Secondary battery, preparation method thereof and electric device

By using a combined structure of gel electrolyte and porous insulating base layer in secondary batteries, the problems of low volume energy density and poor impact resistance of secondary batteries are solved, higher mechanical strength and safety are achieved, and the battery is avoided. Risk of damage and explosion in case of stress.

CN118782897APending Publication Date: 2024-10-15CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310369569.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing secondary batteries have low volumetric energy density and poor impact resistance, which can easily lead to battery damage and internal short circuit under stress, posing a risk of explosion.

Method used

Gel electrolyte and porous insulating base layer are used to form a connection structure between the insulating layer and the gel electrolyte layer, which enhances the mechanical strength, reduces the battery volume through flexible packaging, and reduces the risk of internal short circuit caused by lithium dendrite puncture.

Benefits of technology

It improves the volumetric energy density and mechanical strength of secondary batteries, reduces the risk of damage caused by cell expansion effects and external collisions, and avoids explosion problems under abnormal use conditions such as overcharge, overdischarge, and impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782897A_ABST
    Figure CN118782897A_ABST
Patent Text Reader

Abstract

The invention relates to a secondary battery, a preparation method thereof and a power utilization device. The secondary battery comprises a positive pole piece and a negative pole piece, the negative pole piece is arranged opposite to the positive pole piece; the gel electrolyte layer is arranged between the positive pole piece and the negative pole piece; the gel electrolyte layer is arranged between the positive pole piece and the negative pole piece, the insulation layer is arranged between the gel electrolyte layer and the positive pole piece and / or between the gel electrolyte layer and the negative pole piece, the insulation layer comprises a porous insulation base layer and gel electrolyte filled in pores of the porous insulation base layer, the insulation layer and the gel electrolyte layer are bonded, and the gel electrolyte layer is arranged between the gel electrolyte layer and the negative pole piece. And the gel electrolyte is connected with the gel electrolyte layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of secondary batteries, and specifically relates to a secondary battery and a preparation method and an electrical device thereof. Background Art

[0002] Secondary batteries are widely used in various consumer electronic products and electric vehicles due to their outstanding features such as light weight, no pollution, and no memory effect.

[0003] Currently commonly used secondary batteries, including sodium-ion batteries and lithium-ion batteries, have problems such as low volume energy density resulting in low mileage performance, and poor impact and collision resistance that can easily cause battery damage. Summary of the invention

[0004] Based on this, it is necessary to provide a secondary battery and a preparation method and an electrical device thereof that can take into account both volume energy density and reduce the degree of damage to the battery.

[0005] The present application is implemented through the following technical solutions.

[0006] In one aspect of the present application, a secondary battery is provided, comprising:

[0007] Positive electrode;

[0008] A negative electrode sheet, arranged opposite to the positive electrode sheet;

[0009] A gel electrolyte layer is provided between the positive electrode sheet and the negative electrode sheet; and

[0010] An insulating layer is provided between the gel electrolyte layer and the positive electrode plate, and / or between the gel electrolyte layer and the negative electrode plate, wherein the insulating layer comprises a porous insulating base layer and a gel electrolyte filled in pores of the porous insulating base layer, wherein the insulating layer is bonded to the gel electrolyte layer, and the gel electrolyte is connected to the gel electrolyte layer.

[0011] In the conventional battery using liquid electrolyte and separator, the separator is easily oxidized during the use of the battery, which makes its strength easy to reduce, and then it is easy to cause the battery to break and crack when subjected to the internal mechanical force generated by the expansion effect of the battery cell or the external collision stress, or it is pierced by the lithium dendrites generated by lithium precipitation, resulting in internal short circuit, and there is a risk of failure and explosion. Without wishing to be limited to any theory, the above-mentioned secondary battery of the present application adopts gel electrolyte, and there will be no explosion problems during abnormal use such as overcharge, overdischarge, impact, crushing and puncture, so soft packaging can be used to reduce the volume of the secondary battery and greatly improve the volume energy density of the battery; and in the above-mentioned secondary battery of the present application, the gel electrolyte in the insulating layer is connected to the gel electrolyte layer to form a rivet-like structure, so the bonding force between the insulating layer and the gel electrolyte layer is enhanced, so that the overall mechanical strength of the secondary battery can be improved, and the risk of internal short circuit caused by lithium dendrite piercing and battery failure can be reduced, and the problem of damage to the battery caused by the internal mechanical force and external collision stress generated by the expansion effect of the battery cell during use can be further improved. In summary, the secondary battery not only has a good volume energy density, but also can reduce the degree of damage to the battery.

[0012] In any embodiment of the present application, the insulating layer is bonded to the positive electrode sheet and / or the negative electrode sheet; and / or,

[0013] The gel electrolyte layer is bonded to the positive electrode sheet or the negative electrode sheet.

[0014] In any embodiment of the present application, the 180-degree peel strength of the positive electrode sheet, the porous insulating base layer, the gel electrolyte layer and the negative electrode sheet as a whole is 10 N / m to 35 N / m;

[0015] Optionally, the 180-degree peel strength of the positive electrode sheet, the porous insulating base layer, the gel electrolyte layer and the negative electrode sheet as a whole is 12 N / m to 35 N / m.

[0016] In any embodiment of the present application, the gel electrolyte and the gel electrolyte layer form a continuous phase.

[0017] In any embodiment of the present application, the thickness of the insulating layer is ≤18 μm, and may be 3 μm to 18 μm, and may be 7 μm to 18 μm.

[0018] In any embodiment of the present application, the material of the insulating layer includes at least one of an insulating ceramic material and an insulating polymer material.

[0019] In any embodiment of the present application, the material of the insulating layer includes an insulating ceramic material and an insulating organic material; optionally, the mass ratio of the insulating ceramic material to the insulating polymer material is (7-9): (1-3).

