Preparation method of bi-component carbon brush

By combining low-resistance and high-resistance materials in the carbon brush, the problem of reduced lubrication performance and difficulty in performance coordination of the carbon brush is solved, a balance of resistivity, friction and commutation performance is achieved, and the stability and spark of the carbon brush are improved. Inhibition ability.

CN118783205APending Publication Date: 2024-10-15JIANGSU YUANJINGHONG SCI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410983017.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The lubrication performance of existing carbon brushes decreases when friction heats up, and the performance differences between graphite and binder and imperfect processes make it difficult to coordinate resistivity, friction and commutation performance, making it impossible to meet actual needs.

Method used

A two-component carbon brush preparation method is adopted, which combines low-resistance materials (single-layer graphene, copper powder, tin powder) and high-resistance materials (double-layer graphene, bamboo charcoal fiber), and undergoes plasma treatment, ball milling and sintering. , forming a carbon brush with balanced resistivity and friction properties.

Benefits of technology

It achieves the coordination of the resistivity, friction and commutation performance of the carbon brush, improves stability and spark suppression capabilities, and improves the operating performance of the carbon brush.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004956619500000061
    Figure BDA0004956619500000061
  • Figure BDA0004956619500000071
    Figure BDA0004956619500000071
Patent Text Reader

Abstract

The invention belongs to the field of novel carbon materials, and discloses a bi-component carbon brush and a preparation method thereof. The raw materials of the carbon brush disclosed by the invention comprise a material A and a material B according to a mass ratio of (2-4): 5, the material A is a low-resistance material, and the material B is a high-resistance material; the low-resistance material contains single-layer graphene, and the high-resistance material contains double-layer graphene and bamboo charcoal fibers. The preparation method of the carbon brush comprises the following steps that single-layer graphene, copper powder and tin powder are taken and treated with plasmas respectively; the treated single-layer graphene, copper powder and tin powder are mixed to obtain a mixture, a binder is added into the mixture for mixing, the mixture is pressed into a blank under preset pressure, primary sintering is conducted, and a material A is obtained; ball-milling the double-layer graphene and the bamboo charcoal fiber, adding the copper powder, the tin powder and the binder, mixing, pressing into a blank body under preset pressure, and performing primary sintering; and laminating the prepared material A and the material B, carrying out vacuum pressing, compressing, and carrying out secondary sintering to obtain the bi-component carbon brush.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of novel carbon materials, and in particular relates to a method for preparing a two-component carbon brush. Background Art

[0002] Carbon brushes, also called electric brushes, are widely used as sliding contacts in many electrical devices. The main function of carbon brushes is to conduct electricity while rubbing against metals. It is not like when metal rubs against metal; when metal rubs against metal, the friction may increase, and the intersection may sinter together; but carbon brushes will not, because carbon and metal are two different elements. It is mostly used in electric motors, and its shapes are various, including square and round.

[0003] The materials of carbon brushes are mainly graphite, impregnated graphite, metal (containing copper, silver) graphite, etc. Carbon brushes are devices for transmitting energy or signals between the fixed part and the rotating part of motors, generators or other rotating machinery. They are generally made of pure carbon and a coagulant. They are generally square in shape and stuck on a metal bracket. There is a spring inside to press it tightly on the shaft. When the motor rotates, the electric energy is transmitted to the coil through the commutator. When the carbon brush heats up due to friction, the lubrication performance of the carbon brush itself decreases, which further increases the temperature. In addition, due to the performance differences between graphite and binder and the imperfections in the process, the performance of graphite carbon brushes is affected and cannot meet the requirements of certain environments. At the same time, there is a contradiction that appropriate resistivity, excellent friction and wear, and good commutation performance cannot be coordinated and unified, which cannot meet actual needs well. Summary of the invention

[0004] In view of the above problems existing in the current carbon brushes, the present invention aims to provide a two-component carbon brush and a preparation method thereof, which can balance the resistivity, friction and commutation performance of the carbon brush.

[0005] A two-component carbon brush, wherein the raw materials of the carbon brush include material A and material B in a mass ratio of 2 to 4:5; the material A is a low-resistance material, and the material B is a high-resistance material; the low-resistance material contains a single-layer graphene, and the high-resistance material contains a double-layer graphene and bamboo charcoal fiber.

[0006] Furthermore, the material A is prepared by taking a single layer of graphene, copper powder and tin powder and treating them with plasma respectively; the treated single layer of graphene, copper powder and tin powder are mixed to obtain a mixture, a binder is added to the mixture, and the mixture is pressed into a blank under a predetermined pressure, and sintered once.

