Upper layer system for absorbent articles
By using a specific combination of nonwoven fiber mesh materials and an anti-adhesive layer in feminine sanitary pads, the problems of backflow and stain spread when the topsheet material absorbs fluid quickly are solved, resulting in more efficient fluid management and comfort.
Patent Information
- Application Number
- CN202380023925.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-03
- Filing Date
- 2023-03-03
- Publication Date
- 2024-10-15
AI Technical Summary
The top sheet material of existing feminine sanitary pads is difficult to effectively prevent backflow and stain spread while quickly absorbing fluid, and conventional materials may not be soft enough or mechanically strong enough to meet the multiple needs of consumers.
By employing a specific combination of nonwoven fiber web materials, including a mixture of hydrophobic and hydrophilic fibers, and bonding them through the formation of a pore pattern and heat treatment, combined with an anti-sticking layer, the structure and performance of the fluid management layer are optimized to achieve rapid collection and low backflow.
It improves fluid collection speed, reduces backflow and stain spread, provides better comfort and mechanical strength, and meets the diverse usage needs of consumers.
Smart Images

Figure CN118785877A_ABST
Abstract
Description
Background Art
[0001] Absorbent articles of various designs have been used for many years for the purpose of intercepting, capturing, containing and absorbing body exudates, including menstrual fluids, urine and feces, and for the purpose of managing the exudates to prevent soiling of underwear, outer clothing, bedding, etc.
[0002] A type of absorbent article, a feminine hygiene pad (also known as a "sanitary napkin," "menstrual pad," etc.) has been used by women to manage the discharge of menstrual fluid during menstruation. A typical feminine hygiene pad comprises: a liquid-permeable topsheet that forms the body / wearer-facing surface of the pad; a liquid-impermeable backsheet that forms the outward-facing surface of the pad and acts as a barrier to prevent fluid absorbed by the pad from migrating to and leaving the outward-facing surface of the pad; and an absorbent structure that provides fluid handling functions to a lesser or greater degree in any desired combination during the desired wear / use duration of the pad, including fluid interception, distribution within the pad, absorption, containment, and storage. The configuration, shape, and size of a typical pad are set to be placed and worn in the crotch region of the intended user's underwear. Many pads include a deposit of one or more adhesives on the outward-facing surface of the backsheet to enable the wearer to attach the pad to the inner surface of an undergarment to help keep it in place during wear / use.
[0003] A variety of materials have been developed and used to form topsheets for feminine hygiene pads.
[0004] In some examples, the topsheet may be formed from a polymeric film having a pattern of holes formed therein. The holes are used to allow expelled fluid to pass through the topsheet to the absorbent components of the pad disposed beneath the topsheet. However, some segments of the consumer market may not prefer film topsheets for various reasons, which may include how they feel against the skin.
[0005] In other examples, the top sheet can be formed by a fiber nonwoven web material. Countless combinations of the features of nonwovens are possible. The fiber composition can be relatively long fibers of uncertain and different lengths, or can be short fibers. They can include natural fibers (e.g., cotton fibers); semi-synthetic fibers (e.g., regenerated cellulose (rayon)) fibers. They can include single-component or multi-component fibers. The fibers can be relatively straight, or encircled or curled. Spun fibers can be spun from a variety of polymer components. The aggregates of the precursor batt or the constituent fibers can be consolidated, and the fibers are kept together, whereby the web has fabric-like properties and structural integrity, which are given by a variety of mechanisms including fiber entanglement, fiber-to-fiber melt bonding, fiber-to-fiber binder / adhesive bonding, etc. Any desired selection of different types of fibers can be included, layered and / or blended in any desired weight ratio to form a nonwoven web. Any part or all of the constituent fibers or nonwoven webs can be treated to impart or increase the hydrophobicity or hydrophilicity of the surface of the fibers, or any combination or arrangement thereof.
[0006] Generally speaking, users expect the topsheet of a feminine sanitary pad to:
[0007] - an absorbent component that easily receives menstrual fluid and promotes its rapid downward passage in the z direction to the underlying layer (rapid acquisition);
[0008] -Prevents xy-directional diffusion and contamination of menstrual fluid;
[0009] - inhibits fluid reacquisition from the underlying absorbent component and allows fluid to migrate upward in the z-direction through (rewet) back to the wearer-facing surface (causing a sensation of wetness and / or a perception of incomplete absorption and less effective protection to the wearer);
[0010] - conceal, to the most practical extent, from view therethrough, menstrual fluid that has been absorbed by the underlying absorbent component (for perception of effective absorption and cleansing); and
[0011] - Feels soft and comfortable against the wearer's skin, and dry, including after fluid insult.
[0012] These goals are conflicting to some extent.For example, the top sheet of the nonwoven web material that is easy to wick fluid downward in the z direction may also tend to keep fluid to a certain extent, or be easy to wick back fluid upward in the z direction (re-seepage), or wick fluid along the xy direction, thereby causing stain diffusion.On the contrary, the top sheet that prevents the z-direction fluid from moving from the absorbent component to the surface facing the wearer may also prevent the xy-direction fluid from moving / wicking, but may not be easy to receive fluid and pass it downward to the absorbent component (that is, showing slow collection).The fibrous web with considerable permeability (provided by, for example, large pore volume) may be easy to receive fluid and allow fluid to pass therethrough, but may not be mechanically strong enough for processing on the processing line, or may not be opaque enough or the appearance is not strong enough to be accepted by consumers / users.A variety of methods have been tried, through countless combinations of different components, configurations and features identified above, to meet conflicting goals as well as possible.However, there is still an opportunity for improvement. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Although the specification ends with claims that specifically point out and clearly claim what is considered to be the subject matter of the present invention, it is believed that the invention can be more fully understood from the following description in conjunction with the accompanying drawings. Some of these figures may have been simplified by omitting selected elements in order to more clearly show other elements. Such omissions of elements in certain figures do not necessarily indicate the presence or absence of a particular element in any exemplary embodiment unless such is clearly described in the corresponding text description. The drawings are not drawn to scale.
[0014] Figure 1A A schematic plan view (in the z-direction) of an example of an absorbent article is depicted.
[0015] Figure 1B for Figure 1A A schematic plan view (along the z-direction) of an example of an absorbent core component layer of the absorbent article depicted in .
[0016] Figure 2 is a schematic depiction of an example of an arrangement of equipment and processes that may be configured to manufacture a fluid management layer.
[0017] Figure 3 Schematic depiction of an example of a cross section of a fluid management layer taken along a z-direction plane.
[0018] Figure 4 is a plan view (in the z-direction) image of a portion of a nonwoven web material having a pattern of holes therethrough.
[0019] Figure 5 The image is a plan view (in the z-direction) of a portion of a nonwoven web material having holes therethrough.
[0020] Figure 6 is a top view of a strikethrough plate used in the "Acquisition Time and Rewet Measurement Method" described herein.
[0021] Figure 7 is a bottom view of a strikethrough plate used in the "Acquisition Time and Rewet Measurement Method" described herein.
[0022] Fig. 8A is along the z direction and Figure 6 A cross-sectional view of a strikethrough panel used in the "Acquisition Time and Rewet Measurement Methods" described herein, taken along the plane defined by line AA shown in FIG.
[0023] Figure 8B is along the z direction and Figure 6 A cross-sectional view of a strikethrough panel used in the "Acquisition Time and Rewet Measurement Methods" described herein, taken along the plane defined by line BB shown in FIG.
[0024] Fig. 9 Graph presenting the second acquisition time measured for samples of eight prototype feminine hygiene pads measured using the "Acquisition Time and Rewet Measurement Method" described herein.
[0025] Fig.10 Graph presenting the sum of Surface Free Fluid (SFF) and Rewet measured for samples of 10 prototype feminine hygiene pads measured using the "Acquisition Time and Rewet Measurement Method" described herein. DETAILED DESCRIPTION
[0026] definition
[0027] As used herein, the following terms shall have the meanings specified below:
[0028] "Absorbent article" refers to a wearable device that absorbs and contains liquids, and more specifically, refers to a device that is placed close to or adjacent to the wearer's body and is used to absorb and contain the various exudates discharged from the body. Absorbent articles may include diapers, training pants, adult incontinence underwear (e.g., liners, pads, and briefs) and / or feminine hygiene products, including feminine hygiene pads (also known as, for example, "sanitary napkins", "menstrual pads", "sanitary pads", etc.).
[0029] As used herein, the term "integrated" is used to describe fibers of nonwoven materials that have been interwoven, entangled, and / or pushed / pulled in the positive and / or negative z-direction (thickness direction of the nonwoven material). Some exemplary methods for integrating the fibers of nonwoven webs include hydroentanglement and needle punching. Spunlacing (also referred to as "hydroentangling" or ("water enhancement")) uses multiple high-pressure water jets directed to the precursor batts or aggregates of the fibers transmitted longitudinally to entangle the fibers. Needle punching (also referred to as "needle punching (needle punching)") involves using needles of special features to mechanically push and / or pull fibers, precursor batts of fibers, or aggregates in the z-direction so that they are entangled with other fibers in the batts or aggregates.
[0030] As used herein, the term "combed" is used to describe the structural features of the fluid management layer described herein. The carded nonwoven web is formed by fibers cut into specific limited lengths, which are otherwise referred to as "short length fibers". The short length fibers can have any selected length. For example, the short length fibers can be cut into a length of up to 120 mm, as short as a length of 10 mm. However, if a particular group of fibers is short length fibers, the length of each of the fibers in the carded nonwoven is approximately the same, that is, short length. In the case where more than one composition of fibers is included in a nonwoven web (e.g., a web including polypropylene fibers and viscose fibers), the length of each fiber of the same composition may be substantially the same, while the corresponding short fiber lengths of the corresponding fiber compositions may be different.
[0031] In contrast to staple fibers, filaments such as those produced by weaving, for example, in a spunbond or meltblown nonwoven web manufacturing process, are generally not short-length fibers. Instead, these filaments are sometimes characterized as "continuous" fibers, meaning that they have a relatively long and indefinite length and are not cut into specific lengths after weaving, as their staple counterparts do.
[0032] "Lateral" - with respect to absorbent articles such as feminine hygiene pads or parts thereof, refers to the direction parallel to a horizontal line tangent to the front surface of the upper portion of the wearer's legs adjacent to the torso when the pad is worn normally and the wearer assumes a flat, square, normal standing position. The "width" dimension of any component or feature of an article such as a feminine hygiene pad is measured in the lateral direction. When the article or a component thereof is laid flat on a horizontal surface, the "lateral" direction corresponds to the lateral direction relative to the structure when it is worn, as defined above. With respect to articles such as feminine hygiene pads that are opened and laid flat on a horizontal planar surface, "lateral" refers to the direction perpendicular to the longitudinal direction and parallel to the horizontal planar surface. With respect to feminine hygiene pads, the term "y-direction" is interchangeable with the term "longitudinal direction".
[0033] The "lateral axis" of an absorbent article such as a feminine hygiene pad or component thereof is a lateral line that lies in the xy plane and bisects the length of the pad or component thereof when the pad or component thereof is laid flat on a horizontal surface. The lateral axis is perpendicular to the longitudinal axis.
[0034] "Longitudinal" - with respect to an absorbent article such as a feminine hygiene pad or a component thereof, refers to the direction perpendicular to the lateral direction. The "length" dimension of any component or feature of the article is measured along the longitudinal direction from its forward extent to its rearward extent. When an article such as a feminine hygiene pad or a component thereof is laid flat on a horizontal surface, the "longitudinal" direction is perpendicular to the lateral direction relative to the pad when it is worn, as defined above. With respect to feminine hygiene pads, the term "y-direction" is interchangeable with the term "longitudinal direction".
[0035] The "longitudinal axis" of a feminine hygiene pad or component thereof is a longitudinal line that lies in the xy plane and bisects the width of the pad or component thereof when the pad is laid flat on a horizontal surface. The longitudinal axis is perpendicular to the lateral axis.
[0036] As used herein, the term "rayon" is generally used to include any fiber spun from regenerated cellulose, including but not limited to viscose, lyocell, and the like.
[0037] With respect to absorbent articles such as feminine hygiene pads or components thereof, the "xy plane" refers to any horizontal plane occupied by the horizontal surface or any layer of the article or component when lying flat on a horizontal surface. With respect to the manufacture or processing of web materials, the term "xy plane" refers to the plane substantially occupied by the major surfaces of the web material.
[0038] With respect to the manufacture or processing of web materials, the term "x-direction" is interchangeable with the term "cross direction."
[0039] With respect to the manufacture or processing of web materials, the term "y-direction" is interchangeable with the term "machine direction."
[0040] With respect to absorbent articles (such as feminine hygiene pads or components thereof), the "z-direction" is the direction perpendicular / orthogonal to the xy plane when laid flat on a horizontal surface. With respect to the manufacture or processing of web materials, the term "z-direction" refers to the direction orthogonal to the xy plane substantially occupied by a major surface of the web material.
[0041] The terms "top", "bottom", "upper", "lower", "above", "below", "below", "upper adjacent", "lower adjacent" and similar terms related to relative vertical positioning, when used herein to refer to layers, components or other features of an absorbent article (such as a feminine hygiene pad), are relative to the z-direction and are to be interpreted relative to the pad as it would appear when laid flat on a horizontal surface, with the wearer-facing surface of the pad oriented upward and the outward-facing surface oriented downward.
[0042] With respect to absorbent articles such as feminine hygiene pads, or components or structures thereof, "wearer-facing" is a relative positional term that refers to a feature of a component or structure that is closer to the wearer when in use than another feature of the component or structure. For example, a topsheet has a wearer-facing surface that is closer to the wearer than an opposite, outwardly facing surface of the topsheet.
[0043] With respect to absorbent articles such as feminine hygiene pads, or components or structures thereof, "outwardly facing" is a relative positional term referring to a feature of a component or structure that is further away from the wearer when in use than another feature of the component or structure. For example, a topsheet has an outwardly facing surface that is further away from the wearer than an opposite, wearer-facing surface of the topsheet.
[0044] As used herein, with respect to absorbent articles such as feminine hygiene pads or components thereof, "machine direction" or "MD" refers to the direction parallel to the flow of the article or component through processing / manufacturing equipment.
[0045] As used herein, with respect to absorbent articles such as feminine hygiene pads or components thereof, "cross direction" or "CD" refers to the direction perpendicular / orthogonal to the machine direction.
[0046] When used to characterize the amount of weight, volume, surface area, etc. of an absorbent article or part thereof that is composed of a composition, material, feature, etc., "mainly" and its forms mean that the majority of such weight, volume, surface area, etc. of the absorbent article or part thereof is composed of the composition, material, feature, etc.
[0047] General – Absorbent products; Feminine hygiene pads
[0048] See also Figure 1A, as contemplated herein, absorbent articles, such as feminine hygiene pads 10, will include a wearer-facing surface and an opposite outwardly facing surface. A liquid-permeable top sheet 20 may form at least a portion of the wearer-facing surface, and a liquid-impermeable back sheet may form at least a portion of the outwardly facing surface. The absorbent core includes an absorbent structure 40 disposed between the top sheet and the back sheet, and a fluid management layer 30 may be included and disposed between the absorbent structure 40 and the top sheet 20. (The fluid management layer as described herein is sometimes referred to in the art as a "collection / distribution layer," "distribution layer," or "secondary top sheet," and its purpose is to dissipate the energy from the fluid surge to a desired degree, provide a temporary volume of space for the discharged fluid to occupy during the time required for the absorbent structure of the underlying layer to receive and absorb the fluid, and distribute the fluid through the absorbent structure to maximize its effective utilization). Non-limiting examples of absorbent articles sharing these features include feminine hygiene pads (also known as "sanitary napkins," "menstrual pads," etc.), disposable incontinence pads, disposable incontinence underwear, disposable infant diapers, and disposable infant / child training pants.
[0049] The top sheet 20 and the back sheet 50 may be joined together to form and define the outer perimeter of the pad 10. The absorbent structure 40 and the fluid management layer 30 will each be sized to have an outer perimeter disposed laterally and longitudinally inwardly of the outer perimeter. The sizes and shapes of the absorbent structure 40 and the fluid management layer 30 in the xy direction may be substantially similar or identical to each other, or they may have correspondingly different xy sizes and / or shapes. One or both may be manufactured to have a shape such as Figure 1A The rectangular shape suggested in , or one or both may be manufactured to have any other suitable shape, such as an oval, a stadium shape, a rounded rectangular shape, an hourglass shape, a peanut shape, etc. Shapes with concave profiles along the longitudinal edges may provide enhanced comfort and / or conformity to the wearer's body in some examples.
[0050] The top sheet 20 may be joined to the back sheet 50 by any suitable attachment mechanism. The top sheet 20 and the back sheet 50 may be directly joined to each other in the periphery of the article, and may be indirectly joined together by directly joining them to the absorbent structure 40, the fluid management layer 30, and / or additional layers disposed between the top sheet 20 and the back sheet 50. This indirect or direct joining may be achieved by any suitable attachment mechanism known in the art. Non-limiting examples of attachment mechanisms may include, for example, melt bonding, ultrasonic bonding, pressure bonding, adhesive bonding, or any suitable combination thereof.
[0051] Top sheet
[0052] General Description
[0053] It is usually desired that the top sheet 20 is compliant, soft in feel, and non-irritating to the wearer's skin. Suitable top sheet materials include liquid-permeable materials that are oriented toward the wearer's body and contact the wearer's body, allowing body discharges to see through rapidly, and not allowing fluid to flow back on the wearer's skin through the top sheet. Although the top sheet can allow fluid to pass through and transfer rapidly, the lotion composition can also be made to transfer or migrate to the surface facing the wearer's skin therefrom. The top sheet can be formed by nonwoven material or comprise nonwoven material.
[0054] The nonwoven fibrous top sheet 20 can be produced by any known process for making nonwoven fibrous webs, non-limiting examples of which include spunbonding, carding, wet-laid, air-laid, meltblown, needle-punched, mechanical entanglement, thermo-mechanical entanglement, and hydroentanglement.
[0055] The nonwoven material suitable for use as top sheet can include a fiber layer or can be a laminate of multiple nonwoven layers, and the laminate can include the same or different compositions (e.g., spunbond-meltblown laminate). In a specific example, the top sheet is a carded air-bonded nonwoven.