[0020] In any embodiment of the present application, the secondary battery satisfies at least one of the following conditions (1-a) to (1-c):

[0021] (1-a) The insulating ceramic material includes at least one of aluminum oxide, silicon dioxide, magnesium oxide, boehmite, aluminum hydroxide, magnesium hydroxide, zirconium dioxide, lithium zirconate, lithium phosphate, lithium aluminate, lithium fluoride, lithium carbonate, lithium oxalate, lithium silicate and silicic acid;

[0022] (1-b) The Dv50 particle size of the insulating ceramic material is 0.5 μm to 7 μm, and can be optionally 1 μm to 5 μm;

[0023] (1-c) The insulating polymer material includes at least one of polyvinylidene fluoride, polyethylene, polymethacrylate, polyacrylonitrile and styrene-butadiene rubber.

[0024] In any embodiment of the present application, the secondary battery satisfies at least one of the following conditions (2-a) to (2-b):

[0025] (2-a) The average pore size of the porous insulating base layer is 20 nm to 400 nm, and can be 50 nm to 300 nm;

[0026] (2-b) The porosity of the porous insulating base layer is 30% to 70%, and can be optionally 50% to 65%.

[0027] In any embodiment of the present application, the gel electrolyte and the gel electrolyte layer include a polymer and an electrolyte salt;

[0028] Optionally, the monomer of the polymer includes at least one of an ester monomer, an ether monomer, a nitrile monomer, a sulfone monomer and a siloxane monomer;

[0029] Optionally, the electrolyte salt includes at least one of an electrolyte lithium salt and an electrolyte sodium salt.

[0030] In any embodiment of the present application, the secondary battery satisfies at least one of the following conditions (3-a) to (3-c):

[0031] (3-a) The thickness of the gel electrolyte layer is 0.2 μm to 2 μm;

[0032] (3-b) The positive electrode sheet includes a positive electrode active layer, and the thickness of the positive electrode active layer is 100 μm to 250 μm;

[0033] (3-c) The negative electrode sheet includes a negative electrode active layer, and the thickness of the negative electrode active layer is 80 μm to 200 μm.

[0034] The second aspect of the present application provides a method for preparing the secondary battery provided in the first aspect of the present application, comprising the following steps:

[0035] A porous insulating base layer is provided between the positive electrode sheet and the negative electrode sheet;

[0036] Assembling the positive electrode sheet, the porous insulating base layer and the negative electrode sheet into a battery cell;

[0037] A gel electrolyte solution is injected into the battery cell, and the gel electrolyte solution is solidified to form a gel electrolyte layer and a gel electrolyte between the positive electrode sheet and the negative electrode sheet and in the pores of the porous insulating base layer, respectively.

[0038] In any embodiment of the present application, the step of providing a porous insulating base layer between the positive electrode sheet and the negative electrode sheet comprises:

[0039] A porous insulating base layer is formed on the surface of the positive electrode sheet and / or the negative electrode sheet.

[0040] In any embodiment of the present application, the secondary battery satisfies at least one of the following conditions (3-a) to (3-c):

[0041] (3-a) The thickness of the gel electrolyte layer is 0.2 μm to 2 μm;

[0042] (3-b) The positive electrode sheet includes a positive electrode active layer, and the thickness of the positive electrode active layer is 100 μm to 250 μm;

[0043] (3-c) The negative electrode sheet includes a negative electrode active layer, and the thickness of the negative electrode active layer is 80 μm to 200 μm.

[0044] In a third aspect of the present application, a method for preparing the secondary battery provided in the second aspect of the present application is provided, comprising the following steps:

[0045] A porous insulating base layer is provided between the positive electrode sheet and the negative electrode sheet;

[0046] Assembling the positive electrode sheet, the porous insulating base layer and the negative electrode sheet into a battery cell;

[0047] A gel electrolyte solution is injected into the battery cell, and the gel electrolyte solution is solidified to form a gel electrolyte layer and a gel electrolyte between the positive electrode sheet and the negative electrode sheet and in the pores of the porous insulating base layer, respectively.

[0048] In any embodiment of the present application, the step of providing a porous insulating base layer between the positive electrode sheet and the negative electrode sheet comprises:

[0049] A porous insulating base layer is formed on the surface of the positive electrode sheet and / or the negative electrode sheet.

[0050] In any embodiment of the present application, the preparation method satisfies at least one of the following conditions (4-a) to (4-c):

[0051] (4-a) The gel electrolyte solution comprises a polymerizable monomer, an initiator, an electrolyte salt and a solvent;

[0052] (4-b) The curing temperature is 50 to 100° C., and can be 60 to 90° C.;

[0053] (4-c) The curing time is 5 hours to 20 hours, and can be optionally 10 hours to 20 hours.

[0054] In a fourth aspect of the present application, an electrical device is provided, comprising the secondary battery provided in the second aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0056] Figure 1 is a schematic diagram of a secondary battery according to an embodiment of the present application;

[0057] Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of the present application is shown;

[0058] Figure 3 FIG. 1 is a schematic diagram of an electric device using a secondary battery according to an embodiment of the present application as a power source.

[0059] Description of reference numerals:

[0060] 1. Secondary battery; 11. Casing; 12. Electrode assembly; 13. Cover plate; 2. Electrical device. DETAILED DESCRIPTION

[0061] The present application is further described below in conjunction with specific implementations. It should be understood that these specific implementations are only used to illustrate the present application and are not used to limit the scope of the present application.

[0062] For simplicity, only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value itself can be combined with any other point or single value as a lower limit or upper limit or with other lower limits or upper limits to form an unspecified range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In this application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0063] In the description of this article, it should be noted that, unless otherwise specified, "above" and "below" are inclusive of the number itself, and "several" in "one or several" means two or more.

[0064] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0065] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0066] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0067] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0068] In the description of this article, it should be noted that, unless otherwise specified, "above" and "below" are inclusive of the number itself, and "several" in "one or several" means two or more.