[0007] Furthermore, the material B is prepared by ball-milling double-layer graphene and bamboo charcoal fibers, adding copper powder, tin powder and a binder, and pressing them into an embryo under a predetermined pressure, and sintering them once.

[0008] Furthermore, the binder is a combination of phenolic resin and epoxy resin in a mass ratio of 4 to 8:1.

[0009] A method for preparing a two-component carbon brush, the method for preparing the carbon brush comprising the following steps:

[0010] (1) taking 30 to 40 parts of single-layer graphene, 30 to 40 parts of copper powder, and 20 to 30 parts of tin powder by weight and treating them respectively with plasma; mixing the treated single-layer graphene, copper powder, and tin powder to obtain a mixture, adding a binder of 10 to 15% by weight of the mixture to the mixture, pressing it into an embryo under a predetermined pressure, and sintering it once to obtain material A;

[0011] (2) taking 30-40 parts of double-layer graphene and 12-20 parts of bamboo charcoal fiber by weight, ball-milling them, adding 30-40 parts of copper powder, 12-20 parts of tin powder, and 10-15 parts of binder by weight as above, mixing them, pressing them into an embryo under a predetermined pressure, and sintering them once to obtain material B;

[0012] (3) The prepared material A and material B are pressed together in vacuum until the two parts are equal in volume and size, and then sintered for a second time to obtain a two-component carbon brush.

[0013] Furthermore, the conditions of the plasma treatment in step (1) are as follows: in a nitrogen atmosphere, the gas pressure is adjusted to 50-70 Pa, the treatment power is 100-150 W, and the treatment time is 1-5 min.

[0014] Furthermore, the primary sintering temperature in steps (1) and (2) is 500-650° C., and the temperature is maintained for 1-2 hours in a nitrogen atmosphere.

[0015] Furthermore, the conditions for the secondary sintering in step (3) are: a temperature of 500 to 650° C., a mixed atmosphere of nitrogen and hydrogen in a volume ratio of 3 to 5:1, and heat preservation for 1 to 2 hours.

[0016] Furthermore, the ball milling conditions in step (2) are: using 70-80% anhydrous ethanol of the weight of the double-layer graphene and bamboo charcoal fiber as the medium, and ball milling at 300-500 r / min for 1-3 hours.

[0017] Compared with the prior art, the advantages of the present invention are:

[0018] The two-component carbon brush disclosed in the present invention provides a new solution combining high resistance on one side and low resistance on the other side. The low resistance side adopts activated single-layer graphene, copper powder and tin powder as main raw materials, and contains only a graphene structure of one carbon atom layer (single-layer graphene), which is conducive to significantly reducing resistance and improving the stability of this side. The high resistance side adopts a solution combining double-layer graphene and bamboo charcoal fiber, wherein the double-layer graphene is a graphene with two layers of carbon atoms arranged in a hexagonal lattice structure, and there is a van der Waals force between the two layers of graphene structure, and bamboo charcoal fibers with a honeycomb microporous structure are dispersed therein, which greatly improves the resistivity. Moreover, at a certain temperature, the resistivity of the double-layer graphene will show parity changes, which is combined with the low resistance single-layer graphene side, which is convenient for the commutation performance to be exerted, so that the low-high resistance formation system operates, the self-lubricating performance is good, the overall spark suppression ability is strong, and the operation of the carbon brush is improved. DETAILED DESCRIPTION

[0019] The following provides a specific implementation of a two-component carbon brush and a preparation method thereof of the present invention. It is necessary to point out that the following examples are only used to explain the present invention in more detail, rather than to narrow the scope of protection of the present invention. After reading the present invention, improvements and adjustments made by professionals in this technical field without departing from the concept of the present invention are within the scope of protection claimed by the present invention.

[0020] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0021] Example 1

[0022] A method for preparing a two-component carbon brush comprises the following steps:

[0023] (1) taking 30 parts of single-layer graphene, 30 parts of copper powder, and 20 parts of tin powder by mass and treating them respectively with plasma; mixing the treated single-layer graphene, copper powder, and tin powder to obtain a mixture, adding a binder of 10% by mass of the mixture to the mixture, pressing it into an embryo under a predetermined pressure, and sintering it once to obtain material A;

[0024] (2) 30 parts of double-layer graphene and 12 parts of bamboo charcoal fiber were ball-milled by weight, and then 30 parts of copper powder, 12 parts of tin powder, and 10 parts of binder were added and mixed, and pressed into an embryo under a predetermined pressure, and sintered once to obtain material B;

[0025] (3) The prepared material A and material B are pressed together in vacuum until the two parts are equal in volume and size, and then sintered for a second time to obtain a double-layer carbon brush.