[0056] The topsheet contemplated herein does not include any major portion of the topsheet xy surface area occupied by the film. Some currently known topsheets for feminine hygiene pads include an apertured film, such as a hydroformed film or a vacuum formed film, alone or in combination with an adjacently disposed nonwoven web material. The film can help prevent liquid from resurfacing and contacting the wearer. However, the inventors have found that a topsheet having the features described herein, particularly a topsheet in combination with a fluid management layer described herein, can effectively prevent back-seepage to a comparable degree or better than a pad having a topsheet having a film that includes a major portion of the topsheet xy surface area. Without being bound by theory, it is believed that careful selection of the fiber type and the linear density of the fiber type for each layer in the layering in the fluid management layer can result in a desired combination of appropriately low liquid acquisition time and low back-seepage, overcoming the typical compromises in these conflicting goals associated with existing nonwoven topsheets. The improved performance is evident from the new combination of a unique nonwoven topsheet with the fluid management layer disclosed herein.
[0057] Basis Weight
[0058] In some examples, the nonwoven top sheet material as envisioned herein can be manufactured to have a basis weight of about 15gsm to 80gsm, more preferably about 20gsm to 60gsm or most preferably about 20gsm to 40gsm, specifically listing all values in these ranges and any scope established thus. In a specific example, the top sheet nonwoven can be manufactured to a basis weight of about 18gsm to 40gsm, more preferably about 20gsm to 30gsm, even more preferably about 22gsm to 26gsm, specifically listing all values in these ranges and any scope established thus. The scope of ideal basis weight is subject to the needs of the required web tensile strength level for processing and the substantial preference influence of the consumer to the opacity level and thickness, sensation and outward appearance at the lower limit of the scope. The scope of ideal basis weight is subject to the influence of the needs and material cost problem of suitable rapid fluid acquisition and fluid passing through the top sheet at the upper limit of the scope.
[0059] Fiber composition
[0060] Non-limiting examples of woven and nonwoven materials suitable for use as topsheets include fibrous materials made from natural fibers (e.g., cotton, including 100% organic cotton), modified natural fibers, semi-synthetic fibers (e.g., fibers spun from regenerated cellulose), synthetic fibers (e.g., fibers spun from polymer resins), or combinations thereof. Synthetic fibers may include fibers spun from a single polymer or a blend of polymers.
[0061] However, in some examples, it may be desirable that the nonwoven web of the topsheet include less than 10%, more preferably less than 5%, and even more preferably less than 1% by weight of cotton fibers, other plant fibers, rayon fibers, or any combination of monocomponent fibers comprising polyester or polyamide. Such fibers are generally hydrophilic in nature, and thus may tend to cause the topsheet to retain fluid rather than allowing it to pass along to the absorbent assembly below. For the same reason, such fibers may tend to cause the topsheet to be susceptible to rewetting.
[0062] The synthetic fibers may include monocomponent fibers, bicomponent fibers, or multicomponent fibers. (As used herein, bicomponent fibers or multicomponent fibers are fibers having a cross-section divided into clearly identifiable component portions, each of which is formed from a single polymer or a single homogeneous polymer blend, as distinct from the other portion. Such fibers and methods for making them are known in the art. Examples of bicomponent fiber configurations having a substantially circular cross-section include a side-by-side or "fan-shaped" configuration, an eccentric sheath-core configuration, and a concentric sheath-core configuration.
[0063] The nonwoven top sheet contemplated herein may include fibers having countless combinations of constituent chemical substances. For example, the fiber may be spun from thermoplastic polymer materials such as polyethylene (PE) and / or polyethylene terephthalate (PET). The fiber may be spun in the form of a bicomponent fiber. In some examples, the bicomponent fiber may have a core component of a first polymer (e.g., PET) and a combination of another polymer as a sheath component, in a sheath-core bicomponent configuration. In a more specific example, PE may be combined with a PET core component to form a sheath component. The fiber comprising the PET component may be selected to help provide a main body and resilience and the resulting cushion feel to the nonwoven web. In addition, the fiber comprising the PET component with resilience helps the web to maintain the area and size of the hole (if included) formed therein.
[0064] Other polymer materials may be included. For example, fibers spun from polypropylene, polyethylene, copolyethylene terephthalate, copolypropylene and other thermoplastic resins may be included. It may be desirable to have a polymer with a lower melting temperature to form the sheath component, including a sheath-core bicomponent fiber. In addition, without wishing to be bound by theory, it is believed that using polyethylene terephthalate as a core component can help impart resilience to the fibers, and therefore to the top sheet.
[0065] Compared with other potentially useful thermoplastic polymers, polyethylene as a polymer component that can be spun into fibers has a relatively low melting temperature and exhibits a relatively smooth / silky surface feel. PET has a relatively high melting temperature and exhibits relatively large rigidity and resilience. Therefore, in some examples, it is desirable to have a top sheet nonwoven fiber with a skin-core bicomponent configuration, wherein the skin component is mainly polyethylene and the core component is mainly PET. Polyethylene can be used to impart a silky feel to the fiber and thus to the top sheet, and can be used to cause the skin of adjacent / contacting fibers to melt and fuse at a lower melting temperature of polyethylene via heat treatment to achieve inter-fiber bonding, while PET can be used to impart resilience and does not melt at a lower temperature of molten PE during heat treatment. The inventors have found that a suitable weight ratio in such PE / PET skin-core bicomponent fibers can be from about 40:60 to about 60:40.
[0066] Surface treatment (hydrophilicity / hydrophobicity)
[0067] Depending on the chemical composition of the fiber, the surface of the fiber will be inherently hydrophilic or hydrophobic to varying degrees. For example, the surface of fibers spun or otherwise formed by some types of polymers (such as polyethylene and polypropylene) will be inherently hydrophobic. In contrast, the surface of other types of fibers (such as rayon fibers) will be inherently hydrophilic. The surface of natural fibers can be inherently hydrophilic or hydrophobic, but this may depend on the treatment that the fiber has undergone. For example, harvested cotton fibers carry a coating of natural oils and / or waxes, and therefore their surfaces are hydrophobic. However, after they have undergone a process including scrubbing and bleaching, the oil and / or wax will be stripped, making the fiber surface hydrophilic.
[0068] Manufacturers and / or suppliers of spun synthetic staple fibers currently apply coatings in the form of surface finishes or processing aids to the fibers for the purpose of providing lubricity during, for example, the carding process. These surface finishes or processing aids can be formulated to be hydrophobic or hydrophilic and are substantially durable for purposes herein because they will not dissolve in aqueous fluids over the normal wearing duration of the absorbent article. Therefore, manufacturers or suppliers of spun synthetic staple fibers can provide fibers with a hydrophobic or hydrophilic surface finish, and currently, several manufacturers in the nonwovens industry do so.
[0069] It is noteworthy that spun synthetic staple fibers may have a surface that is inherently hydrophobic or hydrophilic, or have a surface finish that renders its surface hydrophilic or hydrophobic at the option of the purchaser, and it may be desirable to select fibers having a surface that is hydrophilic ("hydrophilic fibers") or hydrophobic ("hydrophobic fibers"), or a blend of these two types of fibers.
[0070] In some examples, it may be preferred that the fiber components of the top sheet are mainly, substantially or completely hydrophobic by weight, or are rendered hydrophobic via the fiber surface finish. A top sheet formed from a nonwoven web having mainly hydrophobic fiber components will resist rewetting. On the other hand, if the size of the pores or interfiber spaces within the fiber structure of such a nonwoven web is not large enough, the top sheet may prevent fluid from passing through the wearer-facing surface to the absorbent core component of the article below it, i.e., fluid will not be easily / quickly collected unless other features as described herein are included in combination.
[0071] In other examples, part, most (by surface area) or all of the fibers that make up the cross-section of the web material from which the top sheet is formed may be a blend of both hydrophobic and hydrophilic fibers. In such examples, the hydrophilic fibers may be used to help wick fluid downward from the wearer-facing surface of the top sheet to the absorbent core component below, while the hydrophobic fibers may be used to help the top sheet prevent re-seepage. The inventors have found that a successful balance can be achieved for such examples.
[0072] Therefore, in some examples, the top sheet nonwoven fabric may include a mixture of hydrophobic fibers and hydrophilic fibers.For example, the nonwoven fabric may include at least about 40% by weight, more preferably at least about 50% by weight or most preferably at least about 60% by weight of the hydrophilic fibers by the weight of the fiber, specifically including all values in these ranges and any scope established thereby.In more specific examples, the nonwoven top sheet may include about 40% by weight to 70% by weight, more preferably about 45% by weight to 68% by weight or most preferably from about 50% by weight to 65% by weight of the hydrophilic fibers, specifically listing all values in these ranges and any scope established thereby.The top sheet nonwoven fabric may include a blend of hydrophilic fibers and hydrophobic fibers, and the weight ratio of hydrophilic fibers to hydrophobic fibers is 30:70 to 70:30, more preferably 35:65 to 65:35 and even more preferably 40:60 to 60:40.As mentioned above, the hydrophilicity of the hydrophilic fibers may be affected by applying a surface treatment composition.
[0073] Without wishing to be bound by theory, it is believed that where a majority of the fibers are hydrophilic, fluid acquisition rates can be improved by combining with the other features described herein without unduly affecting rewet in an unfavorable or unacceptably unfavorable manner. Where less rewet is the goal, the opposite may be true. In this case, a higher weight fraction of hydrophobic fibers may be desirable.
[0074] Line density
[0075] Fibers are typically manufactured, selected, and purchased by linear density specifications, such as expressed as denier or decitex. For fibers of a given polymer composition, linear density is related to fiber size / diameter.
[0076] In some examples, the fibers constituting the topsheet may be selected to have an average linear density of about 1.0 denier to 3.0 denier, more preferably about 1.5 denier to 2.5 denier, and even more preferably about 1.8 denier to 2.2 denier, and all combinations of subranges within these ranges are contemplated herein. Fibers having linear densities varying within the above ranges may also be selected and included.
[0077] In other examples, the fibers constituting the topsheet may be selected to have an average linear density of about 3.0 denier to 5.0 denier, more preferably about 3.5 denier to 4.5 denier, and even more preferably about 3.8 denier to 4.2 denier, and all combinations of subranges within these ranges are contemplated herein. It is understood that the fibers selected within these ranges in combination with the other features disclosed herein may be considered to constitute a topsheet material of acceptable softness to many consumers, as well as providing other advantages over smaller fibers.
[0078] One advantage is that relatively large fibers generally provide a nonwoven web material having relatively large inter-fiber / intra-web spaces or interstices therein, thereby providing larger channels through which fluid can travel more quickly through the nonwoven from the wearer-facing side to the outwardly-facing side (and thus to the absorbent component below the topsheet). Additionally, although relatively large fibers of a given composition are stiffer than smaller fibers of similar composition, which may compromise the surface "softness" attribute to some extent, the greater fiber stiffness may also enhance the perception of greater resiliency, springiness, or cushioned feel of the topsheet nonwoven.
[0079] Short fiber length
[0080] Suitable fibers may be staple fibers having a length in the following ranges: at least about 30 mm, 40 mm, or 50 mm, up to about 55 mm, or about 30 mm to about 55 mm, or about 35 mm to 52 mm, with increments of 1 mm listed for the ranges. In a specific example, the staple fibers may have a length of about 38 mm.
[0081] hole
[0082] The inventors have discovered that in a topsheet nonwoven formed of fibers of relatively small size / linear density and / or fibers that are primarily, substantially or completely hydrophobic, the acquisition speed can be increased appreciably by forming a hole pattern through the web of fibers. In examples where the fibers have relatively large size / linear density, as also contemplated herein, forming and including a hole pattern may not be considered necessary in some cases, but may be helpful in other cases, in order to provide more surface-to-surface channels of relatively large size, thereby allowing discharged body exudates to pass downwardly through the topsheet more quickly.
[0083] Generally speaking, the preferred hole will have a size substantially larger than the average hole / gap size in the nonwoven web. The hole can be formed by any suitable, known pinning process. The process may include using pins arranged in any desired pattern and extending radially from a cylindrical roller with a pin, which is connected to a matching cylindrical roller with a pin receiving hole in its surface. One or two rollers may be heated to a temperature sufficient to cause the nonwoven web fibers to soften and plastically deform without melting them. The nonwoven web material passes through the roller gap between these rollers and can affect the fiber in the nonwoven structure along the x and y directions, and the persistent or substantially permanent displacement of the position in the z direction, thereby producing a hole through the web, when the web is manipulated in a later / downstream process such as winding, unfolding and absorbent article manufacturing process, the hole substantially maintains their size and shape. Preferably, the hole forming process is after the web is bonded via heat treatment, to provide a more reliable formation of holes with more stable size and shape.
[0084] An example of a cross-section of a topsheet nonwoven web material 500 having a pattern of holes 501 therethrough is depicted in FIG. Figure 4 An enlarged image of an example of a hole through a nonwoven web material is depicted in FIG. Figure 5 The pores are distinguishable from randomly disposed inter-fiber / inter-web spaces or voids through the nonwoven web material because the pores are produced by readily discernible displacement of the fibers in the xy direction, thereby producing a concentrated group of displaced fibers defining a perimeter of a z-direction opening through the nonwoven web that is relatively larger than the randomly disposed pores or voids between and in the fibers constituting the material. The pores through the web may be produced by methods and equipment configured to impart an average xy-sized pore area within the range of: 0.5 mm 2 Up to 2.5mm 2 , preferably about 0.6 mm 2 Up to 1.2mm 2 , and all combinations of sub-ranges within these ranges are contemplated herein. Herein, the xy dimension area of the aperture is defined by the visually discernible inside edge of the concentration of displaced fibers 503 around the perimeter of the aperture. Individual fibers that may have left the main structure and / or the concentration of displaced fibers around the perimeter and passed through the deviation into or through the main opening area of the aperture (by way of example, Figure 5 5 (not shown in the figure), are not considered to be subtracted from the hole area for purposes herein. Further, without wishing to be bound by theory, it is believed that where the shape of the hole is too long or too narrow, the fluid acquisition rate may be negatively affected. Thus, it may be desirable for the holes to have a finite maximum average xy-direction aspect ratio (largest dimension: smallest dimension in the xy-direction). Thus, it may be desirable for the holes to have an average aspect ratio of about 2.5:1 to 1:2.5, more preferably about 1.5:1 to 1:1.5, or most preferably about 1:1, and all combinations of sub-ranges within these ranges are contemplated herein. Further, for the purposes of maintaining the structural integrity of the fiber web and the shape integrity of the holes, it is preferred that at least in the region of interest 25 ("ROI," defined below; see Figure 1A The xy plane shape of most or all of the apertures in the top sheet (if not most or all of the top sheet) is circular (e.g., circular, oval, ovoid, elliptical, stadium-shaped, etc.) without sharp corners. Therefore, it is desirable that the pinned roller used to create the apertures have pins without sharp corners when viewed in a radially inward direction toward the axis of the roller.
[0085] The amount of pore area for all pores in the portion of interest of the topsheet is summed up to the xy plane area of the openings in the topsheet nonwoven ("open area"). The inventors have determined the desired open area, in conjunction with the desired average pore size, in order to effectively mitigate potential barriers to fluid acquisition that may be caused by a composition of finer denier fibers and / or fibers that are primarily hydrophobic. Thus, it may be expected that the pores (if included) collectively provide an open area of 6% to 25%, more preferably 8% to 18%, and even more preferably 10% to 15%, and all combinations of sub-ranges within these ranges are contemplated herein. Preferably, such amount of open area is present substantially throughout the portion of the topsheet covering the fluid management layer and / or absorbent structure, or at least as defined below (and see Figure 1A ) in a region of interest 25 ("ROI"). The lower end of these ranges is limited by the need for efficacy / performance; the apertures should provide at least a minimum amount of open area in order to be effective as may be included for the purposes described herein. The upper end of these ranges is limited by the need for consumer acceptance; if the open area is too large, the consumer may perceive the topsheet as fragile or of poor quality; and further, the topsheet becomes less effective in retaining fluids beneath it and in masking stains caused by absorbent fluids present in the absorbent component beneath the topsheet.
[0086] See also Figure 1A For purposes contemplated herein, the region of interest 25 ("ROI") is a rectangular cross-section of the topsheet that is 60.0 mm long in the longitudinal direction and 30.0 mm wide in the lateral direction and is centered in the xy plane at the longitudinal and lateral centers of the fluid management layer. The open area percentage fraction of ROI 25 is the fraction of its xy area that is open in the z direction by the presence of apertures 501 therein. Expressed differently, the open area percentage fraction within the ROI is the total xy area of apertures within the ROI divided by 1,800 mm 2 Multiply by 100%.
[0087] In some examples, the open area percentage fraction in the ROI may be obtained from instructions given or provided by the manufacturer of the top sheet nonwoven web material. Where this is not available, it may be measured via any applicable suitable measurement technique in a manner consistent with the above description of the xy dimension area of the aperture area and the description of "open area", which may include but is not limited to the "aperture open area measurement method" described below.
[0088] Bonding
[0089] Generally speaking, it is desirable that the fibers forming the topsheet nonwoven are bonded after the carding / fiber placement process to impart the fabric-like structure and tensile strength (in both MD and CD) required for the web to substantially maintain its structure in the downstream / later process, and to be in the form of a topsheet during use by the user / wearer. As an alternative to other bonding methods such as mechanical compression point bonding (with or without applying thermal energy), adhesive bonding, etc., it has been found that bonding via air through heating is effective for producing fiber-to-fiber bonding and imparting structural integrity to the web, while maintaining inter-fiber pore / void size and thickness, and imparting resilience to the nonwoven. In an example of a suitable method, air heated to a selected heating temperature is blown and / or drawn (via vacuum) through the carded web as the web is conveyed longitudinally on a conveyor belt through an oven or heating chamber. When the operating parameters including the temperature and speed of the heated air and the exposure time are appropriately adjusted, a plurality of randomly distributed fiber-to-fiber bonds can be generated within the web, which impart structural integrity to the web. When the constituent fibers are, for example, sheath-core bicomponent fibers, where the sheath component is a polymer having a melting temperature lower than that of the core component, the process can be configured so that a melt bond is formed between the sheaths of adjacent contacting fibers without complete melting and loss of the sheath structure, while the core remains in place, unmelted. In such a process, the bond can be formed without applying compression, and therefore, without an associated loss of web thickness and reduction in the size of the inter-fiber pores / voids.
[0090] Anti-stick agent applied
[0091] Absorbent articles may include an anti-adherent agent applied to at least a portion of the wearer-facing surface of the top sheet, wherein the anti-adherent agent includes a polypropylene glycol material. It is believed that the anti-adherent agent applied as described herein plays the following function: including reducing the adhesion of menstrual fluid to the user / wearer's skin, and promoting menstrual fluid to migrate downward from the wearer-facing surface of the top sheet through the fluid management and / or absorbent structure layer below. Providing these functions can enhance the user / wearer's sense of cleanliness to her skin and top sheet, especially after repeatedly discharging menstrual fluid. Examples of suitable anti-adherent agents and / or surfactants that can be used therein are disclosed in US2009 / 0221978 (wherein the composition is called "lotion") and US 8,178,748.