[0069] In the description herein, unless otherwise stated, the term "or" is inclusive. That is, the phrase "A or (or) B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist). Unless otherwise stated, the terms used in this application have the well-known meanings commonly understood by those skilled in the art. Unless otherwise stated, the numerical values ​​of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the embodiments of this application).

[0070] Secondary battery

[0071] A secondary battery is a battery that can be recharged to activate the active materials after being discharged and continue to be used.

[0072] Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, and an electrolyte. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. Furthermore, the secondary battery also includes a separator, which is arranged between the positive electrode sheet and the negative electrode sheet to play a role of isolation. The electrolyte plays a role of conducting ions between the positive electrode sheet and the negative electrode sheet.

[0073] The present application provides a secondary battery, which includes: a positive electrode plate, a negative electrode plate, a gel electrolyte layer and an insulating layer.

[0074] The positive electrode sheet and the negative electrode sheet are arranged opposite to each other. The gel electrolyte layer is arranged between the positive electrode sheet and the negative electrode sheet. The insulating layer is arranged between the gel electrolyte layer and the positive electrode sheet, and / or, the insulating layer is arranged between the gel electrolyte layer and the negative electrode sheet. The insulating layer includes a porous insulating base layer and a gel electrolyte filled in the pores of the porous insulating base layer. The insulating layer is bonded to the gel electrolyte layer, and the gel electrolyte is connected to the gel electrolyte layer.

[0075] It can be understood that the gel electrolyte layer refers to an electrolyte in a gel state, also known as a semi-solid electrolyte. The gel electrolyte layer includes a gel polymer and an electrolyte salt, which has a network structure formed by the gel polymer and has the function of conducting ions of the electrolyte salt. The porous insulating base layer of the insulating layer has the property of electron non-conductivity, so it can also play the role of isolating the positive electrode and the negative electrode, and the gel electrolyte filled in the pores of the porous insulating base layer can play the role of conducting ions.

[0076] In the conventional battery using liquid electrolyte and separator, the separator is easily oxidized during the use of the battery, which makes its strength easy to reduce, and then it is easy to cause the battery to break and crack when subjected to the internal mechanical force generated by the expansion effect of the battery cell or the external collision stress, or it is pierced by the lithium dendrites generated by lithium precipitation, resulting in internal short circuit, and there is a risk of failure and explosion. Without wishing to be limited to any theory, the above-mentioned secondary battery of the present application adopts gel electrolyte, and there will be no explosion problems during abnormal use such as overcharge, overdischarge, impact, crushing and puncture, so soft packaging can be used to reduce the volume of the secondary battery and greatly improve the volume energy density of the battery; and in the above-mentioned secondary battery of the present application, the gel electrolyte in the insulating layer is connected to the gel electrolyte layer to form a rivet-like structure, so the bonding force between the insulating layer and the gel electrolyte layer is enhanced, so that the overall mechanical strength of the secondary battery can be improved, and the risk of internal short circuit caused by lithium dendrite piercing and battery failure can be reduced, and the problem of damage to the battery caused by the internal mechanical force and external collision stress generated by the expansion effect of the battery cell during use can be further improved. In summary, the secondary battery not only has a good volume energy density, but also can reduce the degree of damage to the battery.

[0077] In some of the embodiments, the 180-degree peel strength of the positive electrode sheet, the porous insulating substrate, the gel electrolyte layer and the negative electrode sheet of the secondary battery as a whole is 10 N / m to 35 N / m.

[0078] In some of the embodiments, the insulating layer is bonded to the positive electrode sheet and / or the negative electrode sheet. The insulating layer of the present application can be pre-formed on the surface of the positive electrode sheet and / or the negative electrode sheet by coating or the like, so that the insulating layer is bonded to the positive electrode sheet and / or the negative electrode sheet. The 180-degree peel strength of the positive electrode sheet, the porous insulating base layer, the gel electrolyte layer and the negative electrode sheet of the secondary battery as a whole is 12N / m to 35N / m. The direct bonding force between the insulating layer and the positive electrode sheet or the negative electrode sheet of the present application is strong, so it can provide stress buffering for the positive electrode sheet or the negative electrode sheet, and further improve the mechanical strength of the secondary battery as a whole compared to the battery in which a separate separator is directly provided between the positive electrode sheet and the negative electrode sheet, thereby further improving the risk of internal short circuit and battery failure caused by lithium dendrite piercing of the secondary battery, and the problem of damage to the battery caused by internal mechanical force and external collision stress generated by the expansion effect of the battery cell during use.

[0079] In some embodiments, the gel electrolyte and the gel electrolyte layer are not only connected, but also form a continuous phase therebetween. Specifically, the gel electrolyte and the gel electrolyte layer are an integrated structure formed by one-step curing, so the bonding force between the two is strong.

[0080] In some embodiments, the gel electrolyte layer is bonded to the positive electrode sheet or the negative electrode sheet. It is understood that the gel electrolyte layer can be formed by in-situ curing and then bonded to the positive electrode sheet or the negative electrode sheet. In a specific example, the gel electrolyte layer is directly bonded to the positive active layer on the positive electrode sheet or to the negative active layer on the negative electrode sheet.

[0081] In some embodiments, the thickness of the insulating layer is ≤18μm, and may be 3μm to 18μm, or may be 3μm to 15μm, 7μm to 18μm, or 4μm to 10μm. As an example, the thickness of the insulating layer may be 3nm, 4nm, 5nm, 7nm, 9nm, 10nm, 13nm, 15nm, or 18nm. The insulating layer of the present application may be pre-formed on the surface of the positive electrode sheet and / or the negative electrode sheet by coating or the like, so that a thinner insulating layer may be prepared to further reduce the volume of the secondary battery and increase the volume energy density of the battery.

[0082] In some of the embodiments, the material of the insulating layer includes at least one of an insulating ceramic material and an insulating polymer material.

