Surface-treated silica powder, resin composition, and dispersion
By setting a physical adsorption layer of silane coupling agent on the surface of silica particles, the problems of insufficient dispersion and viscosity stability in the resin are solved, and efficient filling and stability of semiconductor packaging materials are achieved, which is suitable for high-density installation purposes.
Patent Information
- Application Number
- CN202380024121.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-16
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing technology, the dispersion and viscosity stability of silica powder in resin are insufficient, resulting in a mismatch in linear expansion coefficient of semiconductor packaging materials, prone to cracks, and insufficient filling amount.
By setting a physical adsorption layer of silane coupling agent on the surface of silica particles, the ratio of chemical binding to physical adsorption is controlled below 0.7, blocking reactive hydroxyl groups, and improving the viscosity characteristics and time stability of the resin.
The resin composition has excellent viscosity characteristics and time stability, is suitable as a filling material for high-density mounting, and enhances the filling performance of semiconductor packaging materials.
Smart Images

Figure BDA0005014782570000121 
Figure BDA0005014782570000131 
Figure BDA0005014782570000132
Abstract
Description
Technical Field
[0001] The present invention relates to a surface-treated silica powder, a resin composition, and a dispersion that can be suitably used as a filler for semiconductor encapsulation materials, liquid crystal sealants, films, and the like. Background Art
[0002] In recent years, as electronic devices have become more high-performance, smaller and lighter, the form of semiconductor packages installed has also been moving towards high integration, high density and thinness. For the practical application of such semiconductor packages, it is essential to develop packaging materials that are suitable for the design of integrated circuits while designing the integrated circuits.
[0003] For example, the bottom filler filled between the semiconductor chip and the wiring substrate mainly adopts epoxy resin, but epoxy resin, semiconductor chip and wiring substrate each have different linear expansion coefficients. Therefore, if the connection part cannot absorb stress, cracks may appear in the connection part. In order to suppress the occurrence of such cracks, fillers with smaller linear expansion coefficients such as silica are dispersed in the bottom filler. At this time, in order to suppress the linear expansion coefficient of the packaging material, it is necessary to increase the filling amount of the low expansion rate filler. In addition, the bottom filler filled with the filler needs to have low viscosity immediately after filling, and stability over time without increasing viscosity over time after filling.
[0004] In order to increase the filling amount of the filler, a hydrophilic dry silica powder having excellent dispersibility, a small dispersed particle size, and a narrow particle size distribution during dispersion has been proposed (Patent Document 1). However, the silica powder described in Patent Document 1 has a small dispersed particle size, thereby causing a viscosity-increasing effect on the resin composition. Since the viscosity of the resin composition filled with the silica powder increases, there is a possibility that a sufficient filling amount cannot be obtained.
[0005] In addition, a method for improving affinity with resin by surface treating silica particles with silicon compounds has been proposed (e.g., Patent Document 2). It is known that the silica particles described in Patent Document 2 can achieve low viscosity and high fluidity when filled with resin while improving the storage stability of the silica particles themselves by uniformly surface treating with silicon compounds to reduce the silicon compounds that are not bound to the particle surface. However, although the affinity with resin can be improved by surface treatment, there is still the problem that the reactive hydroxyl groups remaining on the particle surface will act on the resin over time, thereby increasing viscosity and reducing fluidity.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2014-152048
[0009] Patent Document 2: International Publication No. 2015 / 119283 Summary of the invention
[0010] Problems to be solved by the invention
[0011] Therefore, an object of the present invention is to provide a surface-treated silica powder having excellent filling properties and stability over time. More specifically, by improving affinity with resin and providing a physically adsorbed layer of a silane coupling agent on the surface of the silica powder, a surface-treated silica powder capable of obtaining a resin composition having high viscosity characteristics and stability over time is provided.