[0092] The anti-adherent may include a polypropylene glycol ("PPG") material. In some examples, the anti-adherent may consist essentially of a polypropylene glycol material (preferably a polypropylene glycol homopolymer such as polypropylene glycol) and optionally a carrier. In other examples, the anti-adherent may include a polypropylene glycol material selected from the group consisting of: a polypropylene glycol copolymer, a polypropylene glycol surfactant, and mixtures thereof. The anti-adherent including the polypropylene glycol material may be used to help reduce the adhesion of menstrual fluid to the top sheet, and the transfer of the anti-adherent to the user / wearer upon contact, reducing the adhesion of the fluid to her skin, thereby reducing staining on the top sheet and reducing soiling of the skin. The anti-adherent may also help improve continuous fluid acquisition of the absorbent article.
[0093] The anti-adherent can be applied to the wearer-facing surface of the top sheet 20 in any known manner and in any known pattern. For example, the anti-adherent can be applied in a pattern of strips or bands that are generally parallel, longitudinally, or laterally. In order to avoid compressing or displacing the position of any part of the top sheet nonwoven or any three-dimensional features thereof, it is desirable to apply the anti-adherent via spraying. The application of substantially uniform spraying can be preferred.
[0094] The amount of the anti-adherent agent applied can vary, and can be adjusted for specific needs. For example, while not being bound by theory, it is believed that the anti-adherent agent can be applied at least about 0.1gsm, 0.5gsm, 1gsm, 2gsm, 3gsm, 4gsm, 5gsm, 10gsm, at most about 15gsm or at most about 12gsm or at most about 10gsm effective level. It is believed that effect will not be further enhanced when being higher than these upper limits, therefore applying with the basis weight exceeding these upper limits may unnecessarily use (waste) anti-adherent agent. Anti-adherent agent can be applied (for example, from about 0.1gsm to about 15gsm) in any sub-range limited by any of the above-mentioned levels. These levels refer to the area of the actual top sheet surface to which anti-adherent agent is applied. It is preferred that the major part, substantially all or all surface areas of the top sheet covering fluid management layer and / or absorbent cores have the anti-adherent agent applied. This is because, as is believed, the anti-sticking agent can enhance the ability of the topsheet to resist backwet.
[0095] The anti-adhesive agents contemplated herein provide significant advantages over other anti-adhesive agents (including non-PPG derived surfactants and other surface modifiers). These advantages can be considered to be particularly useful for feminine sanitary pads. Without wishing to be bound by theory, it is believed that the excellent fluid handling properties of the PPG materials identified herein are the result of the way in which the PPG materials act on the solid components of menstrual fluid, which is contrary to the surface energy treatment that acts on the water component of menstruation. Due to the presence of polar and dispersive components in menstrual fluid, which can inhibit the effectiveness of surface energy treatment, surface energy treatment may not be very effective. Because the PPG materials identified herein are generally not easily soluble in menstrual fluid, they can effectively coat the surface without dissolving in the fluid, which provides a hydration barrier whose electron-donating dipole repels negative dipole proteins, thereby making menstrual fluid less likely to adhere to the surface of the article or the skin of the wearer. Less adhesion of menstrual fluid to the wearer's skin and / or top sheet promotes better and faster movement of fluid through the top sheet, and has fewer, smaller and / or less visible stain patterns on the used product.
[0096] The PPG material identified herein can be applied as a component in an anti-adherent, or can be applied in pure form (i.e., the anti-adherent is composed of the PPG material). The PPG material (pure and / or as part of the anti-adherent) can be applied at different levels of quantity, depending on the desired fluid handling properties and the desired treatment of the wearer's skin. The PPG material can be applied to the outer surface of the top sheet in any pattern, such as a full coating, strips or bands (oriented in the MD or CD direction), droplets, spiral patterns, and other patterns. When present, the anti-adherent comprising the PPG material can also be disposed near the channel or embossed area.
[0097] The anti-adherents contemplated herein may include PPG materials. PPG materials suitable for the purposes contemplated herein include PPG homopolymer materials, PPG copolymer materials and PPG surfactant materials, and mixtures thereof. The anti-adherents may also include other optional ingredients. In one embodiment, the anti-adherents are essentially composed of or consist of PPG materials, preferably polypropylene glycol. In another embodiment, the anti-adherents include a PPG material selected from the group consisting of polypropylene glycol copolymers, polypropylene glycol surfactants and mixtures thereof.
[0098] The anti-adherents contemplated herein may include PPG materials at a level of about 0.1% to 100% by weight of the anti-adherent. In some examples, the anti-adherent may include less than about 10%, preferably about 0.5% to 8%, and more preferably about 1% to 5% of the PPG material by weight of the anti-adherent. In other examples, the anti-adherent may include at least about 50%, preferably about 75% to 100%, and more preferably about 90% to 100% of the PPG material by weight of the anti-adherent.
[0099] Suitable PPG homopolymer materials may include those corresponding to the following formula:
[0100]
[0101] - wherein R is hydrogen, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, benzyl, acetylcarbonyl, propionylcarbonyl, butyrylcarbonyl, isobutyrylcarbonyl, benzocarbonyl, fumarylcarbonyl, aminobenzocarbonyl, carboxymethylene, aminopropylidene, alkylated glucose, alkylated sucrose, alkylated cellulose, alkylated starch or phosphate; and wherein R is preferably hydrogen or methyl;
[0102] - wherein R1 is hydrogen, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, benzyl, acetylcarbonyl, propionylcarbonyl, butyrylcarbonyl, isobutyrylcarbonyl, benzocarbonyl, fumarylcarbonyl, aminobenzocarbonyl, carboxymethylene, aminopropylene, alkylated glucose, alkylated sucrose, alkylated cellulose, alkylated starch or phosphate; and wherein R1 is preferably hydrogen or methyl; and
[0103] - wherein n is 3 to 160, preferably 5 to 120, more preferably 10 to 100, and more preferably 20 to 80.
[0104] Optionally, the PPG homopolymer may include low levels of glycerol or butanediol as part of its monomer raw material. If included, the preferred ratio of glycerol or butanediol to propylene glycol may be 1:1000 to 1:2, most preferably 1:100 to 1:5. The PPG homopolymer may have, but is not necessarily limited to, CAS Nos. 25322-69-4, 25791-96-2, and 25231-21-4, with the latter being most preferred.
[0105] Non-limiting examples of suitable PPG homopolymer materials include: polypropylene glycol 4000, such as Pluriol P-4000 (BASF), Alkapol PPG-4000 (Alkaril Chemical), and Niax Polyol PPG 4025 (Union Carbide); polypropylene glycol 3500; polypropylene glycol 3000, such as Niax PPG 3025 (Union Carbide); polypropylene glycol 2000 such as Alkanol PPG-2000 (Alkaril Chemical) and Pluriol P-2000 (BASF), polypropylene glycol 1200 such as Alkapol PPG-1200 (Alkaril Chemical) and Glucam P-20 Humectant (Noveon); polypropylene glycol 1000 such as Niax PPG 1025 (Union Carbide); polypropylene glycol 600 such as Alkanol PPG-600 (Alkaril Chemical) and Glucam P-10 Humectant (Noveon); polypropylene glycol 400 such as Alkanol PPG-425 (Alkaril Chemical). Polypropylene glycol 4000 glyceryl ether such as Pluriol T-4000 (BASF); polypropylene glycol 2000 glyceryl ether, polypropylene glycol 2000 butylene glycol ether, polypropylene glycol 1500 glyceryl ether such as Pluriol T-1500 (BASF), polypropylene glycol 4000 with monomethyl ether, polypropylene glycol 2000 with dimethyl ether, polypropylene glycol 4000 with monobutyl ether, polypropylene glycol 2000 with monobutyl ether, polypropylene glycol 1200 with dibutyl ether, polypropylene glycol 4000 with bis(2-aminopropyl ether), PPG-10 methyl glucose ether and PPG-20 methyl glucose ether.
[0106] Suitable PPG homopolymer materials will generally have a number average molecular weight of about 400 to 10,000, preferably about 600 to 6,000, and more preferably about 1,200 to 4,800.
[0107] Suitable PPG copolymer materials include those in which polypropylene glycol segments are present as internal block components and / or as terminal components of the copolymer structure. The following formulas exemplify internal block components and terminal block components:
[0108]
[0109] wherein x is 2 to 120, preferably 2 to 80, and more preferably 3 to 60; y is 2 to 100, preferably 2 to 50, and more preferably 3 to 30; R2 is hydrogen, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, benzyl, acetylcarbonyl, propionylcarbonyl, butyrylcarbonyl, isobutyrylcarbonyl, benzocarbonyl, fumarylcarbonyl, aminobenzocarbonyl, carboxymethylene, aminopropylidene, alkylated glucose, alkylated sucrose, alkylated cellulose, alkylated starch or phosphate, and wherein R2 is preferably hydrogen, methyl, ethyl, isopropyl or isobutyl.
[0110] Suitable polymers for forming propoxylated copolymers with PPG for use in the anti-adherent agents of the present invention include homopolymers of alkyl methicone, phenyl methicone, dimethicone, alkyl trimethicone, phenyl trimethicone, polyols, polyethers (e.g., polyoxymethylene, polyoxyethylene and polyoxypropylene), polyimines, polyamides, polyacrylates, polyesters, and copolymers containing one or more of these polymerized units. Non-limiting examples of suitable polymers include polydimethylsiloxane, polyethyleneimine, polyacrylic acid, poly(ethylene-co-acrylic acid), polymethacrylic acid, poly(ethylene-co-methacrylic acid), poly(vinyl acetate), polyvinylpyrrolidone, poly(ethylene-co-vinyl acetate), poly(butylene glycol), poly(neopentyl glycol), poly(ethylene adipate), poly(butylene adipate), poly(ethylene glutamate), poly(butylene glutamate), poly(ethylene sebacate), poly(butylene sebacate), poly(ethylene succinate), poly(butylene succinate), poly(ethylene terephthalate), poly(butylene terephthalate), polycaprolactone, and polyglycerol.
[0111] Non-limiting examples of suitable PPG copolymer materials include PPG-12 dimethicone, such as Sisoft 910 (Momentive); bis-PPG-15 dimethicone / IPDI copolymers such as Polyderm-PPI-SI-WI (Alzo); PPG / polycaprolactone block copolymers; PPG / polybutylene glycol / PEG triblock copolymers; polyethyleneimine / PPG copolymers and polyacrylic acid-g-PPG graft copolymers.
[0112] Another suitable PPG material includes a PPG surfactant material. The following formula represents a suitable PPG surfactant material, wherein the PPG segment constitutes part of the head functional group:
[0113]
[0114] wherein R3 is hydrogen, alkyl, alkylcarbonyl, alkyleneamine, alkyleneamide, alkylenephosphate, alkylenecarboxylic acid, alkylenesulfonate and alkylenequaternaryammonium with a maximum carbon number of less than or equal to 6; R4 is octyl, nonyl, decyl, isodecyl, lauryl, myristyl, cetyl, isohexadecyl, oleyl, stearyl, isostearyl, tallowoyl, linoleyl, jojoba oil, lanolin, behenyl, C24-C28 alkyl, C30-C45 alkyl, dinonylphenyl, dodecylbenzene or soybean; z is 1 to 100, preferably 2 to 30, and more preferably 3 to 25; and F is a functional group selected from the group consisting of an ether group (including an oxy group, a glyceryl group, glucose, sorbitan, sucrose, monoethanolamine or diethanolamine), an ester group (including an ester, a glyceride, a glucose ester, a sorbitan ester or a sucrose ester), an amine group, an amide group and a phosphate group.
[0115] The following formula represents a suitable PPG surfactant material, wherein the PPG segments constitute the interior block groups:
[0116]
[0117] wherein R5 is hexyl, 2-ethylhexyl, octyl, nonyl, decyl, isodecyl, lauryl, cocoyl, myristyl, cetyl, isohexadecyl, oleyl, stearyl, isostearyl, tallow, linoleyl, octylphenyl or nonylphenyl; r is 1 to 120, preferably 4 to 50, and more preferably 6 to 30; and G is an ether, ester, amine or amide bond.
[0118] Non-limiting examples of suitable PPG surfactant materials include PPG-30 cetyl ether, such as Hetoxol C30P (Global Seven); PPG-20 methyl glucose ether distearate such as Glucam P-20 distearate emollient (Noveon), PPG-20 methyl glucose ether acetate, PPG-20 sorbitan tristearate, PPG-20 methyl glucose ether distearate, PPG-20 distearate, PPG-15 stearyl ether such as Alamol-E (Croda-Uniqema) and Procetyl 15 (Croda), PPG-15 stearyl ether benzoate, PPG-15 isocetyl ether, PPG-15 stearate, PPG-15 dicocoate, PPG-12 dilaurate, PPG-11 stearyl ether such as Varonic APS (Evonik); PPG-10 cetyl ether such as Procetyl 10 (Croda); PPG-10 glyceryl stearate, PPG-10 sorbitan monostearate, PPG-10 hydrogenated castor oil, PPG-10 cetyl phosphate, PPG-10 tallow amine, PPG-10 oleamide, PPG-10 cetyl ether phosphate, PPG-10 dinonylphenol ester, PPG-9 laurate, PPG-8 dicaprylate, PPG-8 diethylhexanoate, PPG-7 lauryl ether, PPG-5 lanolin wax ether, PPG-5 sucrose cocoate, PPG-5 lanolin wax, PPG-4 jojoba alcohol ether, PPG-4 lauryl ether, PPG-3 myristyl ether such as Promyristyl PM-3 (Croda), PPG-3 myristyl ether propionate such as Crodamol PMP (Croda), PPG-3 benzyl ether myristate such as Crodamol STS (Croda), PPG-3 hydrogenated castor oil such as Hetester HCP (Alzo), PPG-3-hydroxyethyl soyamide, PPG-2 cocamide, PPG-2 lanolin alcohol ether and PPG-1 coconut fatty acid isopropanolamide such as Amizett IPC (Kawaken Fine Chemicals). A particularly preferred example of a suitable PPG material is PPG-15 stearyl ether, such as the product sold as CETIOL E by BASF Corporation (Florham Park, New Jersey, USA) and / or BASF SE (Ludwigshafen, Germany).
[0119] The anti-adherent agents contemplated herein may include a carrier at a total carrier concentration ranging from about 60% to 99.9%, preferably from about 70% to 99.5%, more preferably from about 80% to 99% by weight of the anti-adherent agent.
[0120] Suitable carriers herein may include oils or fats, such as natural oils or fats, or natural oil or fat derivatives, especially oils or fats of vegetable or animal origin. Non-limiting examples include avocado oil, apricot oil, almond oil, babassu oil, borage oil, borage seed oil, calendula oil, camellia oil, canola oil, carrot oil, cashew oil, castor oil, chamomile oil, cherry pit oil, chia seed oil, coconut oil, cod liver oil, corn oil, corn germ oil, cottonseed oil, eucalyptus oil, evening primrose oil, grape seed oil, hazelnut oil, jojoba oil, juniper oil, kernel oil, linseed oil, macadamia oil, meadowfoam seed oil, menhaden oil, mink oil, moringa oil, mortierella fuchsia oil, olive oil, palm oil, palm kernel oil, peanut oil, peach kernel oil, rapeseed oil, rose hip oil, safflower oil, sandalwood oil, sesame oil, soybean oil, sunflower oil, sunflower seed oil, sweet almond oil, tall oil, tea tree oil, turnip seed oil, walnut oil, wheat germ oil, zedoary turmeric oil, or hardened derivatives thereof. Hardened oils or fats from vegetable sources may include, for example, hardened castor oil, peanut oil, soybean oil, turnip oil, cottonseed oil, sunflower oil, palm oil, kernel oil, linseed oil, corn oil, olive oil, sesame oil, cocoa butter, shea butter, and coconut oil.
[0121] Other non-limiting examples of fats and oils may include: butter, C12-C18 acid triglycerides, camellia oil, caprylic / capric / lauric triglycerides, caprylic / capric / linoleic triglycerides, caprylic / capric / stearic triglycerides, caprylic / capric triglycerides, cocoa butter, C10-C18 triglycerides, egg oil, epoxidized soybean oil, triacetin hydroxystearate, triacetin ricinoleate, glycosphingolipids, human placenta Lipids, Hybrid Safflower Oil, Hybrid Sunflower Seed Oil, Hydrogenated Castor Oil, Hydrogenated Castor Oil Laurate, Hydrogenated Coconut Oil, Hydrogenated Cottonseed Oil, Hydrogenated C12-C18 Triglycerides, Hydrogenated Fish Oil, Hydrogenated Lard, Hydrogenated Menhaden Oil, Hydrogenated Mink Oil, Hydrogenated Deep Sea Fish Oil, Hydrogenated Palm Kernel Oil, Hydrogenated Palm Oil, Hydrogenated Peanut Oil, Hydrogenated Shark Liver Oil, Hydrogenated Soybean Oil, Hydrogenated Shea Butter, Hydrogenated Vegetable Oil, Lanolin and Lanolin Derivatives, Lanolin Alcohol, Porcine Oil, lauric / palmitic / oleic triglycerides, lesquerella oil, maleated soybean oil, white meadowfoam seed oil, neatsfoot oil, oleic / linoleic triglycerides, oleic / palmitic / lauric / myristic / linoleic triglycerides, stearic acid, olive shell oil, omental lipids, deep sea fish oil, golden dog oil, lard oil, lecithin, pistachio oil, placental lipids, rapeseed oil, rice bran oil, shark liver oil, shea butter, sphingolipids, shea butter, glyceryl triglycerides The present invention relates to the present invention to the present invention relates to the present invention. The present invention relates to the present invention ...
[0122] Other suitable carriers may include mono- or di-glycerides, such as those derived from saturated or unsaturated, linear or branched, substituted or unsubstituted fatty acids or fatty acid mixtures. Examples of mono- or di-glycerides include mono- or di-C12-24 fatty acid glycerides, specifically mono- or di-C16-20 fatty acid glycerides, such as monostearate, distearate.
[0123] The carrier may also include esters of straight chain C6-C22 fatty acids with branched chain alcohols.
[0124] Carriers contemplated herein may also include sterols, plant sterols, and sterol derivatives. Sterols and sterol derivatives useful in the anti-adherent agents of the present invention include, but are not limited to, β-sterols having a tail at position 17 and no polar groups, such as cholesterol, sitosterol, stigmasterol, and ergosterol, as well as C10-C30 cholesterol / lanosterol esters, cholecalciferol, cholesterol hydroxystearate, cholesterol isostearate, cholesterol stearate, 7-dehydrocholesterol, dihydrocholesterol, dihydrocholesterol octyldecanoate, dihydrolanosterol, dihydrolanosterol octyldecanoate, calciferol, tall oil sterol, soya sterol acetate, lanosterol, soya sterol, avocado sterol, "AVOCADIN" (trade name of Croda Ltd of Parsippany, NJ), sterol esters and similar compounds, and mixtures thereof. A commercially available example of a phytosterol is GENEROL 122N PRL refined soy sterol available from Cognis Corporation of Cincinnati, Ohio.