[0083] Furthermore, the material of the insulating layer includes insulating ceramic material and insulating polymer material. It is understandable that the insulating polymer material can also play the role of bonding the insulating ceramic material. The presence of the insulating ceramic material is not only more conducive to forming multiple pores, but also can improve the mechanical strength and high temperature resistance of the insulating layer, thereby helping to reduce the risk of lithium dendrites piercing and causing internal short circuits and causing battery failure.

[0084] Optionally, the mass ratio of the insulating ceramic material to the insulating polymer material is (7-9):(1-3). As an example, the mass ratio of the insulating ceramic material to the insulating polymer material is 7:3, 8:2, 9:1. Optionally, the mass ratio of the insulating ceramic material to the insulating polymer material is (7-8):(2-3).

[0085] Optionally, the insulating ceramic material includes but is not limited to at least one of aluminum oxide, silicon dioxide, magnesium oxide, boehmite, aluminum hydroxide, magnesium hydroxide, zirconium dioxide, lithium zirconate, lithium phosphate, lithium aluminate, lithium fluoride, lithium carbonate, lithium oxalate, lithium silicate and silicic acid.

[0086] Further, the Dv50 particle size of the insulating ceramic material is 0.5 μm to 7 μm, and can be 1 μm to 5 μm. As an example, the Dv50 particle size of the insulating ceramic material can be 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm. As an example, the insulating ceramic material is granular.

[0087] Optionally, the insulating polymer material includes but is not limited to at least one of polyvinylidene fluoride, polyethylene, polymethacrylate, polyacrylonitrile and styrene-butadiene rubber.

[0088] In some of the embodiments, the average pore size of the porous insulating base layer in the insulating layer is 20 nm to 400 nm, and can be 50 nm to 300 nm.

[0089] In some of the embodiments, the porosity of the porous insulating base layer is 30% to 70%, and optionally 50% to 65%.

[0090] It is understood that the insulating layer can be a single-layer film or a multi-layer composite film without any particular limitation. When the insulating layer is a multi-layer composite film, the materials of each layer can be the same or different without any particular limitation.

[0091] It is understood that the gel electrolyte and the gel electrolyte layer include a polymer and an electrolyte salt.

[0092] Optionally, the monomers of the polymer in the gel electrolyte and the gel electrolyte layer include at least one of ester monomers, ether monomers, nitrile monomers, sulfone monomers and siloxane monomers. It is understood that the monomers of the polymer in the gel electrolyte and the gel electrolyte layer can be the same or different.

[0093] Furthermore, the ester monomers include, but are not limited to, at least one of vinylene carbonate, vinyl ethylene carbonate, dimethyl allyl malonate, diethyl allyl malonate, vinyl acetate, polyethylene glycol methacrylate, polyethylene glycol methyl ether methacrylate, dimethyl allyl dicarboxylate, diethyl allyl malonate, methallyl carbonate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, and trimethylene carbonate.

[0094] Furthermore, the ether monomer includes but is not limited to at least one of ethylene oxide or 1,3-dioxolane and dioxane.

[0095] Furthermore, the nitrile monomer includes but is not limited to at least one of 2-cyano-2-butyl acrylate, 2-cyano-3,3-diphenylacrylate, and 1-cyclohexeneacetonitrile.

[0096] Furthermore, the sulfone-based monomer includes but is not limited to at least one of methyl vinyl sulfone and ethyl vinyl sulfone.

[0097] Furthermore, the siloxane-based monomer includes but is not limited to at least one of trivinylcyclotrisiloxane and vinylmethoxysilane.

[0098] Optionally, the electrolyte salt in the gel electrolyte and the gel electrolyte layer includes at least one of an electrolyte lithium salt and an electrolyte sodium salt. It is understood that the electrolyte salt in the gel electrolyte and the gel electrolyte layer may be the same or different.

[0099] Further, the electrolyte salt in the gel electrolyte and the gel electrolyte layer includes at least one of a sodium salt, a lithium salt and a potassium salt.

[0100] As an example, the sodium salt in the electrolyte salt can be selected from one or more of sodium perchlorate (NaClO4), sodium tetrafluoroborate (NaBF4), sodium hexafluorophosphate (NaPF6), sodium hexafluoroarsenate (NaAsF6), sodium trifluoroacetate (CF3COONa), sodium tetraphenylborate (NaB(C6H5)4), sodium trifluoromethylsulfonate (NaSO3CF3), sodium bis(fluorosulfonyl)imide (Na[(FSO2)2N]) or sodium bis(trifluoromethylsulfonyl)imide (Na[(CF3SO2)2N]).

[0101] As an example, the lithium salt in the electrolyte salt can be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0102] In some embodiments, the gel electrolyte and the gel electrolyte layer may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, and additives that improve battery low temperature performance.

[0103] In some embodiments, the thickness of the gel electrolyte layer is 0.2 μm to 2 μm. As an example, the thickness of the gel electrolyte layer can be 0.2 μm, 0.5 μm, 1 μm, 1.5 μm, or 2 μm.

[0104] In some embodiments, the positive electrode sheet includes a positive electrode active layer, and the thickness of the positive electrode active layer is 100 μm to 250 μm. As an example, the thickness of the positive electrode active layer can be 100 μm, 150 μm, 200 μm, or 250 μm.

[0105] It is understood that the positive electrode plate also includes a positive electrode current collector, and the positive electrode active layer is formed on the positive electrode current collector. The positive electrode current collector can be a conventional metal foil or a composite current collector, wherein the composite current collector can be formed by arranging a metal material on a polymer substrate. As an example, the positive electrode current collector can be aluminum foil.

[0106] It is understood that the positive electrode active layer contains positive electrode active materials. The specific type of positive electrode active materials is not limited, and active materials known in the art that can be used for secondary battery positive electrodes can be used, and those skilled in the art can select according to actual needs.