[0012] Means used to solve problems
[0013] The inventors have found that, by chemically bonding a silane coupling agent to the surface of the silica particles and intentionally allowing a large amount of the silane coupling agent component that is not chemically bonded to exist on the surface of the silica particles, the resin composition to which the surface-treated silica powder of the present invention is added can have both excellent viscosity characteristics and stability over time because the reactive hydroxyl groups on the surface of the silica particles are physically shielded from the resin.
[0014] That is, the surface-treated silica powder of the present invention is a surface-treated silica powder obtained by surface-treating silica particles with a silane coupling agent, and the amount of the silane coupling agent component chemically bonded to the surface of the silica particles per unit specific surface area of the silica particles is set to C (pieces / nm 2 ), the amount of the silane coupling agent component present per unit specific surface area of the silica particles in the surface treated silica powder is set to T (pieces / nm 2 ), the ratio (C / T) is less than 0.7.
[0015] Effects of the Invention
[0016] The surface-treated silica powder of the present invention, in addition to the silane coupling agent chemically bonded to the surface of the silica particles, also has a large amount of coupling agents physically adsorbed on the surface of the silica particles, so the resin composition added with the surface-treated silica powder is not affected by the reactive hydroxyl groups remaining on the surface of the silica particles, and can have excellent viscosity characteristics and stability over time. Therefore, it is suitable as a filling material for semiconductor packaging materials and semiconductor mounting adhesives. In particular, it can be suitably used as a filling material for high-density mounting resins. DETAILED DESCRIPTION
[0017] Hereinafter, the surface-treated silica powder of the present invention will be described in detail based on embodiments.
[0018] [Surface treated silica powder]
[0019] The surface treated silica powder of the present invention is a surface treated silica powder obtained by surface treating silica particles with a silane coupling agent, wherein the amount of the silane coupling agent component chemically bonded to the surface of the silica particles per unit specific surface area of the silica particles is set to C (unit / nm 2 ), the amount of the silane coupling agent component present per unit specific surface area of the silica particles in the surface treated silica powder is set to T (pieces / nm 2 ), the ratio (C / T) is less than 0.7.
[0020] Here, if C / T is 0.7 or less, the silane coupling agent component physically adsorbed on the surface of the silica particles can physically separate the reactive hydroxyl groups remaining on the surface of the silica particles from the resin, thereby being able to have both excellent viscosity characteristics and stability over time. In particular, C / T is preferably 0.6 or less. When C / T exceeds 0.7, the reactive hydroxyl groups of the silica particles react with the resin, and the stability over time tends to decrease.
[0021] In addition, the amount T of the silane coupling agent component on the surface of the surface-treated silica powder is preferably 2.0 to 22.0 particles / nm 2 , more preferably 4.0 to 18.0 per nm 2 .
[0022] Here, if the amount T of the silane coupling agent component is 2.0 to 22.0 pieces / nm 2 If the number of reactive hydroxyl groups on the surface of silica particles is less than 2.0 / nm, the reactive hydroxyl groups on the surface of silica particles can be fully isolated from the resin. 2 , the affinity with organic resin tends to decrease. In addition, if it exceeds 22.0 / nm 2 , the silane coupling agent fills the inter-particle spaces between the silica particles, and the dispersibility during filling tends to decrease.
[0023] The BET specific surface area of the surface treated silica powder is preferably 1 to 100 m 2 / g, more preferably 2 to 80 m 2 / g, more preferably 5 to 50 m 2 / g.
[0024] Here, if the BET specific surface area of the surface-treated silica powder is 1 to 100 m 2 / g, the resin composition can maintain a low viscosity even if a large amount of surface-treated silica powder is filled in the resin.
[0025] Here, if the BET specific surface area is less than 1 m 2 / g, although the viscosity of the resin composition using the surface treated silica powder after surface treatment is low, the silica particle size is large relative to the gap, and as a result, voids will appear when penetrating the gap, which may lead to poor molding. In other words, it may not be possible to obtain sufficiently narrow gap permeability. If the BET specific surface area exceeds 100m 2 / g, the viscosity of the resin composition is high and a sufficient filler loading may not be obtained.