[0125] Absorbent core
[0126] Fluid Management Layer
[0127] The absorbent core may include a fluid management layer 30 .
[0128] The fluid management layer as contemplated herein may include a structured collection of carded integrated fibers. The fluid management layer increases the thickness of the absorbent article and is generally compressible and may be composed and constructed to be resilient, which may give the article a soft and / or "cushioned" feel. When constructing layer components for absorbent articles, there is generally a trade-off between resilience and softness. Softer (i.e., more compliant or flexible) materials may have a smaller tendency to recover their shape after deformation caused by the application of force in one or more directions. For elastic materials, the opposite may be true. Among the materials that are typically included as components of absorbent articles, elastic materials will recover their original size and / or shape after being deformed by the application of force. However, they may not feel "soft". In addition, many absorbent articles or their layer components may exhibit good resilience properties when dry; however, their resilience is significantly reduced when absorbing liquid. The absorbent articles contemplated herein exhibit good resilience properties under both dry and wet conditions.
[0129] In addition to the softness and resiliency benefits of the compositions and structures for the fluid management layers contemplated herein, stain size control and faster fluid acquisition can also be obtained. Stain size is important to the way absorbent articles are perceived by users. For feminine hygiene pads, when a stain visible on the pad after a duration of use / wear is relatively large in the xy direction, the user may perceive that the pad is close to failure based on the appearance of the stain and its proximity to the outer periphery of the pad. In contrast, smaller stains may have a reassuring effect on the user / wearer by creating a perception that the pad is not close to failure because the edges of the stain do not substantially reach the outer periphery of the pad longitudinally and / or laterally.
[0130] The fluid acquisition speed of the pad can be considered important to the user / wearer because fast acquisition can help the user / wearer feel dry and clean. When the pad takes a relatively long time to drain the drained fluid from the top sheet, it can cause the user to feel wet and feel unclean.
[0131] As described, the fluid management layer 30 as contemplated herein can be formed of a nonwoven material of integrated carded fibers. The fluid management layer contemplated herein can include one or more webs of carded fibers that are integrated with each other. In the case of only a single carded fiber web, the fibers of the single web can be integrated.
[0132] Countless variations in the combination of composition, manufacturing methods, and configurations of the fluid management layer 30 may be designed and manufactured. However, in many cases, it may be desirable for the fluid management layer to have sufficient pore volume to allow for rapid acquisition / uptake of expelled fluids.
[0133] Multiple carded webs may be included to form the fluid management layer, and may be different from each other. For example, one carded web may have a different fiber composition and / or blend thereof than one or more other webs. For example, assuming that the first carded web will be closest to the wearer-facing surface in the absorbent article, the fiber composition selection and manufacturing method of the first carded web may be configured so that the first web has a larger pore volume than the carded webs of one or more lower layers of the fluid management layer. A second or middle carded web of the lower layer may be included and similarly configured. In contrast, the third or bottommost carded web of the lower layer may be configured to draw liquid from the void spaces of the first carded web and the second carded web, and effectively distribute these liquid insults to / across the absorbent structure of the lower layer. In the case where the fiber composition of one of the carded webs forming the fluid management layer is different from the fiber composition of another carded web forming the fluid management layer (regardless of whether the fibers of the corresponding carded webs are integrated), the fluid management layer is considered to be a heterogeneous configuration herein. Alternatively, where the carded fiber webs comprising the fluid management layer all have the same fiber composition, the fluid management layer is considered herein to be of a homogeneous configuration.
[0134] After the fibers of the multiple carded fiber webs that constitute the fluid management system are integrated, the corresponding carded fiber webs cannot be easily separated. However, each carded fiber web of the fluid management system forms a layer within a layer. Even when its fibers are integrated into the upper adjacent / lower adjacent carded fiber web, each layer can maintain at least a portion of its unique characteristics along the z-direction. The fluid management system can draw fluid through and away from the top sheet via capillary action or wicking forces, the magnitude of which is sufficient to overcome any resistance of the fluid to pass through the top sheet, or the attraction that the top sheet may have for the fluid, which forces may exist as a result of the composition and / or configuration of the top sheet. The fluid management system can also effectively utilize the absorbent structure by providing a pore volume as a temporary reservoir and a distribution function to receive and contain fluid gushing, giving it time to receive and absorb fluid.
[0135] Absorbent articles that exhibit a soft cushion feel, good resilience and fluid handling properties are contemplated herein. In order to impart these properties, the thickness of the fluid management layer may be considered important. The typical thickness of the fiber web from a conventional spunlace line achieves a thickness factor (thickness / 10 gsm basis weight) of 0.03 mm / gsm to 0.12 mm / gsm. In contrast, the fluid management layer contemplated herein may exhibit a thickness factor of at least 0.13 mm / gsm, at least about 0.15 mm / gsm, or at least 0.2 mm / gsm, including any values within these ranges and any ranges established therefrom. The fluid management layer contemplated herein may have a thickness factor between 0.13 mm / gsm and about 0.3 mm / gsm, or from about 0.14 mm / gsm to about 0.25 mm / gsm, or from about 0.15 mm / gsm to about 0.22 mm / gsm, including any values within these ranges and any ranges established therefrom. The thickness data for prototype sample 1 and comparative sample 1 are provided below. The thickness and thickness factor of the fluid management layer of the present disclosure can be determined by the Thickness and Thickness Factor Test Method disclosed herein.It is important to note that the thickness factor as previously described is with respect to the thickness obtained using the thickness measurement method described below.
[0136] It has been found that in order to obtain an increase in thickness factor, a relatively simpler method can be used to produce a hydroentangled fiber web. Typically, the fiber web path passing through the hydroentanglement line is tortuous and subjects the fiber web to both compressive and tensile stresses. This tortuous fiber web path requires a water jet pressure of sufficient size to entangle the fibers to achieve the degree required to impart the fiber web with tensile strength sufficient to withstand subsequent treatment. These water jets are generally directed toward both surfaces of the fiber web. The water pressure required to cause sufficient entanglement to obtain the fiber web tensile strength is generally greater than the pressure required to impart the desired fluid treatment pore structure, and also causes a significant reduction in the thickness of the resulting hydroentangled / hydroentangled fiber web. In addition, typically, when the fiber web is routed around a variety of vacuum cylinders and rollers, the fiber web will be subject to significant z-direction compression and longitudinal tensile stresses, so that additional water jets can further entangle the layered constituent fibers. Further routing around a drying roller subjects the fiber web to additional z-direction compression and longitudinal tensile forces.
[0137] However, the inventors have discovered that by using a simplified web path that reduces radial compressive stress / excessive tensile forces and by properly selecting the fibers in the fluid management layer, the thickness of the web from which the fluid management layer is prepared can be maintained. The use of rollers and the number of water jets utilized can be reduced to simplify the process. Although the degree of fiber entanglement obtained is not as great as that provided by conventional methods, sufficient tensile strength can be imparted to the web through the selection of appropriate combinations of fibers (e.g., reinforcing fibers) as disclosed herein, which can be melt-bonded via a heat treatment process that causes melt bonding between the fibers where the fibers contact each other. The simplified path and appropriate fiber selection as described herein allow manufacturers to impart a heretofore unattained thickness factor to the fluid management layer web material.
[0138] It is noteworthy that the thickness factors for the samples of prototype fluid management layer materials manufactured as contemplated herein are derived from thickness data for prototype materials that have been wound into rolls for storage and transport. It is believed that thickness measurements of the same material could be made prior to such winding, which would result in an even higher thickness factor. However, such pre-winding thickness measurements may not necessarily represent the fluid management layer material actually used as a component of an absorbent article, which, after its manufacture, would typically be wound on a roll for storage and transport.
[0139] The fluid management layer contemplated herein may have a basis weight of up to 75 grams per square meter (gsm); or a basis weight of up to 70 gsm; or a basis weight of about 30 gsm to 75 gsm, or more preferably about 45 gsm to 70 gsm, or even more preferably about 50 gsm to about 65 gsm, including any values within these ranges and any ranges created therefrom.
[0140] Some types of absorbent articles may not require a fluid management layer having a basis weight as large as described above. For example, sanitary pads, which are generally not under the same requirements as catamenial pads and do not have the same level of absorbent capacity as catamenial pads, may be suitable for including a fluid management layer having a smaller basis weight than those described above. For example, the fluid management layer of a sanitary pad may be manufactured to have a basis weight of about 20 gsm to 70 gsm, or about 35 gsm to 65 gsm, or even about 40 gsm to 60 gsm, specifically including all values within these ranges and any ranges established thereby. In a specific example, the fluid management layer of the present disclosure may be manufactured to have a basis weight of about 45 gsm to 55 gsm. The basis weight of the fluid management layer may be determined by the basis weight measurement method described below.
[0141] The inventors have also discovered that the processing techniques used to create thickness in the fluid management layer can be used not only for hydroentangled materials in which the layers are heterogeneous, but also for hydroentangled materials in which the layers are homogeneous (e.g., each layer has the same fiber composition). In addition, the inventors have surprisingly discovered that hydroentangled materials made using this method together with appropriate fiber selection can also provide good resiliency and compression recovery, as well as improved fluid handling properties, over those produced via typical hydroentanglement processes.
[0142] As a result of the fiber integration, there is no need to include adhesives or binders within the constituent materials of the fluid management layer to add sufficient tensile strength and / or stability. Furthermore, the carded nonwovens of the fluid management layer contemplated herein can be made from a variety of suitable fiber types that produce desired performance characteristics. In examples contemplated herein, the fluid management layer can include a combination of reinforcing fibers, absorbent fibers, and elastic fibers.
[0143] Absorbent fibers may be included to impart to the fluid management layer the ability to absorb discharged fluids. Reinforcing fibers may be included to bond the fiber web together during heat treatment, thereby imparting greater rigidity and resilience to the fluid management layer. Elastic fibers may be included to impart to the fiber web an enhanced ability to recover its shape and thickness after a compressive force is applied thereto.
[0144] In order to enhance the stabilizing effect of integration, crimped carded fibers may be included. One or more of the absorbent fibers, reinforcing fibers, and elastic fibers may be crimped prior to integration. For example, when synthetic fibers are utilized, these fibers may be mechanically crimped via passing through a nip between a pair of rolls that engage each other. The absorbent fibers may be mechanically crimped and / or may be imparted with a chemically induced crimp.
[0145] The amount of absorbent fibers included can affect the ability of the fluid management layer to wick discharged fluid through and / or out of the topsheet. However, as the absorbent fibers absorb liquid, they tend to lose some of their structural integrity. This loss of structural integrity can reduce the resiliency of the fluid management layer and cause or exacerbate bunching and increased leakage. Thus, while, in principle, a relatively large portion of absorbent fibers in the fluid management layer can make it relatively more effective in quickly draining discharged fluid from the topsheet, this can also lead to other problems or disadvantages of the absorbent article, as described above.
[0146] In light of the potential problems associated with having too large a proportion of absorbent fibers in the fluid management layer, the inventors have discovered that, in order to balance the above advantages and disadvantages, an appropriate weight fraction of absorbent fibers in the fluid management layer may be about 10% to 60%, more preferably about 15% to 50%, and even more preferably about 20% to 40%, specifically including any values within these ranges and any ranges established therefrom. In a specific example, the fluid management layer may include about 20% to 30% by weight of absorbent fibers. The weight fractions of absorbent fibers, elastic fibers, and / or reinforcing fibers may be determined via the "Material Composition Analysis" method disclosed below.
[0147] To mitigate the reduction in structural integrity in the fluid management layer caused by wetting of the absorbent fibers, the fluid management layer may also be comprised of an appropriate weight fraction of elastic fibers, which enhances the ability of the fluid management layer to recover its shape and / or thickness after the application of compressive loads applied during use. Thus, the fluid management layer may be comprised to include elastic fibers in the range of about 15 wt % to 70 wt %, or about 20 wt % to 60 wt %, or about 25 wt % to 50 wt %, specifically reciting all values within these ranges and any ranges created therefrom. In a specific example, the fluid management layer may include about 30 wt % to 40 wt % elastic fibers.
[0148] Reinforcing fibers may be included to further enhance the resilience of the fluid management layer, and therefore to enhance the resilience of the absorbent article. After fiber blending, aggregation, and layup, the reinforcing fibers within the precursor fiber aggregate may be bonded to each other via heat treatment of the fluid management layer material. This bonding of the reinforcing fibers forms a supporting matrix that enhances the resilience and stiffness of the fluid management layer. Thus, the fluid management layer may be comprised of elastic fibers in the range of about 25% to 70% by weight, or about 30% to 60% by weight, or even about 40% to 55% by weight, specifically listing all values within these ranges and any ranges established therefrom. In a specific example, the fluid management layer may include about 40% to 50% by weight of reinforcing fibers.
[0149] Where thickness, resilience and a soft cushion feel are the goals, the weight fraction of reinforcing fibers in the fluid management layer may be greater than or substantially equal to the weight fraction of elastic fibers. The weight fraction of absorbent fibers may be less than the weight fraction of elastic fibers and / or reinforcing fibers. Generally speaking, a higher weight fraction of absorbent fibers is considered beneficial for quickly acquiring discharged fluid from the top sheet; however, where the absorbent fibers are disposed adjacent to the top sheet, it may be beneficial for the absorbent structure below the fluid management layer to draw fluid from the absorbent fibers. In the case where there is a relatively large weight fraction of absorbent fibers in the fluid management layer, a relatively large absorbent structure located below it may be required to drain fluid from the absorbent fibers in the fluid management layer. This generally results in greater material costs. Therefore, an appropriate balance of the weight ratio of absorbent fibers to reinforcing fibers may be selected to be about 1:7 to 2:1, or 1:4 to 1.5:1, or even 1:2 to 1:1, specifically listing all values within these ranges and any ranges established therefrom. Similarly, the weight ratio of absorbent fibers to elastic fibers may be selected to be about 1:7 to 3:1, or 1:2 to 2:1, or even 1:1.5 to 1:1.
[0150] Whether the fluid management layer is included in an adult incontinence product, a catamenial product, a liner, or other hygiene product, the fluid management layer is capable of acquiring and drawing fluid from the topsheet and wicking the fluid to a location beneath the topsheet so that the user / wearer does not feel the topsheet wet at a time after the fluid is discharged. To achieve this, the inventors have discovered that a relatively increased thickness of a fluid management layer manufactured as discussed herein can enhance fluid acquisition via a relatively increased void volume within the fluid management layer. A relatively greater thickness at a given basis weight equates to a relatively greater void volume and higher permeability. In addition, a relatively greater thickness of the fluid management layer can also increase the opacity level of the fluid management layer and thereby increase the fluid stain masking effect.
[0151] Careful selection of the fiber types that make up each of the layers in the fluid management system and selection of the linear density of the fibers (which is related to the fiber size) can meet the desired goals of suitably rapid acquisition and low rewet. The fiber types of the individual layers are discussed below.
[0152] For the purposes of this document, references to the "first" layer, "second layer", etc. below refer to the order in which the layers appear under the topsheet from top to bottom. The "first" layer will be on top of the fluid management layer, closest to the topsheet, and so on.
[0153] Suitable linear density values (expressed in decitex units or "dtex") for absorbent fibers used in the fluid management layer contemplated herein are as follows. In some examples, the average linear density of the absorbent fibers may be selected to be from about 1 dtex to 7 dtex, or from about 1.4 dtex to 6 dtex, or even from about 1.7 dtex to 5 dtex, with all values within these ranges and any ranges established therefrom being specifically listed. In a specific example, the included absorbent fibers may be selected to have an average linear density of from about 0.6 to 2.4 dtex, more preferably from about 0.9 to 2.1 dtex, even more preferably from about 1.1 to 1.9 dtex, and most preferably from about 1.3 to 1.7 dtex. (The average dtex of the absorbent fibers, reinforcing fibers, and elastic fibers may be determined via the "Fiber Decitex Method" disclosed herein if this information is unknown or cannot be obtained from the manufacturer or supplier).
[0154] The absorbent fibers of the fluid management layer may have any suitable cross-sectional shape (wherein the cross section extends along a plane perpendicular to the larger length dimension of the fiber when the fiber is straight). Some examples of suitable shapes may include trilobal, "H", "Y", "X", "T", circular or flat ribbon. In addition, the absorbent fibers may have a cross section that is solid, hollow or multi-hollow. Other examples of suitable multi-lobal absorbent fibers for use in the fluid management layer described herein are disclosed in US 6,333,108, US 5,634,914 and US 5,458,835. The trilobal fiber shape can improve wicking and improve opacity and stain hiding properties. Suitable trilobal rayon fibers are available from Kelheim Fibres GmbH (Kelheim, Germany) and are sold under the trade name GALAXY. Although each layer may include absorbent fibers of different shapes (much like described above), not all carding equipment may be suitable for handling such changes between two / more layers. In one specific example, the fluid management layer can include absorbent fibers having a round (circular) shape.
[0155] The absorbent fibers may include any suitable absorbent material. Some examples of absorbent fiber materials include cotton, cellulose (eg, wood) pulp, rayon, or combinations thereof. In one example, the fluid management layer 30 may include viscose fibers.
[0156] The short length of the absorbent fibers may be selected to be about 20 mm to 100 mm, or 30 mm to 50 mm, or even 35 mm to 45 mm, with all values within these ranges and any ranges created therefrom being specifically listed. Generally, wood pulp has a fiber length of about 4 mm to 6 mm, and pulp fibers are too short to be used in conventional carding machines. Therefore, if wood pulp is desired as a fiber in the fluid management layer, additional processing may be required to mix the pulp and add it to the carded fiber web. In some examples, the pulp may be air-laid between the carded fiber webs and the combination subsequently integrated. As another example, a tissue made from pulp may be utilized in combination with a carded fiber web, and the combination may subsequently be integrated.
[0157] As previously mentioned, in addition to absorbent fibers, the fluid management layer of the present disclosure may include reinforcing fibers. Reinforcing fibers may be included to help impart structural integrity to the fluid management layer. Reinforcing fibers may help increase the structural integrity of the fluid management layer in the longitudinal and / or transverse directions, which may facilitate web manipulation during handling of the fluid management layer for incorporation into a disposable absorbent article.
[0158] Some examples of suitable linear density values for reinforcing fibers may be as follows: the reinforcing fibers may be selected to be about 1.0 dtex to 6 dtex, or more preferably about 1.5 dtex to 5 dtex, or even more preferably about 2.0 dtex to 4 dtex, with all values within these ranges and any ranges established therefrom being specifically listed. In a specific example, the reinforcing fibers may be about 1.8 dtex to 2.6 dtex, or more preferably about 2.2 dtex.