[0107] As an example, the positive electrode active material may include a lithium ion active material, and the lithium ion active material includes, but is not limited to, one or more of lithium transition metal oxides, lithium-containing phosphates with an olivine structure, and their respective modified compounds. Examples of the lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Examples of the lithium-containing phosphates with an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, a composite material of lithium manganese iron phosphate and carbon, and their modified compounds. These materials can all be obtained through commercial channels.

[0108] As an example, the positive electrode active material may include a sodium ion active material, and the sodium ion active material may adopt the positive electrode active material for sodium ion batteries known in the art. As an example, the sodium ion active material may include at least one of the following materials: Prussian blue (PBA) type, with the chemical formula (NaxMA[MB(CN)6]·zH2O, where MA and MB are transition metal ions, which is a compound composed of sodium, transition metal, and cyanide, such as Na4Fe2(CN)6, Na4Fe(CN)6, Na1.72MnFe2(CN)6, NaMnMn(CN)6, NaNiFe(CN)6, etc.; oxide type, with the chemical formula NaxMO2, 0 < x ≤ 1, where M is a transition metal element, which is composed of transition metal oxides, and the variable-valence transition metals involved mainly include vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), and copper (Cu), among which manganese and iron with relatively rich resources are most commonly used, such as NaCrO2, NaMnO2, NaMnO2, Na 0.61 Ti 0.48 Mn 0.52 O2, Na[Fe 0.5 Co 0.5 O2, NaMnO2, Na[Ni 0.25 Fe 0.5 Mn 0.25 O2, etc.; and polyanion compound type, with the chemical formula Na x M y [(XO m ) n- z ​, M is a metal ion with a variable valence state, X is an element such as P, S and V, which is composed of sodium, transition metals and anions, among which the transition metals mainly include iron, vanadium, cobalt, etc., and the anions mainly include phosphate, pyrophosphate, fluorophosphate and sulfate, such as NaMnFe2(PO4)6, Na2MnP2O7, Na3V2(PO4)3, Na2Fe2(SO4)3, NaFePO4, Na3V2(PO4)2F3, Na4Co3(PO4)2(P2O7).

[0109] In some embodiments, the modified compounds of the above materials may be doping-modified and / or surface-coated modified materials.

[0110] The positive electrode active layer may also optionally include a binder, a conductive agent and other optional auxiliary agents.

[0111] As an example, the conductive agent may be one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, Super P (SP), graphene, and carbon nanofibers.

[0112] As an example, the binder can be one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).

[0113] In some embodiments, the negative electrode sheet includes a negative electrode active layer, and the thickness of the negative electrode active layer is 80 μm to 200 μm. As an example, the thickness of the negative electrode active layer can be 80 μm, 100 μm, 120 μm, 150 μm, 180 μm, or 200 μm.

[0114] It is understood that the negative electrode plate also includes a negative electrode current collector, and the negative electrode active layer is formed on the negative electrode current collector. The negative electrode current collector can be a conventional metal foil or a composite current collector. Among them, the composite current collector can be formed by arranging a metal material on a polymer substrate. As an example, the negative electrode current collector can be copper foil, aluminum foil, etc.

[0115] It is understood that the negative electrode active layer contains negative electrode active materials. The specific type of negative electrode active materials is not limited, and active materials known in the art that can be used for negative electrodes of secondary batteries can be used, and those skilled in the art can select according to actual needs.

[0116] As an example, the negative electrode active material may include, but is not limited to, one or more of artificial graphite, natural graphite, hard carbon, soft carbon, silicon-based materials and tin-based materials. The silicon-based material may be selected from one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from one or more of elemental tin, tin oxide compounds, and tin alloys. These materials can all be obtained through commercial channels. Among them, the silicon oxide compound may be silicon monoxide.

[0117] In some embodiments, in order to further improve the energy density of the battery, the negative electrode active material includes a silicon-based material.

[0118] The negative electrode active layer may also optionally include a binder, a conductive agent and other optional auxiliary agents.

[0119] As an example, the conductive agent may be one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0120] As an example, the binder can be one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).

[0121] As an example, other optional auxiliary agents may be thickeners and dispersants (such as sodium carboxymethyl cellulose CMC-Na), PTC thermistor materials, etc.

[0122] An embodiment of the present application further provides a method for preparing the secondary battery, comprising the following steps S10 to S30.

[0123] Step S10: Dispose a porous insulating base layer between the positive electrode sheet and the negative electrode sheet.

[0124] In some of the embodiments, a porous insulating base layer is formed on the surface of the positive electrode sheet and / or the negative electrode sheet, so that the insulating layer is bonded to the positive electrode sheet and / or the negative electrode sheet with strong bonding force.

[0125] In some of the embodiments, a porous insulating base layer is formed in advance on the surface of the positive electrode sheet and / or the negative electrode sheet by coating or the like.

[0126] Step S20: assemble the positive electrode sheet, the porous insulating base layer and the negative electrode sheet into a battery cell.

[0127] Step S30: injecting a gel electrolyte solution into the battery cell and solidifying the gel electrolyte solution to form a gel electrolyte layer and a gel electrolyte between the positive electrode sheet and the negative electrode sheet and in the pores of the porous insulating base layer, respectively.

[0128] After the gel electrolyte solution is injected, it is embedded in the pores of the porous insulating base layer and filled between the positive electrode plate and the negative electrode plate, and then solidifies and polymerizes in situ to form an electrolyte network, thereby improving the interlayer adhesion between the positive electrode plate, the porous insulating base layer, the gel electrolyte layer and the negative electrode plate, thereby greatly improving the overall mechanical strength of the secondary battery.

[0129] In some embodiments, the gel electrolyte solution includes a polymer monomer, an initiator, an electrolyte salt and a solvent. Further, in terms of mass percentage, the gel electrolyte solution includes 1 wt% to 20 wt% of the polymer monomer, 0.2 wt% to 5 wt% of the initiator, 15 wt% to 35 wt% of the electrolyte salt and 50 wt% to 70 wt% of the solvent.