[0026] The conditions of the plasma treatment in step (1) are as follows: in a nitrogen atmosphere, the gas pressure is adjusted to 60 Pa, the treatment power is 120 W, and the treatment time is 5 min.

[0027] The primary sintering temperature in steps (1) and (2) is 600° C. and the temperature is maintained for 1 hour in a nitrogen atmosphere.

[0028] The secondary sintering conditions in step (3) are as follows: temperature of 600° C., nitrogen and hydrogen mixed atmosphere in a volume ratio of 4:1, and heat preservation for 1 hour.

[0029] The ball milling conditions in step (2) are as follows: using the double-layer graphene and bamboo charcoal fiber in anhydrous ethanol (80%) as the medium, and ball milling at 300 r / min for 1 hour.

[0030] Example 2

[0031] A method for preparing a two-component carbon brush comprises the following steps:

[0032] (1) taking 35 parts of single-layer graphene, 35 parts of copper powder, and 25 parts of tin powder by weight and treating them respectively with plasma; mixing the treated single-layer graphene, copper powder, and tin powder to obtain a mixture, adding a binder of 12% by weight of the mixture to the mixture, pressing it into a blank under a predetermined pressure, and sintering it once to obtain material A;

[0033] (2) 35 parts of double-layer graphene and 18 parts of bamboo charcoal fiber were ball-milled by weight, and then 35 parts of copper powder, 18 parts of tin powder, and 13 parts of binder were added by weight, mixed, pressed into an embryo under a predetermined pressure, and sintered once to obtain material B;

[0034] (3) The prepared material A and material B are pressed together in vacuum until the two parts are equal in volume and size, and then sintered for a second time to obtain a double-layer carbon brush.

[0035] The conditions of the plasma treatment in step (1) are as follows: in a nitrogen atmosphere, the gas pressure is adjusted to 60 Pa, the treatment power is 120 W, and the treatment time is 5 min.

[0036] The primary sintering temperature in steps (1) and (2) is 600° C. and the temperature is maintained for 1 hour in a nitrogen atmosphere.

[0037] The secondary sintering conditions in step (3) are as follows: temperature of 600° C., nitrogen and hydrogen mixed atmosphere in a volume ratio of 4:1, and heat preservation for 1 hour.

[0038] The ball milling conditions in step (2) are as follows: using the double-layer graphene and bamboo charcoal fiber in anhydrous ethanol (80%) as the medium, and ball milling at 300 r / min for 1 hour.

[0039] Example 3

[0040] A method for preparing a two-component carbon brush comprises the following steps:

[0041] (1) taking 40 parts of single-layer graphene, 40 parts of copper powder, and 30 parts of tin powder by weight and treating them respectively with plasma; mixing the treated single-layer graphene, copper powder, and tin powder to obtain a mixture, adding a binder of 15% by weight of the mixture to the mixture, pressing it into an embryo under a predetermined pressure, and sintering it once to obtain material A;

[0042] (2) 40 parts of double-layer graphene and 20 parts of bamboo charcoal fiber were ball-milled by weight, and then 40 parts of copper powder, 20 parts of tin powder, and 15 parts of binder were added and mixed, and pressed into an embryo under a predetermined pressure, and sintered once to obtain material B;

[0043] (3) The prepared material A and material B are pressed together in vacuum until the two parts are equal in volume and size, and then sintered for a second time to obtain a double-layer carbon brush.

[0044] The conditions of the plasma treatment in step (1) are as follows: in a nitrogen atmosphere, the gas pressure is adjusted to 60 Pa, the treatment power is 120 W, and the treatment time is 5 min.

[0045] The primary sintering temperature in steps (1) and (2) is 600° C. and the temperature is maintained for 1 hour in a nitrogen atmosphere.

[0046] The secondary sintering conditions in step (3) are as follows: temperature of 600° C., nitrogen and hydrogen mixed atmosphere in a volume ratio of 4:1, and heat preservation for 1 hour.

[0047] The ball milling conditions in step (2) are as follows: using the double-layer graphene and bamboo charcoal fiber in anhydrous ethanol (80%) as the medium, and ball milling at 300 r / min for 1 hour.

[0048] Comparative Example 1: It is basically the same as Example 3, except that the bamboo charcoal fiber is omitted.

[0049] Comparative Example 2: is basically the same as Example 3, except that the double-layer graphene is replaced by a single-layer graphene.