[0159] Suitable examples of reinforcing fibers may include bicomponent fibers including polyethylene and polyethylene terephthalate components or polyethylene terephthalate and copolyethylene terephthalate components. The components of the bicomponent fibers may be arranged in a sheath-core arrangement, a side-by-side arrangement, a concentric sheath-core arrangement, an eccentric sheath-core arrangement, a trilobal arrangement, or other suitable arrangements. In a specific example, the reinforcing fibers may include bicomponent fibers having a polyethylene / polyethylene terephthalate component arranged in a concentric sheath-core structure, wherein the sheath component includes polyethylene.
[0160] Although other materials can be used in a bicomponent fiber having a sheath-core arrangement, the inventors have found that the stiffness of the polyethylene terephthalate included in the core component is useful for imparting resilience to the structure. At the same time, the polyethylene component of the reinforcing fibers having a relatively low melting temperature and included in the sheath component can be used to cause the fibers to bond to each other via a heat treatment, wherein a plurality of randomly arranged fiber-to-fiber bonds can be produced throughout the structure. This can increase the tensile strength of the fiber web in both the machine direction (MD) and the cross direction (CD). In addition, the bonding between the lower melting point components of the reinforcing fibers (e.g., polyethylene-PET sheath-core bicomponent fibers) creates a matrix structure that tends to limit fiber-to-fiber sliding, thereby increasing the resilience of the material.
[0161] One of the benefits provided by including reinforcing fibers is that the integrated nonwoven can be heat treated after the fiber entanglement process. As the weight fraction of reinforcing fibers constituting the fluid management layer or a layer thereof increases, more fiber-to-fiber bonding / connection points will be created. Too many bonding / connection points may result in the fluid management layer being too stiff for consumer acceptance and negatively impact the user / wearer's perception of comfort and / or softness. Therefore, when designing an absorbent article, selecting the weight fraction of reinforcing fibers included in the fluid management layer may be considered important.
[0162] During the thermal strengthening process, the selection of the heating temperature may be influenced in part by the composition of the reinforcing fibers, the design and operating parameters of the heating equipment, and the fiber web processing speed (i.e., the duration of exposure to the thermal environment). In order to impart uniform stiffness across the fluid management layer, the heating equipment and operating parameters should be set to provide uniform heating to the fluid management layer fiber web. Even small temperature variations can significantly affect the formation of fiber-to-fiber bonds between the reinforcing fibers and result in the tensile strength of the fluid management layer. One example of a suitable thermal strengthening method that may be utilized is air through heating, in which air heated to a selected heating temperature is blown and / or drawn (via a vacuum) through the fiber web in a direction generally orthogonal to a larger plane defined by the fiber web.
[0163] As described above, the fluid management layer of the present disclosure may include elastic fibers. Including elastic fibers can help the fluid management layer maintain its permeability and recovery of shape and size after compression. Fibers of any suitable size can be utilized. For example, the elastic fibers may have a linear density (which will be related to the size / diameter) in the following range: about 4 dtex to 15 dtex, or about 5 dtex to 12 dtex, or even about 6 dtex to 10 dtex, specifically listing all values within these ranges and any ranges established thereby. In one specific example, the fluid management layer may include elastic fibers having variable cross-sections, such as circular and hollow spirals, and / or may include elastic fibers having different dtexes. In yet another specific example, the elastic fibers of the present disclosure may have a dtex of about 10. The elastic fibers may be hollow.
[0164] The elastic fiber can be composed / spun of any suitable thermoplastic such as polypropylene (PP), polyethylene terephthalate (PET) or other suitable thermoplastic known in the art. Other suitable examples of elastic fiber components include polyester / coextruded polyester. Other suitable examples of elastic fibers may include bicomponent fibers, such as polyethylene / polypropylene, polyethylene / polyethylene terephthalate, polypropylene / polyethylene terephthalate. These bicomponent fibers can be constructed as a sheath and a core. The use and inclusion of bicomponent fibers can provide a cost-effective way to increase the basis weight of the material while also being able to optimize the pore size distribution. The short length of the elastic fiber can be selected to be about 20mm to 100mm, or about 30mm to 50mm, or even about 35mm to 45mm. The thermoplastic fiber can have any suitable structure or cross-sectional shape. For example, the thermoplastic fiber can be circular, or can have other shapes, such as spiral, fan-shaped elliptical, trilobal, fan-shaped ribbon, etc. In addition, the elastic fiber included can be solid, hollow or multi-hollow. The selected elastic fibers may be solid and circular in cross-sectional shape.
[0165] Optionally, the elastic fiber can be spiral pleated or flat pleated.The elastic fiber can have a curl value of about 4 to 12 curls per inch (cpi), or about 4 to 8 cpi, or about 5 to 7 cpi, or about 9 to 10 cpi.
[0166] Specific non-limiting examples of elastic fibers are available from Wellman International Ltd / Indorama Ventures (Mullagh, Kells Co. Meath, Republic of Ireland) under the trade names H1311 and T5974. Other examples of elastic fibers suitable for use in the carded staple nonwovens detailed herein are disclosed in US 7,767,598.
[0167] The reinforcing fibers and elastic fibers should be carefully selected. For example, although the compositional chemistry of the reinforcing fibers and elastic fibers or their components may be similar, it may be desirable that the composition of the elastic fibers should be selected so that their melting temperature is higher than the melting temperature of the composition of the reinforcing fibers. Otherwise, during heat treatment, bonds may form between the elastic fibers and the reinforcing fibers, resulting in a structure that is too stiff.
[0168] Within the gsm range disclosed herein, for weight fractions of absorbent fibers in the fluid management layer above about 30%, the elastic fibers and / or reinforcing fibers should be carefully selected. For the case of a soft cushion fluid management layer having a thickness factor of at least 0.13 or greater as described herein, resilient and / or reinforcing fibers may be selected to offset the loss of structural integrity of the absorbent fibers when wetted. For example, relatively high dtex elastic fibers may be used to mitigate the loss of rigidity exhibited by the absorbent fibers when wetted. In such cases, elastic fibers having a linear density of about 5 dtex to 15 dtex, or about 6 dtex to 12 dtex, or even about 7 dtex to 10 dtex may be utilized.
[0169] Alternatively or in combination, reinforcing fibers may be selected to further enhance structural integrity. For example, the reinforcing fibers may include bicomponent fibers in a sheath-core configuration, wherein the sheath is copolyethylene terephthalate (CoPET). However, with such changes in materials, additional issues may occur. For example, the joining of materials within the fluid management layer may thus be joined only via an adhesive or binder, rather than via melt bonding affected by heat treatment.
[0170] In other examples, material selection and methods can be configured to affect a greater number of bonds between reinforcing fibers. When the absorbent fibers constitute more than about 30% of the fluid management layer by weight, the heat to which the reinforcing fibers are bonded can be increased and / or the exposure time can be increased. This can increase the number of bonds in the reinforcing fiber matrix, which can mitigate the loss of absorbent fiber stiffness when wetted. However, as the number of bonds increases, stiffness increases. The increase in stiffness may reduce the user's perception of softness.
[0171] In a similar aspect, in addition or alternatively, the linear density of the reinforcing fibers can be increased to mitigate the loss of absorbent fiber stiffness, wherein the absorbent fibers comprise about 30% by weight or more. In such cases, the linear density of the reinforcing fibers can be selected to be about 3 dtex to 6 dtex, or about 4 dtex to 6 dtex.
[0172] While it may appear that the solution to the "wet collapse" of a fluid management layer is simply to increase the linear density of reinforcing and / or elastic fibers, their selection and proportion should be balanced. Particularly for viscous fluids, the fluid management layer contemplated herein should have a degree of capillarity to help draw fluid from the wearer-facing surface of the article. While the inclusion of relatively high decitex fibers may have thickness retention benefits, it may reduce capillarity, which reduces the ability of the fluid management layer to draw fluid from the topsheet.
[0173] The fluid management system contemplated herein may be incorporated into a variety of absorbent articles. A non-limiting example of a schematic representation of an absorbent article in the form of a feminine hygiene pad as contemplated herein is shown at Figure 1A As reflected, the pad 10 as contemplated herein may include a top sheet 20, a back sheet 50, and an absorbent structure 40 disposed between the top sheet 20 and the back sheet 50. The fluid management layer 30 may be disposed between the top sheet 20 and the absorbent structure 40. The pad has a wearer-facing surface 60 and an opposite outwardly facing surface 62. The wearer-facing surface 60 is primarily formed by the top sheet 20, while the outwardly facing surface 62 is primarily formed by the back sheet 50. Additional components (not shown) may be included adjacent to the wearer-facing surface 60 and / or the outwardly facing surface 62. For example, if the absorbent article is an incontinence pad, a pair of barrier cuffs extending generally parallel to the longitudinal axis 100 of the pad 10 may also form a portion of the wearer-facing surface 60. Similarly, one or more deposit fixing adhesives (to be used by the user / wearer to attach the pad in a suitable position within her underwear for use) may be present on the back sheet 50 and form a portion of the outwardly facing surface 62 of the absorbent article.
[0174] A non-limiting example of a configuration for the fluid management layer 30 is schematically depicted in Figure 1B As reflected, the fluid management layer 30 can have opposite end edges 32A and 32B that can extend generally parallel to the lateral axis 200, and side edges 31A and 32B that can extend generally parallel to the longitudinal axis 100. Similarly, the absorbent structure 40 can have opposite end edges 42A and 42B that can extend generally parallel to the lateral axis 200, and side edges 41A and 41B that can extend generally parallel to the longitudinal axis 100.
[0175] As reflected in the figure, each of the end edges 32A and 32B of the fluid management layer 30 can be disposed longitudinally outside the absorbent structure 40. However, this need not be the case. For example, the end edges 32A and / or 32B can be coextensive with the absorbent structure 40, or the end edges 32A and / or 32B can be disposed longitudinally inside the end edges 42A and / or 42B of the absorbent structure 40.
[0176] Similarly, side edges 31A and / or 31B may be disposed laterally outboard of side edges 41A and / or 41B of absorbent structure 40. Alternatively, side edges 31A and / or 31B may be laterally coextensive with side edges 41A and / or 41B of absorbent structure 40.
[0177] exist Figure 2 Schematically depicted is an arrangement of equipment along a production line that is configured to perform a process for forming a fluid management layer of the present disclosure. As reflected, a plurality of carding machines 210, 220, and 230 may each form a carded fiber web 214, 224, and 234 that is deposited on a conveyor belt 240 that moves along the machine direction MD. Each of the carded fiber webs 214, 224, and 234 may be provided to the conveyor belt 240 via a chute 212, 222, 232, respectively. Typically, a carding machine may have limitations on the volume and mass of fiber material that it can process and discharge at a desired production rate, and therefore, it may impose an upper limit on the basis weight of the carded fiber web that it can produce. Therefore, for a relatively low basis weight / lower thickness fluid management layer, a single carding machine may be sufficient to lay down the aggregate of carded fibers to achieve a desired basis weight at a desired production rate. For a fluid management layer having a larger desired basis weight / larger thickness, two, three, or more carding machines may be required to "stack" the carded fiber web of aggregated fibers to achieve a desired basis weight, such as Figure 2 After the first carded fiber web 214 is deposited on the conveyor belt 240, the second carded fiber web 224 is then deposited / covered on the first carded fiber web 214 on the conveyor belt 240. Similarly, the third carded fiber web 234 (if included) is next deposited / covered on the second carded fiber web 224 and the first carded fiber web 214 on the conveyor belt 240.
[0178] Subsequently, one or more carded webs 214, 224, and 234 are conveyed to consolidation equipment 250, which may utilize needles and / or high pressure water jets to entangle the fibers of the webs and consolidate them in the z-direction.Both carding and consolidation processes are known in the art.
[0179] Fewer or more than three carding machines may be utilized in the process. For example, a fluid management layer as contemplated herein may be produced using only two carding machines. In such an example, the first carded web 214 would be deposited on the conveyor belt 240. Subsequently, the second carded web 224 would be deposited / covered on the first carded web 214. The first carded web 214 and the second carded web 224 would then be integrated as described herein.
[0180] use Figure 2The arrangement of the equipment schematically depicted in the figure can produce a variety of configurations of the fluid management layer. However, one goal is that the fluid management layer has sufficient pore volume to allow rapid acquisition of fluid, and is also able to keep the fluid away from the top sheet to reduce the chance of back-seepage. With these design goals in mind, the fiber composition of the carded fiber webs (e.g., 214, 224 and / or 234), the carded fiber webs, can be selected to be different from each other. Assuming that the first carded fiber web will be closest to the wearer-facing surface of the absorbent article, the fiber selection for the first carded fiber web 214 can be such that there is more pore volume associated with the fiber web. The second carded fiber web 224 can adopt a similar construction. In contrast, the third carded fiber web 234 can have a fiber composition adapted to absorb fluid from the void space / pore volume in the first and second carded fiber webs 214 and 224, and distribute the fluid to the absorbent structure and across the absorbent structure. Alternatively, the first carded fiber web 214, the second carded fiber web 224 and the third carded fiber web 234 can have similar fiber compositions.
[0181] A schematic depiction of a non-limiting example of a cross section through a plane along the z-direction of a fluid management layer as contemplated herein is provided at Figure 3 As shown, the fluid management layer 30 has a first surface 300a, which is the wearer-facing surface of the layer 30, and an opposing second surface 300b, which is the outward-facing surface. Between the first surface 300a and the second surface 300b, the fluid distribution layer 30 may have two or more identifiable strata 30a, 30b, 30c along the z-direction resulting from the successive laydowns of the carded webs. These strata may be roughly depicted by fiber integration interface regions 30b, 30d, where the fibers of one carded web have been integrated with the fibers of the above or below adjacent carded webs by the above-described process.
[0182] Examples of suitable fluid management layers (also referred to as, for example, "secondary topsheets" or "acquisition / distribution layers") are further described in U.S. patent application serial numbers 16 / 831,862, 16 / 831,854, 16 / 832,270, 16 / 831,865, 16 / 831,868, 16 / 831,870, 16 / 831,879, and 17 / 490,193 and U.S. provisional patent application serial number 63 / 086,701. Additional suitable examples are described in US 9,504,613, WO 2012 / 040315, and US2019 / 0021917.
[0183] Absorption structure
[0184] The absorbent structure 40 of the present disclosure may have any suitable shape, including but not limited to an oval, a stadium shape, a rectangle, an asymmetric shape, a peanut shape, a trapezoid, a rounded trapezoid, an oval, and an hourglass shape. In some examples, the absorbent structure 40 may have a contoured shape, for example, it is narrower in the longitudinal middle region than in the end regions. In other examples, the absorbent structure may have a tapered shape that is wider in one end region of the pad and tapers to a narrower width in the other end region of the pad. The absorbent structure 40 may have different stiffnesses in the longitudinal and transverse directions.
[0185] The configuration and construction of the absorbent structure 40 may vary (e.g., the absorbent structure 40 may have different thickness zones, hydrophilic gradients, superabsorbent gradients, or lower average density and lower average basis weight acquisition zones). In addition, the size and absorbent capacity of the absorbent structure 40 may also vary to accommodate a variety of wearers. However, the total absorbent capacity of the absorbent structure 40 should be consistent with the design load and intended use of the disposable absorbent article or incontinence pad 10.
[0186] In some examples, the absorbent structure 40 may include multiple layers, each having specific features and / or functions. In some examples, the absorbent structure 40 may include a wrapper (not shown) that is included to encapsulate the absorbent components of the absorbent structure. The wrapper may be formed of one or more nonwoven materials, tissues, films, or other materials, or laminates thereof. In one form, the wrapper may be formed of only a single material, substrate, laminate, or other material that is at least partially wrapped around itself.
[0187] The absorbent structure 40 may include one or more adhesives, for example, to help secure the SAP or other absorbent material within the first and second laminates.
[0188] Suitable absorbent structures comprising relatively large amounts of superabsorbent polymers ("SAP" - also called "absorbent gelling materials" or "AGM") with various pore designs are disclosed in US 5,599,335, EP 1447 066, WO 95 / 11652, US 2008 / 0312622 A1 and WO 2012 / 052172.
[0189] It has been envisioned to be added to the absorbent structure. Potential additions to the absorbent structure are described in US 4,610,678, US 4,673,402, US 4,888,231 and US 4,834,735. The absorbent structure may further include a layer simulating a dual core system comprising a collection / distribution core of chemically rigid fibers positioned above the absorbent storage core, as described in US 5,234,423 and US No. 5,147,345. These may be considered useful as long as they do not offset or conflict with the effects of the following laminates of the absorbent structure of the present invention.
[0190] Some further examples of suitable absorbent structures 40 that can be used in the absorbent articles of the present disclosure are described in US2018 / 0098893 and US2018 / 0098891.
[0191] As mentioned above, absorbent articles comprising a fluid management layer contemplated herein may include a storage layer. Figure 1A and Figure 1B , the storage layer will generally be positioned at a position corresponding to the absorbent structure 40 depicted therein. The storage layer can be constructed as described with respect to the absorbent structure. The storage layer can contain conventional absorbent materials. In addition to conventional absorbent materials such as crepe cellulose fillers, fluff cellulose fibers, rayon fibers, and pulverized wood pulp fibers (also known as air felt or fluff pulp) and textile fibers, the storage layer can also include particles or fibers of superabsorbent materials that accept fluid and form hydrogels. (Such materials are also referred to as absorbent gelling materials (AGM)). AGM is generally capable of absorbing a relatively large weight of body fluid / dry weight AGM, keeping it under moderate pressure. Synthetic fibers spun from polymers, such as cellulose acetate, polyvinyl fluoride, polyvinylidene chloride, acrylic resins (such as Orlon), polyvinyl acetate, insoluble polyvinyl alcohol, polyethylene, polypropylene, polyamides (such as nylon), polyesters, bicomponent fibers, tricomponent fibers, mixtures thereof, and the like, can also be included in the second storage layer. The storage layer can also include filler materials, such as perlite, diatomaceous earth, vermiculite, or other suitable materials that can play a role in reducing rewet changes.
[0192] The storage layer or fluid storage layer may include an overall uniform distribution of absorbent gelling material (AGM), or may include an uneven distribution of absorbent gelling material. The AGM may be distributed and / or concentrated by depositing it into channels or pockets, or may be deposited in a pattern, including stripes, crisscross patterns, swirls, dots, or any other conceivable two-dimensional or three-dimensional pattern. The AGM may be sandwiched between a pair of fibrous cover layers. The AGM may be at least partially encapsulated by a single fibrous cover layer.