[0130] The selection of the types of polymer monomers and electrolyte salts is described above and will not be described in detail here.

[0131] Furthermore, the initiator includes but is not limited to at least one of 2,2-azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate and benzoyl peroxide.

[0132] In some embodiments, the solvent includes at least one of an ether solvent, an ester solvent and a sulfone solvent.

[0133] As an example, the ether solvent may include at least one of ethylene glycol dimethyl ether (DME), diethylene glycol dimethyl ether (DEGDME), triethylene glycol dimethyl ether (TRGDME), tetraethylene glycol dimethyl ether (TEGDME), and 1,3-dioxolane (DOL).

[0134] As an example, the ester solvent may include at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), γ-butyrolactone (BL), 1,3-propane sultone (1,3-PS), methyl propionate (MP), methyl butyrate (MB), ethyl acetate (EA), ethyl propionate (EP), propyl propionate (PP) and ethyl butyrate (EB).

[0135] As an example, the sulfone-based solvent includes dimethyl sulfoxide (DMSO).

[0136] It is understood that curing can be achieved by applying a temperature to reach the temperature required for curing the polymerized monomer. In some embodiments, the curing temperature is 50-100°C, optionally 60-90°C, 70-90°C; further, the curing time can be 5h-20h, optionally 8h-20h, 10h-20h. As an example, the curing temperature is 80°C and the time is 12h.

[0137] The embodiment of the present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 1 is a square structure as an example.

[0138] In some embodiments, reference Figure 2 , the outer packaging may include a shell 11 and a cover plate 13. Among them, the shell 11 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 11 has an opening connected to the receiving cavity, and the cover plate 13 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 12 through a winding process or a lamination process. The electrode assembly 12 is encapsulated in the receiving cavity. The above-mentioned gel electrolyte is impregnated in the electrode assembly 12. The number of electrode assemblies 12 contained in the secondary battery 1 can be one or more, and those skilled in the art can select according to specific actual needs.

[0139] In addition, the present invention further provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided by the present invention. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. Among them, the mobile device may be, for example, a mobile phone, a laptop computer, etc.; the electric vehicle may be, for example, a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., but are not limited thereto.

[0140] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.

[0141] Figure 3 The power consumption device 2 is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle.

[0142] As another example, the device may be a mobile phone, a tablet computer, a laptop computer, etc.

[0143] In order to make the purpose, technical solutions and advantages of the present invention more concise and clear, the present invention is described with the following specific embodiments, but the present invention is by no means limited to these embodiments. The embodiments described below are only preferred embodiments of the present invention, which can be used to describe the present invention and cannot be understood as limiting the scope of the present invention. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

[0144] In order to better illustrate the present invention, the present invention is further described below in conjunction with the embodiments. The following are specific embodiments.

[0145] Example 1

[0146] 1) Preparation of positive electrode: Active material LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM111), conductive carbon black (SP), and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 96.8:2.2:1, dissolved in N-methylpyrrolidone (NMP), and the positive electrode active slurry is prepared after slurrying, coated on aluminum foil, dried, cold pressed, and cut to obtain positive electrode sheets; the thickness of the positive electrode active layer is 200μm.

[0147] 2) Prepare negative electrode sheets: Graphite, binder styrene butadiene rubber (SBR), dispersant (CMC-Na), conductive carbon black (Super-P, SP), and carbon nanotubes (CNT) are mixed in a proper amount of deionized water at a weight ratio of 96%: 2%: 1%: 0.7%: 0.3% to prepare negative electrode slurry. Then, the negative electrode active slurry is coated on a 6μm thick copper foil, dried and cold pressed to form a negative electrode active material layer, and cut into negative electrode sheets; the thickness of the negative electrode active layer is 150μm.

[0148] 3) Preparation of a porous insulating base layer: Silicon dioxide (insulating ceramic material) with a Dv50 particle size of 0.5 μm and polyacrylonitrile are mixed with a solvent in a mass ratio of 8:2 to prepare a base layer slurry, and the base layer slurry is coated on the surface of the positive active layer of the positive electrode plate, and dried to obtain a porous insulating base layer with a thickness of 7 μm.

[0149] 4) Preparation of gel electrolyte solution: using EC, EMC and DEC in a volume ratio of 1:1:1 as a mixed solvent, adding LiPF6 as a lithium salt, and preparing a 1M LiPF6 electrolyte; then adding vinylene carbonate monomer and azobisisoheptanenitrile as an initiator to obtain a gel electrolyte solution. The content of vinylene carbonate is 15wt%, and the content of the initiator is 0.5wt%.

[0150] 5) The negative electrode sheet and the positive electrode sheet with an insulating layer on the surface are assembled into a battery cell, and the above-mentioned gel electrolyte solution is injected and solidified at 80° C. to obtain a secondary battery with a gel electrolyte layer thickness of 1 μm.

[0151] Embodiments 2 to 17

[0152] The same as Example 1, the different parameters are shown in Table 1.

[0153] Embodiment 18

[0154] It is basically the same as Example 1, except that the positive electrode plate is not provided with the above-mentioned porous insulating base layer, and the above-mentioned porous insulating base layer is formed only on the negative electrode plate; the preparation process of the porous insulating base layer is the same, and the composition and thickness of the prepared porous insulating base layer are the same.