[0026] Furthermore, the amount of coarse particles in the surface-treated silica powder can be calculated using the following formula: 90 To express.
[0027] V 90 ={(D 90 -D 50 ) / D 50}×100
[0028] D 50 : Cumulative 50 volume % particle size of volume-based particle size distribution obtained by laser diffraction scattering method
[0029] D 90 : Cumulative 90% volume particle size of volume-based particle size distribution obtained by laser diffraction scattering method
[0030] Here, V 90 It is preferably 10 or more and less than 100, more preferably 10 to 95, and even more preferably 20 to 90. 90 When V is greater than 10 and less than 100, good gap penetration can be obtained when the resin composition penetrates into the gap. 90 When it is 100 or more, there are many coarse particles, and voids will appear when penetrating the gaps, which may cause poor molding. When it is less than 10, industrial production may be difficult.
[0031] [use]
[0032] The use of the surface-treated silica powder of the present invention is not particularly limited. For example, it can be used as a filling material for semiconductor packaging materials or semiconductor mounting adhesives, a filling material for die attach films or die attach pastes, or a filling material for resin compositions such as insulating films of semiconductor packaging substrates. In particular, the surface-treated silica powder obtained by the present invention can be suitably used as a filling material for a high-density mounting resin composition.
[0033] Furthermore, the surface treated silica powder obtained by the present invention can also be used as abrasive grains for CMP (Chemical Mechanical Polishing) abrasives, abrasive grains for grindstones for grinding, etc., toner additives, additives for liquid crystal sealing materials, dental filling materials or inkjet coating agents, etc.
[0034] [Method for producing surface-treated silicon dioxide powder]
[0035] Next, the method for producing the surface-treated silica powder of the present invention will be described.
[0036] By adding a silane coupling agent to a silica powder, mixing, and heat-treating, the surface of the silica particles reacts with a portion of the coupling agent (chemically bonded), thereby obtaining a treated powder in which both a silane coupling agent component chemically bonded to the surface of the silica particles and a silane coupling agent component not chemically bonded exist. The obtained treated powder is dried and by-products are removed to obtain a surface-treated silica powder. This is described in detail below.
[0037] <Silicon dioxide powder>
[0038] The silicon dioxide powder used in the present invention preferably has a BET specific surface area of 1 to 100 m 2 / g、V 90 The hydrophilic silica powder has a value of 10 or more and less than 100.
[0039] In addition, as silica powder, silica powder containing silica particles surface-treated with a surface treatment agent other than a silane coupling agent (such as other additives such as hexamethyldisilazane) can also be used. That is, by using silica powder surface-treated with a surface treatment agent, a surface-treated silica powder with various surface properties can be obtained. For example, a surface-treated silica powder composed of a trimethylsilyl group and an epoxy group can be easily obtained. The surface-treated silica powder composed of different functional groups can control the affinity with the resin when filled into the resin, and a resin composition having excellent viscosity characteristics and stability over time can be obtained.
[0040] <Silane coupling agent>
[0041] Examples of the silane coupling agent include a silane coupling agent represented by the following formula (1).
[0042] R n -Si-X (4-n) (1)
[0043] However, in the above formula (1), R is an organic group having 1 to 18 carbon atoms, X is a hydrolyzable group, and n is an integer of 1 to 3.
[0044] In addition, as the above-mentioned X, alkoxy groups having 1 to 3 carbon atoms such as methoxy, ethoxy and propoxy and / or halogen atoms such as chlorine atoms can be listed, among which methoxy and / or ethoxy are preferred. In addition, when n is 1 or 2, a plurality of Xs may be the same or different, preferably the same. In addition, n is an integer of 1 to 3, preferably 1 or 2, and particularly preferably 1.
[0045] Examples of the silane coupling agent represented by the formula (1) include methyltrimethoxysilane, methyltriethoxysilane, hexyltrimethoxysilane, decyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxytrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane. 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N,N-dimethyl-3-aminopropyltrimethoxysilane, N,N-diethyl-3-aminopropyltrimethoxysilane, 4-phenyltrimethoxysilane, etc.