[0193] Portions of the storage layer may be formed substantially only of superabsorbent material / AGM, or may be formed of AGM distributed and dispersed in a suitable carrier structure such as cotton wool or an aggregate of cellulose fibers in the form of fluff or reinforcing fibers. A non-limiting example of a storage layer may include a first layer formed substantially only of AGM particles or fibers, which are placed or deposited onto a second layer, which is formed of a distribution of AGM particles or fibers within cellulose fibers.
[0194] Examples of absorbent structures formed of superabsorbent / AGM layers and / or superabsorbent / AGM layers dispersed in other aggregates of cotton wool or cellulose fibers that can be used in absorbent articles contemplated herein (e.g., sanitary napkins, incontinence products) are disclosed in US2010 / 0228209A1. Absorbent structures comprising relatively high levels of SAP / AGM using various core designs are disclosed in the following patents: US 5,599,335, EP 1 447 066, WO 95 / 11652, US.2008 / 0312622A1, WO2012 / 052172, US 8,466,336, and US 9,693,910 issued to Carlucci. These can be used to construct absorbent structures or storage layers.
[0195] Negatives
[0196] The backsheet 50 may be disposed beneath the absorbent structure 40 and is the outermost layer of the article, thereby forming the outwardly facing surface of the article. The backsheet 50 may be joined to the absorbent structure 40 and / or the topsheet (around the outer periphery) by any suitable attachment method known in the art. For example, the backsheet 50 may be secured to the absorbent structure 40 by a uniform continuous layer of adhesive, a patterned layer of adhesive, or an array of separate lines, spirals, or spots of adhesive. Alternatively, the attachment method may include the use of heat bonding, pressure bonding, ultrasonic bonding, dynamic mechanical bonding, or any other suitable attachment method or combination of these attachment methods as known in the art.
[0197] Backsheet 50 can be impermeable or substantially impermeable to liquid (e.g., urine, menstrual fluid) under common use conditions, and can be made of thin plastic film, but other liquid-impermeable flexible materials can also be used. Backsheet 50 can prevent or at least inhibit the wetting of the outflow absorbed and contained in the absorbent structure 40 from contacting or adjacent underwear, outerwear, bedding, etc. with the article 10. However, in some examples, backsheet 50 can be constructed to allow vapor to escape from the absorbent structure 40 (i.e., "breathable"), and in examples, backsheet 50 can be constructed so that vapor is impermeable (i.e., impermeable). Backsheet 50 can include polymer films, such as polyethylene films or polypropylene films. Suitable materials for backsheet 50 are thermoplastic films with a thickness of about 0.012mm (0.5 mil) to 0.051mm (2.0 mils). Any suitable liquid-impermeable backsheet known in the art can be used in the present invention.
[0198] The backsheet 50 acts as a barrier to prevent the fluid absorbed and held in the absorbent structure 40 from migrating to the outwardly facing surface of the pad. Preferred materials are soft, smooth, compliant, liquid and vapor permeable materials that provide comfortable softness and conformability and produce less noise so that no annoying noise is caused during exercise.
[0199] Non-limiting examples of materials suitable for forming the backsheet are described in US 5,885,265, US 6,462,251, US 6,623,464 and US 6,664,439. Examples of suitable double or multi-layer breathable backsheets include those described in US 3,881,489, US 4,341,216, US 4,713,068, US 4,818,600, EP 203 821, EP 710 471, EP 710 472 and EP 793952. Additional examples of suitable single layer breathable backsheets include those described in GB A 2184 389, GB A 2184 390, GB A 2184 391, US 4,591,523, US 3 989 867, US 3,156,242 and WO 97 / 24097.
[0200] The backsheet may be a nonwoven web having a basis weight of about 20 gsm to 50 gsm. In one example, the backsheet may be a 23 gsm spunbond nonwoven web of hydrophobic 4 denier polypropylene fibers, available from Fiberweb Neuberger under the trade name F102301001. The backsheet may be coated with an insoluble liquid swellable material as described in US 6,436,508.
[0201] The backsheet has an outwardly facing side and an opposite wearer-facing side. The outwardly facing side of the backsheet may include a non-adhesive area and an adhesive area. In order to enable the user / wearer to attach the pad to the wearer-facing surface of her undergarment in a position suitable for use, the adhesive area may be provided by any conventional means. Pressure sensitive adhesives have been found to be well suited for this purpose.
[0202] test
[0203] For the purpose of experimentation and discovery, the inventors have manufactured and tested a number of prototype samples of absorbent articles in the form of feminine hygiene pads including topsheets and fluid management layers in various configurations as contemplated herein. The prototype samples had the following features.
[0204] Top sheet
[0205] The topsheets of all prototype samples had a basis weight of about 24 gsm.
[0206] The topsheets of all prototype samples were cut from a nonwoven web of carded staple length fibers having an average staple length of 38 mm and an average denier of 4. The fibers were bicomponent, having a concentric sheath-core configuration, wherein the core component was PET and the sheath component was low density polyethylene (LDPE); the weight ratio of the components was about 1: 1. The nonwoven web included a plurality of randomly distributed fiber-to-fiber bonds that had been created by air through heat bonding of the carded fibers.
[0207] The topsheet is attached to the underlying adjacently disposed fluid management layer via application of a pressure sensitive adhesive applied in a discontinuous series of narrow spiral paths oriented generally in the longitudinal direction. The fluid management layer is attached to the underlying adjacently disposed absorbent structure in a similar manner.
[0208] Further details vary among the samples as described below:
[0209] Sample #1: Topsheet nonwoven formed from a blend of hydrophilic and hydrophobic fibers in a 60:40 ratio of hydrophilic fiber weight to hydrophobic fiber weight. The topsheet nonwoven did not include apertures or applied anti-stick agents.
[0210] Sample #2: The topsheet nonwoven is formed from a blend of hydrophilic and hydrophobic fibers in a ratio of 60:40 hydrophilic fiber weight to hydrophobic fiber weight. The topsheet nonwoven includes a hole pattern having a 0.55 mm 2 The average xy-size pore area is 1.33 xy-1.67 mm and constitutes about 6% open area. The topsheet nonwoven does not include an applied anti-stick agent.
[0211] Sample #3: Topsheet nonwoven formed from a blend of hydrophilic and hydrophobic fibers in a 60:40 ratio of hydrophilic fiber weight to hydrophobic fiber weight. The nonwoven included a regular pattern of holes therethrough having a diameter of 0.60 mm. 2 The average xy pore area is 1.33 xy and constitutes about 12% open area. The topsheet nonwoven does not include an applied anti-stick agent.
[0212] Sample #4: Topsheet nonwoven formed from a blend of hydrophilic and hydrophobic fibers in a 60:40 ratio of hydrophilic fiber weight to hydrophobic fiber weight. The nonwoven included a regular pattern of holes therethrough having a 2.3 mm 2 The average xy pore area is 1.33 xy and constitutes about 19% open area. The topsheet nonwoven does not include an applied anti-stick agent.
[0213] Sample #5: Topsheet nonwoven formed substantially entirely of hydrophobic fibers. The topsheet nonwoven did not include apertures or applied anti-stick agents.
[0214] Sample #6: Topsheet nonwoven formed substantially entirely of hydrophobic fibers. The nonwoven includes a regular pattern of holes therethrough having a diameter of 0.55 mm. 2 The average xy pore area is 1.33 xy and constitutes about 6% open area. The topsheet nonwoven does not include an applied anti-stick agent.
[0215] Sample #7: Topsheet nonwoven formed substantially entirely of hydrophobic fibers. The nonwoven includes a regular pattern of holes therethrough, the holes having a diameter of 0.6 mm. 2 The average xy dimension pore size was 1000 Å and constituted about 12% open area. The topsheet nonwoven did not include an applied anti-stick agent.
[0216] Sample #8: Topsheet nonwoven formed substantially entirely of hydrophobic fibers. The nonwoven includes a regular pattern of holes therethrough having a 2.3 mm 2 The average xy dimension pore size was 1.33 xy and constituted about 19% open area. The topsheet nonwoven did not include an applied anti-stick agent.
[0217] Fluid Management Layer
[0218] All prototype samples included a fluid management layer of substantially common structure and composition disposed adjacent to the topsheet. The common fluid management layer had a basis weight of about 65 gsm. It was composed of: about 20% by weight of 1.3 dtex viscose fibers; about 30% by weight of 10 dtex hollow spiral polyethylene terephthalate fibers; and about 50% by weight of 2.2 dtex bicomponent fibers having a concentric sheath-core configuration, wherein the core component was PET and the sheath component was PE, with a weight ratio of PET:PE of about 1:1. These bicomponent fibers had an average dtex of about 2.2. The fluid management layer had two layers, each layer having the same homogenous fiber blend, which was lightly hydroentangled and air-bonded by heat.
[0219] Absorption structure
[0220] All prototype samples included an absorbent structure having a substantially common structure and composition, which was disposed adjacent to the fluid management layer. The common absorbent structure was an airlaid blend of pulp fibers, absorbent gelling material, and bicomponent fibers, having a basis weight of 182 gsm, available from Glatfelter Corporation (Charlotte, North Carolina, USA) in the form of a pre-made festoon web. The structure and composition of the absorbent structure were not believed to have any significant effect in the performance differences measured between the various prototype samples.
[0221] Negatives
[0222] All prototype samples included a common backsheet disposed beneath the absorbent structure, the backsheet being formed from an extruded polyethylene film.
[0223] Test results and data
[0224] The amounts of all eight prototype samples were measured and tested using the "Acquisition Time and Rewet Measurement Method" described below.
[0225] Fig. 9 The second acquisition time (ACQ-2) measured for each of the 8 samples is reported. For the purposes of this article, it is believed that the second acquisition time (ACQ-2) is most relevant to actual user experience because it reflects the fluid acquisition of a feminine hygiene pad that has been used / worn for a period of time and has absorbed some fluid, but is subsequently exposed to a relatively large fluid discharge, such as may occur when the user / wearer's body posture suddenly changes after a period of inactivity or a relatively low activity level. The thick horizontal line drawn at the 30 second mark in the chart represents the highest acquisition time that the inventors believe will be acceptable to relevant consumers / users.
[0226] Fig.10 The sum of the surface free fluid (SFF) and rewet measured for each of the 8 samples is reported. For the purposes of this article, it is believed that this sum is most relevant to actual user experience because it reflects the extent to which a pad that has absorbed a large amount of fluid will allow fluid to return to the topsheet surface under moderate pressure, which reflects the cause of an unsatisfactory wet feel for the user / wearer. The bold horizontal line drawn at the 400 mg mark in the chart represents the highest SFF+rewet that the inventors believe will be acceptable to relevant consumers / users.
[0227] from Fig. 9 As can be seen from the graph in , all prototype samples exhibited a second acquisition time that was considered acceptable. Prototype samples 1-4 exhibited the best performance, with prototype sample 3 exhibiting the best performance of all samples.
[0228] from Fig.10 As can be seen in the graphs in , all prototype samples exhibited SFF+Rewet values that were considered acceptable. Prototype Sample 1 exhibited the best performance among all samples, followed by Prototype Samples 8, 7, and 5, in that order.
[0229] From this data, it can be concluded that Prototype Sample 1 was the most successful, as it appeared in the top four performers in both categories. However, in a different situation, the product designer may choose to prioritize fast acquisition (e.g., Prototype Sample 3 was the top performer among the samples tested), or alternatively, low rewet values (e.g., Prototype Sample 1 was the top performer among the samples tested).
[0230] Test and measurement methods
[0231] thickness
[0232] The thickness of the specimen is measured as the distance between the reference platform on which the specimen rests and the pressure foot that applies a specified amount of pressure to the specimen for a specified amount of time. All measurements are made in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity, and the specimens are conditioned in this environment for at least 2 hours prior to testing.
[0233] Thickness is measured with a manually operated micrometer equipped with a pressure foot capable of applying a steady pressure of 0.50 kPa ± 0.01 kPa to the test specimen. The manually operated micrometer is a deadweight instrument with readings accurate to 0.01 mm. A suitable instrument is a Mitutoyo series 543ID-C Digimatic, or equivalent, available from VWR International. The pressure foot is a flat circular movable surface with a diameter smaller than the specimen and capable of applying the required pressure. A suitable pressure foot has a diameter of 25.4 mm, but smaller or larger pressure feet may be used depending on the size of the specimen being measured. The specimen is supported by a horizontal, flat reference platform that is larger than and parallel to the surface of the pressure foot. The system is calibrated and operated in accordance with the manufacturer's instructions.
[0234] If necessary, obtain the sample by removing it from the absorbent article. When cutting the sample from the absorbent article, be careful not to cause any contamination or deformation to the sample layer during the process. The sample is taken from an area without folds or wrinkles and must be larger than the pressure foot.
[0235] To measure thickness, first zero the micrometer relative to a horizontal flat reference platform. Place the specimen on the platform with the test position centered under the pressure foot. Gently lower the pressure foot at a rate of descent of 3.0mm ± 1.0mm per second until full pressure is applied to the specimen. Wait 5 seconds, then record the thickness of the test specimen to the nearest 0.001mm. Repeat in a similar manner for a total of ten replicate test specimens. Calculate the arithmetic mean of all thickness measurements and report as "Thickness" to the nearest 0.001mm.
[0236] Thickness factor
[0237] As previously stated the thickness factor is the thickness per 10 gsm of sample basis weight. Therefore, the formula is thickness / (basis weight / 10).
[0238] Basis Weight
[0239] The basis weight of a sample of sheet or web material is the mass (in grams) per unit area (in square meters) of a single material layer. If it is not otherwise known or available, the basis weight can be measured using EDANA Pharmacopoeia Method NWSP130.1. The mass of the test sample is cut into a known area, and the mass of the test sample is determined using an analytical balance accurate to 0.0001 grams. All measurements are performed in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity, and the test sample is conditioned in this environment for at least 2 hours before testing.
[0240] The test sample taken from the raw material roll or raw material sheet or the test sample obtained from the material layer removed from the absorbent article is measured. When the material layer is cut out from the absorbent article, it is noted that no contamination or deformation is caused to the layer during the process. The cut layer should not contain residual adhesive. In order to ensure that all adhesives are removed, the layer is soaked in a suitable solvent that will dissolve the adhesive and will not adversely affect the material itself. One such solvent is THF (tetrahydrofuran, CAS109-99-9, which is used for general purposes and is purchased from any convenient source). After the solvent is soaked, the material layer is allowed to be thoroughly air-dried in a manner that prevents excessive stretching or other deformation of the material. After the material has dried, the test sample is obtained. The specimen must be as large as possible to take into account any inherent material variability.
[0241] Measure the dimensions of the single-layer specimen using a calibrated steel metal ruler from NIST or equivalent. Calculate the area of the specimen and record it to the nearest 0.0001 square centimeter. Use an analytical balance to obtain the mass of the specimen and record it to the nearest 0.0001 gram. Calculate the basis weight by dividing the mass (in grams) by the area (in square meters) and record it to the nearest 0.01 grams per square meter (gsm). Repeat in a similar manner for a total of ten replicate test specimens. Calculate the arithmetic mean of the basis weight and report it to the nearest 0.01 grams per square meter.
[0242] Material composition analysis
[0243] If the information is not available otherwise, the quantitative chemical composition of test specimens comprising a mixture of fiber types is determined using ISO 1833-1. All tests are performed in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity.
[0244] The test sample taken from the raw material roll or raw material sheet or the test sample obtained from the material layer removed from the absorbent article is analyzed. When the material layer is cut out from the absorbent article, it is noted that no contamination or deformation is caused to the layer during the process. The cut layer should not contain residual adhesive. In order to ensure that all adhesives are removed, the layer is immersed in a suitable solvent that will dissolve the adhesive and will not adversely affect the material itself. A kind of such solvent is THF (tetrahydrofuran, CAS109-99-9, which is used for general purposes and is purchased from any convenient source). After the solvent is soaked, the material layer is allowed to be thoroughly air-dried in a manner to prevent excessive stretching or other deformation of the material. After the material has dried, the test sample is obtained and tested according to ISO 1833-1 to quantitatively determine its chemical composition.
[0245] Average fiber dtex or denier
[0246] Textile webs (e.g., woven webs, nonwoven webs, air-laid webs) are composed of individual material fibers. In one aspect, the fibers are characterized by their linear mass density, reported in denier or decitex. The decitex value is the mass (in grams) of the fibers present in 10,000 meters of the fiber. The denier value is the mass (in grams) of the fibers present in 9,000 meters of the fiber. The average decitex value or denier value of the fibers in the web of the material is often reported by the manufacturer as part of the specification. If the average decitex value or denier value of the fiber cannot be known or is not available in other ways, it can be calculated in the following manner: the cross-sectional area of the fiber is measured via a suitable microscopic technique such as a scanning electron microscope (SEM), the composition of the fiber is determined with a suitable technique such as FT-IR (Fourier transform infrared) spectroscopy and / or DSC (dynamic scanning calorimetry), and then the literature value of the density of the composition is used to calculate the mass (in grams) of the fibers present in 10,000 meters of fiber (for decitex) or 9,000 meters of fiber (for denier).
[0247] All tests were conducted in a chamber maintained at a temperature of 23°C ± 2.0°C and a relative humidity of 50% ± 2%, and the specimens were conditioned in the same environmental conditions for at least 2 hours prior to testing.
[0248] If desired, a representative sample of the web material of interest can be cut out from the absorbent article. In this case, the web material is removed in order to prevent the sample from being stretched, deformed or contaminated.
[0249] SEM images are obtained and analyzed as follows to determine the cross-sectional area of the fiber. In order to analyze the cross-section of a sample of a fiber mesh material, a test sample is prepared as follows. A sample of approximately 1.5 cm (height) × 2.5 cm (length) and no creases or wrinkles is cut from the fiber mesh. The sample is immersed in liquid nitrogen and the edge is broken along the length of the sample with a razor blade (No. 9 VWR single-edged industrial razor blade, surgical carbon steel). The sample is sputter-coated with gold and then adhered to the SEM mount using double-sided conductive tape (Cu, 3M, purchased from electron microscopy sciences). The sample is oriented so that the cross section is as perpendicular to the detector as possible to minimize any tilt distortion of the measured cross section. SEM images are obtained at a resolution sufficient to clearly illustrate the cross section of the fiber present in the sample. The fiber cross section may vary in shape, and some fibers may be composed of multiple individual filaments. In any case, the area of each cross section in the fiber cross section is determined (for example, using the diameter of a circular fiber, the major and minor axes of an elliptical fiber, and image analysis for more complex shapes). If the fiber cross section indicates a non-uniform cross-sectional composition, the area of each identifiable component is recorded and the decitex contribution of each component is calculated and then summed. For example, if the fiber is bicomponent, the cross-sectional areas of the core and sheath are measured separately and the decitex contributions from the core and sheath are calculated separately and summed. If the fiber is hollow, the cross-sectional area does not include the interior portion of the fiber composed of air, which does not contribute significantly to the fiber decitex. In general, at least 100 such measurements of the cross-sectional area are made for each fiber type present in the sample and are reported in square micrometers (μm 2 ) is used as the unit to record the cross-sectional area a of each fiber k The arithmetic mean (accurate to 0.1 μm) 2 ).