[0155] Embodiment 19

[0156] The positive electrode sheet and negative electrode sheet and the assembly process are basically the same as those in Example 7, except that 3) the preparation of the porous insulating base layer is omitted, and a 7μm isolation film (composition: silicon dioxide and polyacrylonitrile in a mass ratio of 8:2, and the Dv50 particle size of silicon dioxide is 0.5μm) is directly used between the positive electrode sheet and the negative electrode sheet, and the same gel electrolyte solution as in Example 1 is used for in-situ curing. Among them, the composition of the isolation film includes a 5μm PE substrate and a composite film layer coated on two opposite surfaces of the PE substrate, the total thickness of the composite film layer is 2μm, and the composition of the composite film layer is silicon dioxide and polyacrylonitrile in a mass ratio of 8:2, and the Dv50 particle size of silicon dioxide is 0.5μm.

[0157] Comparative Example 1

[0158] The positive electrode sheet, negative electrode sheet and assembly process are basically the same as those of Example 19, with the only difference being that the steps of preparing the gel electrolyte solution in 4) and curing in 5) are omitted, that is, instead of using the gel electrolyte solution, an electrolyte not containing vinyl carbonate monomer and initiator is used, and the electrolyte is prepared as follows: EC, EMC and DEC in a volume ratio of 1:1:1 are used as a mixed solvent, and LiPF6 is added as a lithium salt to prepare a 1M LiPF6 electrolyte.

[0159] Comparative Example 2

[0160] It is basically the same as Example 1, except that it omits the step 3) of preparing a porous insulating base layer, and directly injects the above-mentioned gel electrolyte solution between the positive electrode plate and the negative electrode plate; that is, the above-mentioned insulating layer is not formed, and no isolation membrane is used.

[0161] The following is a performance test.

[0162] 1. 180 degree peel strength

[0163] Specifically, the test method for 180 degree peel strength is as follows:

[0164] The prepared battery cells (including the stacked positive electrode sheets, insulating layer, gel electrolyte layer and negative electrode sheets as a whole) were used as test samples. The test standard was based on GB / T 2792-2014. The test results of 180-degree peel strength are shown in Table 1.

[0165] It should be noted that the test result of the 180-degree peel strength represents the corresponding strength when the two layers with the smallest bonding force are peeled off when the sample is tested as a whole. In Comparative Example 1, the electrolyte is liquid, so the 180-degree peel strength test is not performed.

[0166] 2. Volumetric energy density

[0167] At 25°C, charge to the upper limit voltage at 0.33C standard, charge to 0.05C at the upper limit voltage constant voltage, let it stand for 10 minutes, and discharge to the lower limit voltage at 0.33C. Record the discharge capacity and then calculate the energy density during discharge.

[0168] Energy density (Wh / L) = discharge capacity (Wh) / secondary battery volume (L).

[0169] 3. Self-discharge voltage drop after 48 hours of full charge storage

[0170] At 25°C, charge to the upper limit voltage at 0.33C standard, charge to 0.05C at the upper limit voltage constant voltage, let stand for 10 minutes, discharge at 0.33C for 2.1 hours, test the open circuit voltage at this time, recorded as OCV1, store at 60°C to 80% SOH and let stand for 48 hours, test the open circuit voltage again, recorded as OCV2, and the self-discharge voltage drop is the difference between the two.

[0171] Self-discharge voltage drop = OCV1-OCV2.

[0172] The self-discharge voltage drop of a fully charged battery stored at 60°C for 48 hours is used to examine the damage caused by lithium dendrites generated by high-temperature storage to the battery.

[0173] 4. Acupuncture test

[0174] Charge to the upper limit voltage at 0.33C standard at 25℃, charge to 0.05C at the upper limit voltage constant voltage, then use a φ1mm steel needle to penetrate 6mm into the battery cell at a speed of 0.1mm / s, then let it stand for 60 minutes and observe the battery cell status.

[0175] Table 1

[0176]

[0177]

[0178] As can be seen from Table 1, Comparative Example 1 uses an independent isolation membrane and liquid electrolyte, which has the risk of explosion. However, each embodiment of the present application uses a gel electrolyte, and no explosion occurs in the needle puncture test.

[0179] Furthermore, compared with the various embodiments of the present application, Comparative Example 1 has a higher self-discharge voltage drop, indicating that the battery is prone to produce a large number of lithium dendrites that are detrimental to the battery, causing damage to the battery; in addition, the volume energy density of Comparative Example 1 is relatively low.

[0180] Comparative Example 2 does not have a porous insulating base layer, and only uses in-situ curing to form a gel electrolyte layer. Its self-discharge voltage drop is large, significantly higher than that of each embodiment of the present application, indicating that the battery is prone to produce a large number of lithium dendrites that are unfavorable to the battery, causing damage to the battery. In addition, Comparative Example 2 does not have a porous insulating base layer, so its peel strength is relatively small; its volume energy density is relatively high because the battery thickness is small and the volume is reduced.

[0181] Compared with comparative examples 1 to 2, the embodiments of the present application, while having a higher volume energy density, improve the overall mechanical strength of the secondary battery, reduce the self-discharge voltage drop of the battery caused by lithium dendrites, and reduce the risk of battery failure and damage caused by lithium dendrites; in addition, the problem of damage to the secondary battery caused by external collision stress during use can be further improved.

[0182] It can be seen from Examples 1 to 5 that the batteries made with SiO2 Dv50 in the insulating layer of 0.5 μm to 7 μm have good volume energy density, while reducing the risk of battery failure caused by lithium dendrites and the degree of damage caused by external collision stress during use of the secondary battery. It can be seen from Examples 6 to 9 that the thickness of the insulating layer is ≤ 18 μm, and can be greater than 3 μm, for example, 7 μm to 18 μm.

[0183] It can be seen from Examples 10 to 13 that the curing temperature is within the range of 50 to 100°C, further preferably 60 to 90°C, and further preferably 70 to 90°C.

[0184] It can be seen from Examples 14 to 17 that the curing time is within 5 hours to 20 hours, and can be selected as 10 hours to 20 hours.

[0185] It can be seen from Example 1 and Example 18 that the insulating layer is formed on the positive electrode sheet or the negative electrode sheet, and the performance of the batteries produced therefrom is equivalent.