[0050] Comparative Example 3: is basically the same as Example 3, except that the single-layer graphene is replaced by a double-layer graphene.

[0051] The carbon brushes obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to performance tests, and the obtained results are as follows.

[0052] Table 1. Volume resistivity test results

[0053]

[0054]

[0055] As can be seen from Table 1, the two-component carbon brushes of Examples 1 to 3 have significant performance in improving the spark level. Comparative Example 1 omits the bamboo charcoal fiber, which causes the friction coefficient on the B side to decrease to a certain extent, and the spark level remains unchanged; Comparative Examples 2 and 3 show that replacing the double-layer graphene with a single-layer graphene increases the friction coefficient, and the friction coefficient on the B side decreases to a certain extent, and the spark level remains unchanged. Comparative Example 3 replaces the single-layer graphene with a double-layer graphene, which causes the friction coefficient on the A side to increase to a certain extent, and the spark level becomes 1 / 2 level. It can be seen that the two-component carbon brush disclosed in the present invention has a significant effect in controlling the friction coefficient and spark level, which is conducive to commutation.

[0056] Note: The above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention; therefore, although this specification has described the present invention in detail with reference to the above embodiments, a person skilled in the art should understand that the present invention can still be modified or replaced by equivalents; and all technical solutions and improvements thereof that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A two-component carbon brush, characterized in that: The raw materials of the carbon brush include material A and material B in a mass ratio of 2 to 4:5; the material A is a low-resistance material, and the material B is a high-resistance material; the low-resistance material contains single-layer graphene, and the high-resistance material contains double-layer graphene and bamboo charcoal fiber.

2. The two-component carbon brush according to claim 1, characterized in that: Preparation of the material A: taking a single layer of graphene, copper powder, and tin powder and treating them with plasma respectively; mixing the treated single layer of graphene, copper powder, and tin powder to obtain a mixture, adding a binder to the mixture, pressing it into a green body under a predetermined pressure, and performing a sintering process.

3. The two-component carbon brush according to claim 1, characterized in that: Preparation of the material B: double-layer graphene and bamboo charcoal fiber are ball-milled, copper powder, tin powder and a binder are added and mixed, pressed into an embryo under a predetermined pressure, and sintered once.

4. The two-component carbon brush according to claim 2 or 3, characterized in that: The binder is a combination of phenolic resin and epoxy resin in a mass ratio of 4 to 8:

1.

5. A method for preparing a two-component carbon brush according to any one of claims 1 to 4, characterized in that: The preparation method of the carbon brush comprises the following steps: (1) Taking 30 to 40 parts by mass of single-layer graphene, 30 to 40 parts of copper powder, and 20 to 30 parts of tin powder and treating them respectively with plasma; mixing the treated single-layer graphene, copper powder, and tin powder to obtain a mixture, adding a binder in an amount of 10 to 15% by mass of the mixture to the mixture, pressing it into a blank under a predetermined pressure, and sintering it once to obtain material A; (2) 30-40 parts by mass of double-layer graphene and 12-20 parts by mass of bamboo charcoal fiber were ball-milled, and then 30-40 parts by mass of copper powder, 12-20 parts by mass of tin powder, and 10-15 parts by mass of a binder were added and mixed, and pressed into an embryo under a predetermined pressure, and sintered once to obtain material B; (3) The prepared material A and material B are pressed together in vacuum until the two parts have equal volume and size, and then sintered for the second time to obtain a two-component carbon brush.

6. The method for preparing a two-component carbon brush according to claim 5, characterized in that: The conditions for the plasma treatment in step (1) are as follows: under a nitrogen atmosphere, the gas pressure is adjusted to 50-70 Pa, the treatment power is 100-150 W, and the treatment time is 1-5 min.

7. The method for preparing a two-component carbon brush according to claim 5, characterized in that: The primary sintering temperature in steps (1) and (2) is 500-650° C., and the temperature is kept at 1-2 hours under a nitrogen atmosphere.

8. The method for preparing a two-component carbon brush according to claim 5, characterized in that: The conditions for the secondary sintering in step (3) are: a temperature of 500-650° C., a mixed atmosphere of nitrogen and hydrogen in a volume ratio of 3-5:1, and heat preservation for 1-2 hours.

9. The method for preparing a two-component carbon brush according to claim 5, characterized in that: The ball milling conditions in step (2) are: using 70-80% anhydrous ethanol of the weight of the double-layer graphene and bamboo charcoal fiber as the medium, and ball milling at 300-500 r / min for 1-3 hours.