[0250] The fiber composition is determined using common characterization techniques such as FTIR spectroscopy. For more complex fiber compositions (such as polypropylene core / polyethylene sheath bicomponent fibers), a combination of common techniques (e.g., FTIR spectroscopy and DSC) may be required to fully characterize the fiber composition. This process is repeated for each fiber type present in the fiber web material.
[0251] Average decitex of each fiber type in the web material k The value is calculated as follows:
[0252] d k =10 000m×a k ×ρ k ×10 -6
[0253] where d kIn grams (per 10,000 m of calculated length), a k In μm 2 is a unit, and ρ k In grams per cubic centimeter (g / cm 3 ) in units. Report the average dtex to the nearest 0.1 g (per 10,000 calculated meters) and the fiber type (e.g., PP, PET, cellulose, PP / PET bicomponent). The average denier value for each fiber type in the web material is its dtex. k value × 0.9.
[0254] Hole Open Area Percentage Measurement Method
[0255] The open area percentage is measured on an image of an open top sheet sample collected using a flatbed scanner. The scanner is capable of scanning in reflective mode at a resolution of 2400 dpi and 8-bit grayscale. A suitable scanner is an Epson Perfection V750 Pro purchased from Epson America Inc. (Long Beach, California, USA), or one having substantially similar functionality. The scanner interacts with a computer running an image analysis program. A suitable program is ImageJ v.1.47 (National Institute of Health, USA), or a program having substantially similar functionality. The sample image is distance calibrated based on the image collected of a ruler certified by NIST. In order to achieve maximum contrast, the sample is backed with an opaque background sheet of uniform black color before the image is collected. All measurements are performed in a conditioning room maintained at about 23 ± 2°C and about 50 ± 2% relative humidity.
[0256] The measurement samples were prepared as follows:
[0257] Obtain the desired number of samples of the absorbent article of interest. To obtain a measurement sample, tap the sample absorbent article around its perimeter (i.e., not taped on the area below the fluid management layer), with the wearer-facing side facing up, to a horizontal, flat work surface in a flat configuration. Any elastic material included (e.g., in the leg cuffs), if present, may be cut to facilitate laying the article flat. Identify and mark the outer boundaries of the apertured topsheet area covering the fluid acquisition layer of the article. Now cut through the topsheet and any adhered underlying layers with a new razor blade or other reasonably new sharp cutting tool, around and through the marked outer boundaries. Then carefully separate the sample of the apertured topsheet from the cut-out portion and remove it from the underlying layers so that its longitudinal and lateral dimensions are not altered to avoid deformation of the apertures. If the topsheet is adhered to the underlying layers via an adhesive, apply any solvent suitable for dissolving the adhesive and allowing the topsheet to be easily separated from the underlying layers without dissolving the polymer material of the fibers constituting the nonwoven web material of the topsheet before attempting separation. (In many examples, tetrahydrofuran (THF) may be a suitable solvent for this purpose. As long as the solvent does not dissolve the polymer that makes up the fiber itself, there is no need to worry about whether the solvent dissolves the surface finish coating applied to the fiber.) Once the cut-out portion of the topsheet that makes up the measurement sample is removed, its wearer-facing side is identified. Five replicate measurement samples obtained from five samples of the absorbent article of interest are prepared for measurement. Prior to imaging, the samples are conditioned at about 23°C ± 2°C and about 50% ± 2% relative humidity for 2 hours.
[0258] The images were obtained as follows.
[0259] A ruler was placed on the scanning bed so that it was oriented parallel to the side of the scanner glass. An image of the ruler (calibration image) was acquired in reflection mode at a resolution of 2400 dpi (approximately 94 pixels / mm) and 8-bit grayscale. The calibration image was saved as an uncompressed TIFF format file. After obtaining the calibration image, the ruler was removed from the scanner glass and all samples were scanned under the following scanning conditions.
[0260] Place the measurement sample flat on the center of the scanning bed, with the body-facing surface of the sample facing the glass surface of the scanner. The corners and edges of the sample are fixed so that its initial longitudinal and lateral dimensions (as on the article before removal) are maintained. The sample is oriented so that its major and minor axes are aligned parallel and perpendicular to the sides of the glass surface of the scanner, respectively. A black background is placed on top of the sample, the scanner lid is closed, and a scanned image of the entire sample is acquired with the same settings as those used for the calibration image. The sample image is saved as an uncompressed TIFF format file. The remaining four replicate samples are scanned and saved in a similar manner.
[0261] The sample image is analyzed as follows. Open the calibration image file in the image analysis program and calibrate the image resolution using an imaging ruler to determine the number of pixels per millimeter. Now open the sample image in the image analysis program and set the distance scale using the image resolution determined from the calibration image. Now identify a rectangular cross-section (region of interest, or "ROI") centered longitudinally and laterally on the sample having a longitudinal dimension of 60.0 mm and a lateral dimension of 30.0 mm along the longitudinal axis, and visually inspect the image of the holes present within the ROI. Now using the software tool, manually outline each of the holes in the ROI (as well as any portions thereof at the edges of the ROI). Appropriate contours will be drawn around the perimeter of the hole along the visually discernible inner edge of the concentrated portion of the displacement fibers 503. Individual fibers that may have left the main structure and / or the concentrated portion of the displacement fibers around the perimeter and passed through the deviation of the main opening area entering or passing through the hole (illustrated in an exemplary manner, Figure 5 The individual fibers 504 shown as deviated in FIG. 5 are not considered to be subtracted from the hole area for purposes herein. ) The software is then used to measure the area within each discrete hole contour (full and partial) within the ROI and record each to the nearest 0.01 mm. 2 , and the sum is calculated. The area of each discrete hole is defined as the xy surface area within the visually discernible outline of the open area, which is generated by mechanical penetration of the fiber web and the xy displacement of the fibers during the opening process that creates the holes through the fiber web. (See, for example, Figure 5 , where discrete hole areas 501 and visually discernible boundaries 502 are depicted. The dark area of the depicted holes is an image of the black construction paper used as a backing for the sample from which this particular image was made. ) The sum of the areas of all holes within the ROI is recorded as the "hole area" to the nearest 0.01 mm 2 Now divide the “hole area” by the ROI area (1,800mm 2 ), then multiply by 100 and record as the "opening area" to the nearest 0.1%.
[0262] In a similar manner, the entire procedure was repeated for the remaining four replicate images. The arithmetic mean of the "Open Area" across all five replicates was calculated and reported as the "Mean Open Area" to the nearest 0.1%.
[0263] Collection time and back-infiltration measurement method
[0264] This method describes how to measure the outflow acquisition time, interface free fluid amount and low pressure and high pressure re-seepage value of the absorbent article loaded with new artificial menstrual fluid (nAMF) prepared as described herein.After the pre-treatment step, nAMF of known volume is introduced into the absorbent article three times.The absorbent article is used to collect the required time of each nAMF dosage in the nAMF dosage using a strike-through plate and an electronic circuit interval timer.After each fluid dosage, when the fluid is transferred to the filter paper from the bottom surface of the strike-through plate, the interface free fluid (IFF) is measured by gravimetric analysis. Subsequently, low pressure and high pressure re-seepage are measured after the last fluid dosage.Surface free fluid (SFF) is the amount of fluid retained in the top sheet of the absorbent article.SFF is measured by carrying out low pressure (0.1psi) re-seepage.After measuring SFF, the re-seepage of higher pressure (0.5psi) is immediately carried out to measure the total re-seepage of the absorbent article.All tests are carried out in a room maintained at 23 ℃ ± 2 ℃ and 50% ± 2% relative humidity.
[0265] Gear and Supplies
[0266] Moisture permeable board configuration
[0267] refer to Figure 6 , Figure 7 , Fig. 8A and Figure 8B , the strike-through plate 601 is composed of a transparent Plexiglas or equivalent having overall dimensions of 10.2 cm long (y direction) x 10.2 cm wide (x direction) x 3.1 cm high. (All positional and spatial references herein present the strike-through plate as it would have when resting on a horizontal surface, bottom side down. All references to the x, y, and z directions in this measurement method description are relative only to the directions appearing on the surface.) Figure 6 , Figure 7 , Fig. 8A and Figure 8B603. The references to the x, y, and z directional arrow indicators in the drawings and do not necessarily apply to such references appearing elsewhere in this specification). A central test fluid well 608 having a circular opening and a cylindrical wall having a diameter of 25 mm opens at the top surface of the plate and extends vertically downward (z-direction) from the top surface of the plate to a depth of 15 mm and then turns radially inward to define a tapered wall extending vertically downward an additional 7.5 mm from the top surface while tapering uniformly to a diameter matching the diameter of the test fluid port 603. The test fluid port 603 is concentric / coaxial with the test fluid well 608 and has a cylindrical wall having a diameter of 6.6 mm that extends vertically downward a further 5 mm from the top surface to a longitudinal fluid channel 607. The longitudinal fluid channel 607 is machined or otherwise formed in the bottom of the plate. The longitudinal fluid channel 607 has a depth from the bottommost surface of the plate defined by vertical side walls that extend upward (z direction) 3.5 mm at the midpoint of the channel (at the test fluid port 603) and then slope downward at an angle 607a of 0.72° toward each longitudinal end of the channel. The longitudinal fluid channel opens at the bottom surface of the plate to allow fluid to be introduced onto the underlying specimen and to allow flow along the xy area defined by the fluid channel 607. The fluid channel 607 is centered below the test fluid port 603 and extends with its length in the y direction, which is perpendicular to the length of the x-direction path of the electrode 604 through the plate. The longitudinal fluid channel 607 has an x-direction width of 5 mm and a y-direction length of 80 mm, with upper corners rounded with a radius 607b of 1.0 mm around the entire perimeter of the channel. The wall at the opposite distal end of the longitudinal fluid channel 607 has a cylindrical radius 609 of 2.5 mm in the xy plane.
[0268] Two rectangular cavities 602 (80.5 mm long (x-direction) x 24.5 mm wide (y-direction) x 25 mm deep (z-direction)) are symmetrically arranged outside of the fluid ports 603 and centered about the y-direction axis of the plate. These can be loaded with lead shot (or other weighting material) to the extent necessary to adjust the total mass of the plate plus the weighting material to provide 0.10 psi (7.0 g / cm2) over the total xy area of the defined plate. 2 ) pressure, which for the purposes of this article is considered to be 10.2 cm x 10.2 cm = 104.04 cm 2, without subtracting the area defined by the longitudinal fluid channel 607. Electrodes 604 are embedded in the plate 601, each electrode providing an electrical connection between one of the two external banana-type sockets 606 and another opposite position on the inner wall 605 of the longitudinal fluid channel 607. The bottommost portion of the end of the electrode 604 exposed in the port 603 is 1.57 mm from the bottommost surface of the plate 601. A circuit interval timer is connected to the socket 606 to monitor the impedance or resistance between the two electrodes 604 and measure the time from the introduction of nAMF into the port 603 (establishing an electrical connection between the electrodes and / or significantly reducing the impedance or resistance therebetween) until the nAMF is discharged from the port 603 and the channel 607 into the sample until the level below the electrode (disconnecting the electrical connection between the electrodes and / or significantly increasing the impedance or resistance therebetween). The circuit interval timer has a resolution of 0.01 seconds.
[0269] Pre-treatment board
[0270] The pretreatment plate (not shown) is used in combination with a pretreatment weight (not shown) to apply a droplet of nAMF to the surface of the specimen, thereby preparing the surface of the sample before introducing the full fluid dose specified below. The pretreatment plate is rectangular, made of transparent plexiglass or equivalent, 14 inches (35.6cm) long × 8 inches (20.3cm) wide, and a thickness (thickness) / caliper of about 0.25 inches (6.4mm). The pretreatment plate is marked with five circular marks, each 5mm in diameter, placed 1cm apart (center to center) and centered along the longitudinal axis of the plate. The five center marks are centered at the lateral midpoint of the longitudinal axis of the plate. These marks indicate the position of the nAMF droplets. The mark is located on the lower side of the pretreatment plate and can be milled out or simply drawn in any way with a permanent marker or equivalent so that they are visible through the top surface of the pretreatment plate.
[0271] Pre-processing heavy objects
[0272] The pretreatment weight (not shown) is 10.2 cm x 10.2 cm in x and y dimensions and is composed of a flat, smooth, rigid material (e.g., stainless steel). The pretreatment weight has a total mass of 726 g ± 0.5 g to produce a 104.04 cm diameter across the bottom of the pretreatment weight. 2 0.10 psi (7.0 g / cm 2 ) pressure.
[0273] IFF Rubber Pads
[0274] When measuring the amount of interface fluid, a rubber pad with a flat surface ("IFF rubber pad") (not shown) is used. The IFF rubber pad is made of high-strength neoprene with a 40A durometer and 1 / 8 inch thickness / caliper (available from WW Grainger, Inc, item #1DUV4, or equivalent) and cut into a size of 6 inches (15.2 cm) x 6 inches (15.2 cm).
[0275] Backflow weight assembly
[0276] For the entire rewet portion of the test, a padded weight assembly ("rewet weight assembly") (not shown) was required, which was constructed to fit within its 10.2 cm x 10.2 cm (104.04 cm 2 ) surface area with 0.5 psi (35.1 g / cm 2 ). The back permeation weight assembly is assembled as follows.
[0277] Lay a piece of polyethylene film (about 25 microns thick and about 22.5 square centimeters in the xy direction, from any convenient source) flat on a horizontal work surface. Place a piece of polyurethane foam (25 mm thick, density 1.0 lb / ft 3 , IDL 24 psi, available from Concord-Renn Co., Cincinnati, OH, or equivalent) cut to 10.2 cm x 10.2 cm and then placed in the center of the top of the membrane. A piece of clear Plexiglas (10.2 cm x 10.2 cm and approximately 6.4 mm thick) is then stacked on top of the polyurethane foam. Next, the polyethylene film is gently stretched taut under the polyurethane foam, and the portion of the polyethylene film extending outward from under the polyurethane foam is wrapped around and over the polyurethane foam and Plexiglas sheet and secured thereabout with clear tape. A metal weight of appropriate mass is selected and stacked on top of the Plexiglas sheet and secured to the Plexiglas sheet so that the total mass of the assembly (re-infiltration weight assembly) is 3.6 kg ± 0.1 kg.
[0278] filter paper
[0279] For the IFF, SFF and overall re-infiltration steps, various numbers of layers of filter paper are required (not shown). Prior to testing, the filter paper to be used is conditioned at 23°C ± 2°C and 50% ± 2% relative humidity for at least 2 hours. Suitable filter paper has a basis weight of about 88 gsm, a thickness of about 249 microns, has an absorption rate of about 5 seconds, and can be purchased from Ahlstrom-Munksjo (Mt. Holly Springs, PA) with grade 632 or equivalent. Each filter paper is square and has a size of 5 inches by 5 inches (12.7 cm by 12.7 cm).
[0280] program
[0281] 1) Prior to testing, place the test sample (an example of the absorbent article of interest) at 23°C ±
[0282] Condition at 2°C and 50% ± 2% relative humidity for at least 2 hours.
[0283] 2) Remove the test samples from their outer packaging and, if applicable, open the wrapping to unfold the product, being careful not to press down or pull on the product while handling. Do not attempt to smooth out wrinkles. Using scissors, cut any release paper covering the adhesive attaching flaps (if present), and place the samples on a horizontal work surface with the wearer-facing surface facing upward (i.e., facing outwardly downward).
[0284] 3) For each sample, determine the dose location as follows. The dose location is the intersection of the midpoints of the longitudinal and lateral axes of the fluid management layer. Once the dose location is identified, mark it with a small dot using a black, fine-tip, permanent marker.
[0285] 4) For each test of a sample, pre-treat the test sample with nAMF as follows.
[0286] a) Place the pre-treated plate on a level work surface with the side with the circular marking facing downwards.
[0287] b) Using a single channel, fixed volume pipette, dispense 50 μL of nAMF into each of the five locations on the top side of the pre-treated plate, covering each of the five circular markings.
[0288] c) Position the test sample over the pre-treatment plate with the wearer-facing surface of the sample facing downward, facing the pre-treatment plate, such that the longitudinal axes of the sample and pre-treatment plate are aligned and the pre-marked dose position on the test sample is centered over the center drop of nAMF on the pre-treatment plate.
[0289] d) After it is properly positioned above the pre-treatment plate, bring the test sample down into contact with the pre-treatment plate, and then quickly place the pre-treatment weight over / on the outward (upward) side of the test sample, centering it over the dose position / center drop of nAMF on the pre-treatment plate, and immediately start a stopwatch type timer after 40 seconds, set to alarm. After 40 seconds have passed, remove the pre-treatment weight from the test sample, and remove the test sample from the pre-treatment plate. Flip the test sample so that the side facing the wearer is upward, place it on a horizontal work surface, and quickly continue with the following steps.
[0290] 5) The first acquisition time (ACQ-1) was measured as follows.
[0291] a) Connect an electronic circuit interval timer to the strike-through plate 601 and reset the timer to zero.
[0292] b) Position the strike-through plate 601 over the wearer-facing surface of the test sample so that the long (y-direction) axis of the longitudinal fluid channel 607 on the underside of the strike-through plate 601 is aligned with the longitudinal axis of the test sample, and ensure that the fluid port 603 is centered over the pre-marked dose location on the test sample. The center nAMF droplet applied to the test sample should now be visible through the fluid port 603 at the dose location on the test sample.
[0293] c) After it is properly positioned over the test sample, gently rest the strike-through sheet 601 over / on the test sample.
[0294] d) using a pipette with adjustable volume, 2.0mL nAMF is dispensed into the fluid well 608 in the permeable plate 601. Fluid is dispensed smoothly without splashing along the tapered portion of the wall of the fluid well 608 in 3 seconds or less. When fluid enters port 603, the electrical connection between the electrodes 604 will be established by the fluid and the circuit interval timer will start timing. When the fluid is collected by the test sample, the electrical connection between the electrodes 604 will be disconnected and the circuit interval timer will stop timing. After the circuit interval timer stops timing, a stopwatch type timer is quickly started, which is set to sound an alarm after 2 minutes, during which the permeable plate is placed on the test sample. Rapidly record the first acquisition time (ACQ-1) displayed on the circuit interval timer, accurate to 0.1 seconds.
[0295] e) After 2 minutes had passed, the first interface free fluid (IFF-1) was measured as follows.