[0046] <Surface treatment agent (other additives)>
[0047] In addition, in addition to the silane coupling agent, a surface treatment agent selected from at least one of silicone oil, siloxanes and / or silazanes can also be added. The surface treatment agent can be added simultaneously with the silane coupling agent, or the silane coupling agent can be added after the surface treatment agent is added. Further, the surface treatment agent can also be added after the silane coupling agent is added. Thus, a surface treated silica powder with various surface properties can be obtained. For example, a surface treated silica powder composed of a trimethylsilyl group and an epoxy group can be easily obtained.
[0048] In the case of silicone oil, the amount of the surface treatment agent used is preferably 0.05 to 80 parts by weight, more preferably 0.1 to 60 parts by weight, and most preferably 1 to 20 parts by weight, relative to 1 part by weight of silica powder. Similarly, in the case of siloxanes, it is preferably 0.001 to 40 parts by weight, more preferably 0.003 to 30 parts by weight, and most preferably 0.005 to 20 parts by weight, relative to 1 part by weight of silica powder. Similarly, in the case of silazanes, it is preferably 0.001 to 40 parts by weight, more preferably 0.003 to 30 parts by weight, and most preferably 0.005 to 20 parts by weight, relative to 1 part by weight of silica powder.
[0049] <Mixed>
[0050] The silica powder and the silane coupling agent are mixed by a known method. For example, the silica powder is added to a mixing container, and a predetermined amount of the silane coupling agent is added by dripping, spraying, etc., while the silica powder is fluidized by shaking or stirring. For example, the silica powder is added to a container, and stirring is started by rotating a stirring blade. The silane coupling agent is added thereto using a peristaltic pump. The addition speed can be appropriately changed according to the amount added.
[0051] After adding the silane coupling agent, preferably continue stirring for more than 10 minutes. By continuing stirring, the silane coupling agent can be uniformly attached to the surface of the silica powder. Thus, the silane coupling agent physically adsorbed on the surface of the surface-treated silica powder can be reduced.
[0052] Examples of mixing containers include Henschel mixers and Loedige mixers that are equipped with stirring blades and mixing blades, air mixers that mix air flows by air, and V-type mixers, double cone mixers, and swing mixers that mix by rotating or shaking the container body.
[0053] <Heat Treatment>
[0054] By performing the heat treatment, a portion of the added silane coupling agent reacts with the surface of the silica particles (i.e., chemically bonded), while the remaining silane coupling agent remains on the surface of the silica particles without chemical bonding (i.e., physically adsorbed). As for the temperature of the heat treatment, if the temperature is low, the reaction proceeds slowly, resulting in reduced production efficiency, while if the temperature is high, the decomposition and rapid polymerization reaction of the silane coupling agent and the surface treatment agent promotes the formation of flocculation. Therefore, depending on the surface treatment agent used, it is usually carried out at a temperature of 25 to 300°C, preferably 40 to 250°C.
[0055] The heat treatment time can be appropriately determined according to the reaction properties of the surface treatment agent used, etc. Usually, sufficient reaction efficiency can be obtained within 1 hour or more and 500 hours.
[0056] In addition, when the heating treatment can be performed in the mixing container used for mixing, the mixed powder can be directly subjected to the heating treatment in the device.
[0057] <Drying treatment>
[0058] The drying temperature is not particularly limited, but when the temperature is high, the silane coupling agent component that is not chemically bound (physical adsorption) will volatilize and be removed from the silica powder, which is not ideal; when the temperature is low, the by-products cannot be fully removed. Therefore, the drying temperature is preferably 25 to 200°C, more preferably 25 to 180°C, and further preferably 25 to 150°C. By drying at 25°C or above, the by-products generated when the silane coupling agent reacts with the surface of the silica particles can be fully removed.