[0186] It can be seen from Examples 7 and 19 that, compared with setting up an independent isolation film, pre-forming an insulating layer on the positive electrode plate can further improve the peel strength of the battery, reduce the self-discharge voltage drop of the battery caused by lithium dendrites, and reduce the degree of damage to the battery caused by collision.

[0187] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0188] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description and drawings can be used to interpret the content of the claims.

Claims

1. A secondary battery, It is characterized in that include: Positive electrode; A negative electrode sheet, arranged opposite to the positive electrode sheet; A gel electrolyte layer, disposed between the positive electrode sheet and the negative electrode sheet; and An insulating layer is provided between the gel electrolyte layer and the positive electrode plate, and / or between the gel electrolyte layer and the negative electrode plate, wherein the insulating layer comprises a porous insulating base layer and a gel electrolyte filled in pores of the porous insulating base layer, wherein the insulating layer is bonded to the gel electrolyte layer, and the gel electrolyte is connected to the gel electrolyte layer.

2. The secondary battery according to claim 1, It is characterized in that The insulating layer is bonded to the positive electrode sheet and / or the negative electrode sheet; and / or, The gel electrolyte layer is bonded to the positive electrode sheet or the negative electrode sheet.

3. The secondary battery according to claim 1, It is characterized in that The 180-degree peel strength of the positive electrode sheet, the porous insulating base layer, the gel electrolyte layer and the negative electrode sheet as a whole is 10 N / m to 35 N / m; Optionally, the 180-degree peel strength of the positive electrode sheet, the porous insulating base layer, the gel electrolyte layer and the negative electrode sheet as a whole is 12 N / m to 35 N / m.

4. The secondary battery according to claim 1, It is characterized in that The gel electrolyte forms a continuous phase with the gel electrolyte layer.

5. The secondary battery according to claim 1, It is characterized in that The thickness of the insulating layer is ≤18 μm, and may be 3 μm to 18 μm, and may be 7 μm to 18 μm.

6. The secondary battery according to any one of claims 1 to 5, It is characterized in that The material of the insulating layer includes at least one of an insulating ceramic material and an insulating polymer material.

7. The secondary battery according to claim 6, It is characterized in that The material of the insulating layer includes insulating ceramic material and insulating organic material; optionally, the mass ratio of the insulating ceramic material to the insulating polymer material is (7-9): (1-3).

8. The secondary battery according to claim 6, It is characterized in that The secondary battery satisfies at least one of the following conditions (1-a) to (1-c): (1-a) The insulating ceramic material includes at least one of aluminum oxide, silicon dioxide, magnesium oxide, boehmite, aluminum hydroxide, magnesium hydroxide, zirconium dioxide, lithium zirconate, lithium phosphate, lithium aluminate, lithium fluoride, lithium carbonate, lithium oxalate, lithium silicate and silicic acid; (1-b) The Dv50 particle size of the insulating ceramic material is 0.5 μm to 7 μm, and can be optionally 1 μm to 5 μm; (1-c) The insulating polymer material includes at least one of polyvinylidene fluoride, polyethylene, polymethacrylate, polyacrylonitrile and styrene-butadiene rubber.

9. The secondary battery according to any one of claims 1 to 5, 7 to 8, It is characterized in that The secondary battery satisfies at least one of the following conditions (2-a) to (2-b): (2-a) The average pore size of the porous insulating base layer is 20 nm to 400 nm, and can be 50 nm to 300 nm; (2-b) The porosity of the porous insulating base layer is 30% to 70%, and can be optionally 50% to 65%.

10. The secondary battery according to any one of claims 1 to 5, 7 to 8, It is characterized in that The gel electrolyte and the gel electrolyte layer include a polymer and an electrolyte salt; Optionally, the monomer of the polymer includes at least one of an ester monomer, an ether monomer, a nitrile monomer, a sulfone monomer and a siloxane monomer; Optionally, the electrolyte salt includes at least one of an electrolyte lithium salt and an electrolyte sodium salt.

11. The secondary battery according to any one of claims 1 to 5, 7 to 8, It is characterized in that The secondary battery satisfies at least one of the following conditions (3-a) to (3-c): (3-a) The thickness of the gel electrolyte layer is 0.2 μm to 2 μm; (3-b) The positive electrode sheet includes a positive electrode active layer, and the thickness of the positive electrode active layer is 100 μm to 250 μm; (3-c) The negative electrode sheet includes a negative electrode active layer, and the thickness of the negative electrode active layer is 80 μm to 200 μm.

12. A method for preparing a secondary battery, It is characterized in that The steps include: A porous insulating base layer is provided between the positive electrode sheet and the negative electrode sheet; Assembling the positive electrode sheet, the porous insulating base layer and the negative electrode sheet into a battery cell; A gel electrolyte solution is injected into the battery cell, and the gel electrolyte solution is solidified to form a gel electrolyte layer and a gel electrolyte between the positive electrode sheet and the negative electrode sheet and in the pores of the porous insulating base layer, respectively.

13. The preparation method according to claim 12, It is characterized in that The step of providing a porous insulating base layer between the positive electrode sheet and the negative electrode sheet comprises: A porous insulating base layer is formed on the surface of the positive electrode sheet and / or the negative electrode sheet.

14. The preparation method according to claim 12 or 13, It is characterized in that The preparation method satisfies at least one of the following conditions (4-a) to (4-c): (4-a) The gel electrolyte solution comprises a polymerizable monomer, an initiator, an electrolyte salt and a solvent; (4-b) The curing temperature is 50 to 100° C., and can be 60 to 90° C.; (4-c) The curing time is 5 hours to 20 hours, and can be optionally 10 hours to 20 hours.

15. An electrical device, It is characterized in that Comprising the secondary battery according to any one of claims 1 to 11.

Citation Information

Cited By

  • High-rate negative pole piece and preparation method thereof, sodium ion battery and electric equipment