[0296] i) Place the IFF rubber mat on a horizontal work surface. Weigh the first single fresh sheet of filter paper (IFF-1 filter paper sheet) used for this IFF-1 measurement and record the weight as IFF-1 初始. Place the IFF-1 filter paper sheet on top of the IFF rubber mat so that it is squared and centered. Quickly lift and move the strike-through plate 601 from the test sample to the IFF-1 filter paper sheet so that the plate is squared and centered on the filter paper, and immediately start a stopwatch type timer set to alarm in 8 minutes.
[0297] ii) After 10 seconds on the 8 minute timer, remove the strikethrough plate from the IFF-1 filter paper and gently place it back onto the test sample, positioned exactly as before.
[0298] iii) Within the next 10 seconds, measure the mass of the IFF-1 filter paper to the nearest 0.0001 g and record it as IFF-1 最终 .
[0299] 6) The second acquisition time (ACQ-2) of the test sample was measured as follows.
[0300] a) After 8 minutes have passed according to the previously set timer, use an adjustable volume pipette to dispense a 4.0 mL dose of nAMF into the fluid well 608 in the permeable plate 601. Dispense the fluid smoothly without splashing along the tapered portion of the wall of the fluid well 608 in 3 seconds or less. After the circuit interval timer stops timing, quickly start a stopwatch type timer set to sound an alarm after 2 minutes, during which time the permeable plate is placed on the test sample. Quickly record the second acquisition time (ACQ-2) displayed on the circuit interval timer, accurate to 0.1 seconds.
[0301] b) After 2 minutes had passed, the second interface free fluid (IFF-2) was measured as follows.
[0302] i) Place the IFF rubber mat on a horizontal work surface. Weigh the second single fresh sheet of filter paper used for this IFF-2 measurement (IFF-2 filter paper sheet) and record the weight as IFF-2 初始 . Place the IFF-2 filter paper sheet on top of the IFF rubber mat so that it is square and centered. Quickly lift and move the strike-through plate 601 from the test sample to the IFF-2 filter paper sheet so that the plate is square and centered on the filter paper, and immediately start a stopwatch type timer set to alarm in 8 minutes.
[0303] ii) After 10 seconds on the 8 minute timer, remove the strikethrough plate from the IFF-2 filter paper and gently place it back onto the test sample, positioned exactly as before.
[0304] iii) Within the next 10 seconds, measure the mass of the IFF-2 filter paper to the nearest 0.0001 g and record it as IFF-2 最终 .
[0305] 7) The third acquisition time (ACQ-3) was measured as follows.
[0306] a) After 8 minutes have passed according to the previously set timer, a 2.0 mL dose of nAMF is dispensed into the fluid well 608 in the permeable plate 601 using an adjustable volume pipette. The fluid is dispensed smoothly without splashing along the tapered portion of the wall of the fluid well 608 in 3 seconds or less. After the circuit interval timer stops timing, a stopwatch type timer is quickly started, set to sound an alarm after 2 minutes, during which time the permeable plate is placed on the test sample. The third acquisition time (ACQ-3) displayed on the circuit interval timer is quickly recorded to the nearest 0.1 second.
[0307] b) After 2 minutes had passed, the second interface free fluid (IFF-3) was measured as follows.
[0308] i) Place the IFF rubber mat on a horizontal work surface. Weigh the third single fresh sheet of filter paper used for this IFF-3 measurement (IFF-3 filter paper sheet) and record the weight as IFF-3 初始 . Place the IFF-3 filter paper sheet on top of the IFF rubber mat so that it is square and centered. Quickly lift and move the strike-through plate 601 from the test sample to the IFF-3 filter paper sheet so that the plate is square and centered on the filter paper, and immediately start a stopwatch type timer set to alarm in 8 minutes.
[0309] ii) After 10 seconds on the 8 minute timer, remove the strike through plate from the IFF-3 filter paper sheet and secure it on its side so that the bottom side of the plate does not contact the work surface.
[0310] iii) Within the next 10 seconds, measure the mass of the IFF-3 filter paper to the nearest 0.0001 g and record it as IFF-3 最终 .
[0311] 8) Measure the surface free fluid (SFF) as follows. Weigh the first clean stack of 5 fresh filter paper pieces for this SFF measurement (SFF filter paper stack) and record the weight as SFF 初始 . After 8 minutes have passed according to the timer set previously, the SFF filter paper stack is placed on top of the wearer-facing side of the test sample so that it is centered over the dosing location. The strike-through plate 601 is now placed on top of the SFF filter paper stack so that the bottom side of the plate is centered on the filter paper stack and a stopwatch type timer is immediately started, set to alarm in 10 seconds. After 10 seconds have passed, the strike-through plate 601 is removed from the filter paper stack and set aside. The mass of the SFF filter paper stack is measured to the nearest 0.0001 g and recorded as SFF 最终 . Continue immediately to the next step.
[0312] 9) Measure total rewet as follows. Weigh the second clean stack of 5 fresh filter paper sheets used for this REWET measurement (REWET filter paper stack) and record the weight as REWET 初始 . Place the rewet filter paper stack on top of the wearer-facing side of the test sample so that it is centered over the dosing location. Now place the rewet weight assembly on top of the rewet filter paper stack so that the weight is centered on the stack and immediately start a stopwatch type timer set to alarm in 30 seconds. After 30 seconds have passed, remove the rewet weight assembly and measure the mass of the rewet filter paper stack to the nearest 0.0001 g and record as REWET 最终 .
[0313] 10) Before testing the next sample, discard the test sample and thoroughly clean and then dry the strike-through plate 601 including the fluid wells 608, fluid ports 603, longitudinal fluid channels 607 and bottom surface.
[0314] 11) For each of the measured parameters, the following calculations are performed. 最终 Subtract IFF-1 初始 Calculate IFF-1 and record to the nearest 0.0001 g. 最终 Subtract IFF-2 初始 Calculate IFF-2 and record to the nearest 0.0001 g. 最终 Minus IFF-3 初始 IFF-3 is calculated and recorded to the nearest 0.0001 g. 最终 Minus SFF 初始 SFF is calculated and recorded to the nearest 0.0001 g. 最终 Minus REWET 初始 The total back permeation was calculated and recorded to the nearest 0.0001 g.
[0315] The entire procedure was repeated for a total of three replicate test samples. The reported value for each of the parameters is the average of three individually recorded measurements for each acquisition time to 0.1 seconds (ACQ-1, ACQ-2, and ACQ-3), interface free fluid to 0.0001 g (IFF-1, IFF-2, and IFF-3), surface free fluid to 0.0001 g (SFF), and total back permeation to 0.0001 g.
[0316] Preparation of new artificial menstrual fluid (nAMF)
[0317] New artificial menstrual fluid (nAMF) is a mixture of defibrillated sheep blood, phosphate buffered saline solution, and a mucus component. nAMF is prepared so that it has a viscosity between 7.40 and 9.00 centipoise at 23°C.
[0318] The viscosity of nAMF is measured using a low viscosity rotational viscometer (a suitable instrument is a Brookfield DV2T equipped with a Brookfield UL adapter purchased from AMETEK Brookfield, Middleboro, MA, or an equivalent instrument). A spindle of appropriate size within the viscosity range is selected and the instrument is operated and calibrated according to the manufacturer. The measurement is carried out at 23°C ± 1°C and at 60rpm. The results are reported to the nearest 0.01 centipoise.
[0319] The reagents required for nAMF preparation include: defibrinated sheep blood with a packed cell volume of 38% or greater (collected under sterile conditions and purchased from Cleveland Scientific, Inc., Bath, OH, or a suitable equivalent source), gastric mucin with a viscosity target of 3 to 4 centistokes when prepared as a 2% aqueous solution (sterile, crude form, purchased from American Laboratories, Inc., Omaha, NE, or a suitable equivalent source), anhydrous disodium hydrogen phosphate (reagent grade), sodium chloride (reagent grade), sodium dihydrogen phosphate monohydrate (reagent grade), sodium benzoate (reagent grade), benzyl alcohol (reagent grade), and distilled water, each purchased from VWR International or a suitable equivalent source.
[0320] The phosphate buffered saline solution consists of two separately prepared solutions (solution A and solution B). To prepare 1 L of solution A, add 1.38 ± 0.005 g of sodium dihydrogen phosphate and 8.50 ± 0.005 g of sodium chloride to a 1000 mL volumetric flask and add distilled water to the flask. Mix thoroughly. To prepare 1 L of solution B, add 1.42 ± 0.005 g of sodium dihydrogen phosphate and 8.50 ± 0.005 g of sodium chloride to a 1000 mL volumetric flask and add distilled water to the flask. Mix thoroughly. To prepare approximately 200 mL of phosphate buffered saline solution, add 49.50 g ± 0.10 g of solution A and 157.50 g ± 0.10 g of solution B to a bottle of sufficient size with a well-sealed lid. Then add 1.0 g of sodium benzoate and 1.60 g of benzyl alcohol to the bottle along with a stirring bar and set aside.
[0321] The mucus component of nAMF is a mixture of phosphate buffered saline solution and gastric mucin. The amount of gastric mucin added to the mucus component directly affects the final viscosity of the nAMF prepared. In order to determine the amount of gastric mucin required for obtaining nAMF within the target viscosity range (7.4 centipoise to 9.0 centipoise at 23 ℃ and 60rpm), 3 batches of nAMF with different amounts of gastric mucin were prepared in the mucus component, and then the required accurate amount was obtained by interpolation from the concentration to viscosity curve using the least squares linear fit through three points. The successful range of gastric mucin is usually 13 grams to 15 grams of nAMF per 400mL batches, but this can vary significantly based on the supplier, age and batch (production batch) of mucin.
[0322] To prepare about 200 mL of the mucus component, a predetermined amount of gastric mucin is added to a bottle containing the previously prepared phosphate buffer solution, and then a lid is applied. The bottle is placed on a wrist-shaking oscillator for 5 minutes at maximum speed. After 5 minutes, the flask of the mucus component is taken out from the wrist-shaking oscillator and placed on a magnetic stirring plate. Stir for at least 2 hours until there are no mucin lumps, then remove the stirring bar from the flask. Using a homogenizer, the mucus component is blended at 10,000 rpm for 5 minutes. A suitable homogenizer is a T18 Ultra-Turrax equipped with a S18N-19G dispersion tool (19 mm stator diameter, 12.7 mm rotor diameter, and a gap of 0.4 mm between the rotor and the stator), both of which can be purchased from IKAWorks, Inc, Wilmington, NC, or a suitable equivalent source. After the final mixing step, measure and record the viscosity of the mucus component to the nearest 0.01 centipoise using a viscometer with a UL adapter at 23°C ± 1°C and 20 rpm. Ensure that the viscosity of the prepared mucus component is within the target range of 9.0 centipoise to 11.0 centipoise.
[0323] nAMF is a 50:50 mixture of mucus component and sheep blood. Make sure the temperature of the sheep blood and mucus component is 23°C ± 1°C. To prepare approximately 400 mL of nAMF, add 200 g of mucus component to a glass bottle with a capacity of at least 500 mL. Now add 200 g of sheep blood to the bottle along with a stirring bar. Mix on a magnetic stirring plate until well combined. Make sure the viscosity of the prepared nAMF is within the target range of 7.4 centipoise to 9.0 centipoise when measured using a viscometer with a UL adapter at 23°C ± 1°C and 60 rpm. If the viscosity is too high, the viscosity can be adjusted by adding the previously prepared phosphate buffered saline solution in 0.5 g increments, followed by stirring for 2 minutes, and then rechecking the viscosity until the target range is reached.
[0324] Qualified nAMF should be refrigerated at 4°C unless intended for immediate use. After preparation, nAMF may be stored in an airtight container at 4°C for up to 48 hours. Prior to testing, nAMF must be brought to 23°C ± 1°C. After testing is complete, discard any unused portion.
[0325] ***
[0326] The dimensions and values disclosed herein are not to be understood as being strictly limited to the exact numerical values cited. Instead, unless otherwise indicated, each such dimension is intended to mean both the stated value and a functionally equivalent range around that value. For example, a dimension disclosed as "40 mm" is intended to mean "approximately 40 mm".
[0327] Unless expressly excluded or otherwise limited, each document cited herein, including any cross-referenced or related patent or application, is incorporated herein by reference in its entirety. Citation of any document is not an admission that it is prior art to any of the present invention disclosed or claimed herein, or that it, by itself or in combination with any one or more references, proposes, suggests, or discloses any such invention. In addition, to the extent that any meaning or definition of a term in this invention conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this invention shall govern.
[0328] Although specific embodiments of the present invention have been illustrated and described, it will be apparent to those skilled in the art that various other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended that all such changes and modifications within the scope of the present invention be covered in the appended claims.
[0329] Based on the above description, the following non-limiting embodiments are contemplated. Any of these examples and others may be claimed in whole or in part based on the disclosure herein in one or more subsequent non-provisional patent applications:
Claims
1. A feminine sanitary pad (10), the feminine sanitary pad having a longitudinal axis oriented along the y direction, a transverse axis oriented along the x direction and perpendicular to the longitudinal axis, and a pad thickness measured along the z direction orthogonal to the longitudinal axis and the transverse axis, and comprising a liquid permeable top sheet (20), a fibrous fluid management layer (30) located below the top sheet, an absorbent structure (40) located below the fluid management layer, and a bottom sheet (50) located below the absorbent structure, the top sheet comprising a single fibrous nonwoven web, in: The fibrous nonwoven web comprises bicomponent short topsheet fibers, wherein: The topsheet fibers have an average denier of 3.0 to 5.0; The topsheet fibers have a sheath-core bicomponent configuration, wherein the sheath component comprises polyethylene (PE) and the core component comprises polyethylene terephthalate (PET), the weight ratio of PE to PET being 40:60 to 60:40; and The topsheet fibers comprise a blend of intermixed hydrophilic fibers and hydrophobic fibers in a weight ratio of hydrophilic fibers to hydrophobic fibers of 30:70 to 70:30, more preferably 35:65 to 65:35, and even more preferably 40:60 to 60:40, wherein the hydrophilicity of the hydrophilic fibers is affected by applying a surface treatment composition; and The fibrous nonwoven web includes a plurality of interfiber bonds randomly distributed within the fibrous nonwoven web along the x-direction, the y-direction, and the z-direction, wherein the interfiber bonds exist where the sheaths of adjacent fibers are melt-bonded together without compression.
2. A feminine sanitary pad according to claim 1, wherein the fluid management layer (30) comprises carded staple fibers, the carded staple fibers comprising absorbent fibers of regenerated cellulose accounting for 10% to 60% by weight of the fluid management layer, bicomponent reinforcing fibers accounting for 25% to 70% by weight of the fluid management layer, and elastic fibers accounting for 15% to 70% by weight of the fluid management layer.
3. The feminine sanitary pad according to claim 2, wherein the reinforcing fiber has a sheath-core configuration, wherein the core component comprises PET and the sheath component comprises PE.
4. The feminine hygiene pad according to any one of claims 2 or 3, wherein the elastic fiber is 4 to 15 dtex, or more preferably 5 to 12 dtex, or even more preferably 6 to 10 dtex.
5. The feminine hygiene pad according to claim 4, wherein the elastic fiber comprises a polymer selected from the group consisting of polypropylene (PP), polyethylene (PE), polyethylene terephthalate (PET), and combinations thereof.
6. The feminine hygiene pad according to any one of the preceding claims, wherein the fluid management layer comprises a plurality of randomly distributed inter-fiber bonds, wherein adjacent fibers are melt-bonded together without compression.
7. A feminine sanitary pad (10), the feminine sanitary pad having a longitudinal axis oriented along the y direction, a transverse axis oriented along the x direction and perpendicular to the longitudinal axis, and a pad thickness measured along the z direction orthogonal to the longitudinal axis and the transverse axis, and comprising a liquid permeable top sheet (20), a fibrous fluid management layer (30) located below the top sheet, an absorbent structure (40) located below the fluid management layer, and a bottom sheet (50) located below the absorbent structure, the top sheet comprising a single fibrous nonwoven web, in: The fibrous nonwoven web comprises bicomponent short topsheet fibers, wherein: The topsheet fibers have an average denier of 3.0 to 5.0; The topsheet fibers have a sheath-core bicomponent configuration, wherein the sheath component comprises polyethylene (PE) and the core component comprises polyethylene terephthalate (PET), the weight ratio of PE to PET being 40:60 to 60:40; and A major weight fraction of the fibrous nonwoven web, and preferably all, are hydrophobic; and The fibrous nonwoven web includes a plurality of interfiber bonds randomly distributed within the fibrous nonwoven web along the x-, y-, and z-directions, wherein the interfiber bonds exist where the sheaths of adjacent fibers are melt-bonded together without compression.
8. A feminine sanitary pad according to claim 7, wherein the fluid management layer (30) comprises carded staple fibers, the carded staple fibers comprising absorbent fibers of regenerated cellulose accounting for 10% to 60% by weight of the fluid management layer, bicomponent reinforcing fibers accounting for 25% to 70% by weight of the fluid management layer, and elastic fibers accounting for 15% to 70% by weight of the fluid management layer.
9. The feminine hygiene pad according to claim 8, wherein the absorbent fibers are from 1 to 7 dtex, or more preferably from 1.4 to 6 dtex, or even more preferably from 1.7 to 5 dtex.
10. The feminine hygiene pad according to claim 8, wherein the absorbent fibers are 0.6 to 2.4 dtex, more preferably 0.9 to 2.1 dtex, even more preferably 1.1 to 1.9 dtex, and most preferably 1.3 to 1.7 dtex.
11. The feminine hygiene pad according to any one of claims 8 to 10, wherein the reinforcing fibers are from 1.0 to 6 dtex, more preferably from 1.5 to 5 dtex, or even more preferably from 2.0 to 4 dtex.
12. A feminine hygiene pad according to any one of claims 8 to 11, wherein the reinforcing fiber has a sheath-core configuration, wherein the core component comprises PET and the sheath component comprises PE.
13. The feminine hygiene pad according to any one of claims 8 to 12, wherein the fluid management layer comprises a plurality of randomly distributed inter-fiber bonds, wherein adjacent fibers are melt-bonded together without compression.
14. A feminine sanitary pad according to any of the preceding claims, wherein the single fiber nonwoven web of the top sheet comprises less than 10%, more preferably less than 5%, and even more preferably less than 1% by weight of any combination of cotton fibers, other plant fibers, rayon fibers, or monocomponent fibers comprising polyester or polyamide.
15. A feminine sanitary pad according to any of the preceding claims, wherein the single fibrous nonwoven web of the top sheet comprises less than 50%, more preferably less than 35%, and even more preferably no more than 25% of its total wearer-facing surface area that has been mechanically deformed along the z-direction.