[0059] The device used for drying is not particularly limited, and a conventionally known drying device can be used. In addition, when drying can be performed in a reaction vessel used in the heat treatment, the treated powder can be directly dried in the device.
[0060] The pressure in the device during drying is preferably a pressure above atmospheric pressure. Specifically, it is preferably above 1000 hPa. By drying under a pressure above atmospheric pressure, unreacted silane coupling agent can be fully removed. If it is above 1000 hPa, the physically adsorbed silane coupling agent component will not volatilize, and by-products can be fully removed.
[0061] The drying time is not particularly limited and can be appropriately selected according to the drying conditions such as drying temperature and pressure, but is generally about 1 to 48 hours, thereby obtaining a surface-treated silica powder from which by-products have been removed.
[0062] [Dispersion]
[0063] The surface-treated silica powder of the present invention can be dispersed in a liquid solvent to form a dispersion. The solvent used to disperse the surface-treated silica powder is not particularly limited as long as it is a solvent that easily disperses the surface-treated silica powder.
[0064] As the solvent, for example, organic solvents such as water, alcohols, ethers and ketones can be used. As the alcohols, for example, methanol, ethanol and 2-propanol can be cited. As the solvent, a mixed solvent of water and any one or more of the above organic solvents can also be used. In addition, in order to improve the stability and dispersibility of the surface-treated silica powder, various additives such as dispersants such as surfactants, thickeners, wetting agents, defoamers or acidic or alkaline pH regulators can be added. In addition, the pH of the dispersion is not limited.
[0065] As the use of the dispersion, there are examples of filling semiconductor packaging materials and semiconductor mounting adhesives. If it is a dispersion, that is, surface-treated silica powder pre-dispersed in a solvent, it is easy to disperse in a resin. For example, by mixing the resin and the dispersion and then removing the solvent, an underfill with a good filler dispersion can be easily prepared.
[0066] [Resin composition]
[0067] There is no particular limitation on the type of resin to be used with the surface-treated silica powder in order to prepare the resin composition of the present invention. The type of resin can be appropriately selected according to the desired application, and examples thereof include epoxy resins, acrylic resins, silicone resins, olefin resins, polyimide resins and / or polyester resins.
[0068] The resin composition may be produced by appropriately adopting a known method, and the surface-treated silica powder and various resins and other components may be mixed as needed.
[0069] When the dispersion of the present invention is mixed with a resin, a resin composition having a good dispersion state of the silica powder in the resin can be obtained compared to the case where the silica powder in a dry state is mixed with the resin. A good particle dispersion state means that there are fewer agglomerated particles in the resin composition. Therefore, the viscosity characteristics and gap permeability of the resin composition containing the surface-treated silica powder of the present invention as a filler can be further improved.
[0070] The resin composition can be used in semiconductor encapsulating materials and semiconductor mounting adhesives. The resin composition containing the surface-treated silica powder can suppress the linear expansion coefficient and is therefore suitable for such applications.
[0071] [Summarize]
[0072] As can be understood from the above description, the surface-treated silica powder involved in the first aspect of the present invention is characterized in that the surface-treated silica powder is a surface-treated silica powder in which silica particles are surface-treated with a silane coupling agent, and the amount of the silane coupling agent component chemically bonded to the surface of the silica particles per unit specific surface area of the silica particles is set to C (pieces / nm 2 ), the amount of the silane coupling agent component present per unit specific surface area of the silica particles in the surface treated silica powder is set to T (pieces / nm 2 ), the ratio (C / T) is less than 0.7.
[0073] According to this surface-treated silica powder, in addition to the silane coupling agent chemically bonded to the surface of the silica particles, a large amount of physically adsorbed silane coupling agent is present, and the resin composition added with the surface-treated silica powder according to the first aspect of the present invention can have both excellent viscosity characteristics and stability over time.
[0074] The surface-treated silica powder according to the second aspect of the present invention is characterized in that, in the surface-treated silica powder according to the first aspect, the amount T of the silane coupling agent component is 2.0 to 22.0 particles / nm 2 .
