mixtures under working conditions 1, 2 and 3 was 4 days, 10 days and 10 days respectively.

[0055] Forecast value of stable period:

[0056] According to formula (2), the stable period of recycled mixture performance under different working conditions is predicted and compared with the actual measurement. The results are shown in Table 6.

[0057] Table 6 Deviation between predicted values ​​and measured values

[0058] Working condition number Actual value (day) Prediction value (days) error(%) 1 4 3.5 12.5 2 10 9.6 4.0 3 10 10.4 4.0

[0059] It is not difficult to see from Table 5 that for the recycled mixture with 25% RAP dosage, the method of the present invention can more accurately predict the performance stability of the recycled mixture, and the prediction error can be controlled within 15% (in engineering, if the error between the predicted value and the actual detection value of the recycled mixture exceeds 20%, it is generally regarded as a prediction failure).

[0060] Example 3

[0061] A method for predicting the stable period of performance of factory-mixed hot recycled mixture, the steps are as follows:

[0062] The recycled asphalt mixture was prepared by using 70# matrix asphalt, limestone and RAP material obtained by milling in an actual project. The target gradation was AC-20, the RAP material content was 30%, and the design gradation curve was 3 Figure 3 The relevant indicators of RAP and asphalt used are the same as those in Example 2. According to the Marshall design method in the Technical Specifications for Highway Asphalt Pavement Construction, the asphalt-to-stone ratio in the recycled mixture is determined to be 4.1% when the RAP dosage is 30%.

[0063] Prediction method of stable period of recycled mixture performance:

[0064] Determination of specific working conditions and stability period of recycled mixture:

[0065] The recycled mixture was prepared using 30% RAP admixture, three curing temperatures and two RAP materials with different aging degrees. The specific working conditions are shown in Table 7 below:

[0066] Table 7 Different recycled mixture conditions

[0067] Working condition number LMS / % RAP dosage / % Health temperature / ℃ 4 10.7 30 25 5 15 40 25 6 15.7 40 25

[0068] The high temperature performance, low temperature performance and water stability performance of the mixtures under different working conditions were tested at different placement times. The performance stabilization period was determined based on the test results. It was found that the performance stabilization period of the recycled mixtures under working conditions 1, 2 and 3 was 4 days, 14 days and 14 days respectively.

[0069] Forecast value of stable period:

[0070] According to formula (2), the stable period of the performance of the recycled mixture under different working conditions is predicted and compared with the actual measurement. The results are shown in Table 8.

[0071] Table 8 Deviation between predicted values ​​and measured values

[0072] Working condition number Actual value (day) Prediction value (days) error(%) 4 4 4.6 15 5 14 12.8 8.6 6 14 13.8 1.4

[0073] It is not difficult to see from Table 7 that for the recycled mixture with a RAP content of 30%, the method of the present invention can more accurately predict the performance stability of the recycled mixture, and the prediction error can be controlled within 15%.

[0074] Example 4

[0075] A method for predicting the stable period of performance of factory-mixed hot recycled mixture, the steps are as follows:

[0076] The recycled asphalt mixture was prepared by using 70# matrix asphalt, limestone and RAP material obtained by milling in an actual project. The target gradation was AC-20, the RAP material content was 40%, and the designed gradation curve was as follows: Figure 4 The relevant indicators of RAP and asphalt used are the same as those in Example 2. According to the Marshall design method in the Technical Specifications for Highway Asphalt Pavement Construction, the asphalt-stone ratio in the recycled mixture is determined to be 4.1% when the RAP content is 40%.

[0077] Prediction method of stable period of recycled mixture performance:

[0078] Determination of specific working conditions and stability period of recycled mixture

[0079] The recycled mixture was prepared using 40% RAP admixture, three curing temperatures and two RAP materials with different aging degrees. The specific working conditions are shown in the following table:

[0080] Table 9 Working conditions of different recycled mixtures

[0081] Working condition number LMS / % RAP dosage / % Health temperature / ℃ 7 10.7 40 25 8 10.7 40 40

[0082] The high temperature performance, low temperature performance and water stability performance of the mixtures under different working conditions were tested at different placement times. The performance stabilization period was determined based on the test results. It was found that the performance stabilization period of the recycled mixtures under working conditions 1 and 2 was 10 days and 7 days, respectively.

[0083] Stable period forecast value

[0084] According to the formula given in step (4), the stable period of the performance of the recycled mixture under different working conditions is predicted and compared with the actual measurement. The results are shown in Table 10.

[0085] Table 10 Deviation between predicted values ​​and measured values

[0086] Working condition number Actual value (day) Prediction value (days) error(%) 7 10 8.3 17.0 8 7 6.8 2.9

[0087] It is not difficult to see from Table 9 that for the recycled mixture with a RAP content of 40%, the method of the present invention can more accurately predict the performance stability of the recycled mixture, and the prediction error can be controlled within 17%.

[0088] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of ​​the present invention. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for predicting the stable period of performance of hot recycled mixture in factories. It is characterized in that The following steps are involved: S11, determining the proportion of RAP material in the recycled mixture; S12, determining the LMS value of the asphalt in the RAP material; S13, determining the curing temperature of the recycled mixture; S14. Determine the stable period of performance of recycled mixture; The calculation method of the stable period of the performance of the recycled mixture is shown in formula (1): Among them, D stab is the stable period, days; RAP perc is the dosage of RAP material, %; T is the storage temperature, ℃; LMS is the macromolecular content based on GPC test.

2. The prediction method according to claim 1, It is characterized in that The method for determining the LMS value of asphalt in the regenerated asphalt is as follows: S21, taking the RAP material used in the regenerated mixture, and soaking it in a tetrahydrofuran solution; S22, after the soaking is completed, 1 mL of the solution is extracted and filtered, and 0.5 μm of the filtered solution is injected into a gel permeation chromatography test instrument; S23, 40 min later, the chromatogram of asphalt in RAP was collected, and the LMS of asphalt was quantified according to formula (2) based on the collected chromatogram; 3. The prediction method according to claim 1, It is characterized in that The material-liquid ratio of the RAP material and the tetrahydrofuran solution is 1 g:30 mL.

4. The prediction method according to claim 1, It is characterized in that The soaking time is ≥ 2 days.

5. The prediction method according to claim 1, It is characterized in that The curing temperature of the recycled mixture is 20°C-60°C.