[0075] The surface-treated silica powder according to the third aspect of the present invention is characterized in that, in the surface-treated silica powder according to the first aspect or the second aspect, the cumulative 50 volume% particle size (D 50 ) and cumulative 90 volume % particle size (D 90 ), the amount of coarse particles of the surface-treated silicon dioxide powder obtained according to Formula 1 (V 90 ) is greater than 10 and less than 100.
[0076] V 90 ={(D 90 -D 50 ) / D 50}×100(1)
[0077] The surface-treated silicon dioxide powder according to the fourth aspect of the present invention is characterized in that, in the surface-treated silicon dioxide powder according to any one of the first to third aspects, the BET specific surface area is 1 to 100 m 2 / g.
[0078] The resin composition according to the fifth aspect of the present invention is obtained by dispersing the surface-treated silica powder according to any one of the first to fourth aspects in a resin.
[0079] The dispersion according to the sixth aspect of the present invention is obtained by dispersing the surface-treated silica powder according to any one of the first to fourth aspects in a liquid solvent.
[0080] Example
[0081] Hereinafter, although examples in this embodiment are given and described in detail, the present invention is not limited to these examples at all.
[0082] The methods for measuring and evaluating the physical properties of the silica powder and the surface-treated silica powder are as follows.
[0083] (C / T measurement method)
[0084] 1) Surface-treated silica powder was suspended in ethanol at a concentration of 3 wt %, and the resulting suspension having a total volume of 30 mL was placed in a centrifuge tube (Violamo centrifuge tube II 50 mL manufactured by AsOne), and dispersed for 10 minutes using a desktop ultrasonic cleaner (M2800-J manufactured by Branson, output power 110 W, oscillation frequency 40 kHz. An example of an ultrasonic disperser) to obtain a dispersed slurry 1.
[0085] 2) The centrifuge tube containing the dispersed slurry 1 was placed in a centrifuge (CN-1050 manufactured by As One) and centrifuged at 5000 rpm for 30 minutes, and then the supernatant separated to the upper layer was removed to obtain a precipitate cake in the centrifuge tube (solid-liquid separation).
[0086] 3) Add ethanol to the centrifuge tube in 2) above to make the total volume 30 mL, and disperse for 10 minutes in the same manner as 1) above to obtain dispersed slurry 2.
[0087] 4) The above 2) to 3) were repeated 3 times, and the cake 1 obtained in 2) for the third time was vacuum dried at room temperature for 1 hour (molded vacuum dryer MVD-100 manufactured by As One, drying vacuum pump manufactured by As One) to obtain a washed powder.
[0088] 5) The amount of chemically bonded components C (units / nm) was calculated using the following formula: 2 ) and the amount of silane coupling agent component T (pieces / nm 2 ).
[0089] T(pcs / nm 2 ) = carbon content (wt%) of surface treated silica (i.e., unwashed powder) / 100 / 12 (atomic weight of carbon) / {number of carbon atoms in silane coupling agent - N} × Avogadro constant (atom / mol) / BET specific surface area of silica powder (m 2 / g) / 10 18
[0090] C(pcs / nm 2 ) = carbon content of washed powder (wt%) / 100 / 12 (atomic weight of carbon) / {number of carbon atoms in silane coupling agent - N} × Avogadro constant (atom / mol) / BET specific surface area of silica powder (m 2 / g) / 10 18
[0091] (wherein, the number of carbon atoms of the silane coupling agent is the number of carbon atoms in the molecular formula of the silane coupling agent used. For example, when KBM-403 manufactured by Shin-Etsu Silicone is used, the silane coupling agent has a molecular formula of C9H 20 O5Si, so the number of carbon atoms in the silane coupling agent is 9. N is the number of carbon atoms of the hydrolyzable group X of the silane coupling agent × 2. For example, when X is a methoxy group, N is 2, and when X is an ethoxy group, N is 4. Avogadro's constant is 6.02×10 23 (pcs / mol).
[0092] 6) Based on the above C and T, the ratio (C / T) of the amount T of the silane coupling agent component on the surface of the surface-treated silica powder to the amount C of the chemically bonded component is determined.
[0093] T: Total amount of silane coupling agent per unit area of surface treated silica powder
[0094] C: Amount of chemically bonded silane coupling agent per unit area of surface treated silica powder
[0095] (Carbon content)
[0096] The carbon content (weight %) was measured using a total nitrogen and total carbon measuring apparatus (SUMIGRAPH NC-22F manufactured by Sumika Analytical Center). The silica sample to be measured was 50 to 100 mg.
[0097] (BET specific surface area)
[0098] The BET specific surface area S (m2) was measured by the nitrogen adsorption BET single-point method using a specific surface area measuring device (SA-1000 manufactured by Shibata Rikagaku Co., Ltd.). 2 / g).
[0099] (Volume-based particle size distribution based on laser diffraction scattering method)
[0100] About 0.1 g of surface-treated silica powder was weighed into a 50 mL glass bottle using an electronic balance, and about 40 mL of ethanol was added. The powder was dispersed using an ultrasonic homogenizer (Sonifier 250 manufactured by Branson) at 40 W for 10 minutes. The average particle size (nm) and coefficient of variation of the surface-treated silica powder were then measured using a laser diffraction scattering particle size distribution measuring device (LS13 320 manufactured by Beckman Coulter). The average particle size (nm) described herein refers to the cumulative 50% volume particle size. The cumulative 50% volume particle size (D 50 ) and cumulative 90 volume % particle size (D 90 ). From the obtained D 50and D 90 The amount of coarse particles of the surface-treated silica powder (V 90 ).
[0101] V 90 ={(D 90 -D 50 ) / D 50}×100 (1)
[0102] (Evaluation of dispersibility of surface-treated silica powder)
[0103] 36 g of surface treated silica powder was added to a mixture of 17 g of bisphenol F epoxy resin (YDF-8170C manufactured by Nippon Steel Chemical & Material) and 7 g of amine curing agent (KARAHARD AA manufactured by Nippon Kayaku) and mixed by hand. The hand-mixed resin composition was pre-mixed using an auto-rotational mixer (manufactured by THINKY, Awatori Rentaro AR-500) (mixing: 1000 rpm, 8 minutes; defoaming: 2000 rpm, 2 minutes). The pre-mixed resin composition was stored in a constant temperature water tank at 25°C and then rolled using three rollers (BR-150HCV manufactured by Aimex, roller diameter ) and kneaded the mixture. The kneading conditions were kneading temperature of 25° C., distance between rolls of 20 μm, and kneading number of 8 times. The obtained resin composition was defoamed for 30 minutes under reduced pressure using a vacuum pump (TSW-150 manufactured by Sato Vacuum).
[0104] A rheometer (HAAKE MARS40 manufactured by Thermo Fisher Scientific) was used at a shear rate of 1 s -1 The initial viscosity (η1) and the viscosity (η2) after one day of the kneaded resin composition were measured at 25°C. In addition, the measurement temperature was 25°C, and the sensor used was C35 / 1 (cone-plate type, diameter 35 mm, angle 1°, material titanium). Here, the resin composition was stored at 25°C.
[0105] The rate of change in viscosity over time was calculated from the following formula using the viscosity (η1) at the time of preparation of the resin composition and the viscosity (η2) after one day.
[0106] Viscosity change rate over time [%] = {(η2-η1) / η1} × 100
[0107] When the viscosity change rate over time is 100% or less, the viscosity index is judged to be good, and when the viscosity change rate over time exceeds 100%, the viscosity index is judged to be poor. Here, if the viscosity index is good, it is considered that the surface-treated silica powder has excellent viscosity characteristics and stability over time.
[0108] (Gap permeability evaluation)
[0109] Two sheets of glass were overlapped to form a gap of 30 μm in advance, heated to 110° C., and the mixed resin composition prepared in (5) (during preparation) was subjected to a high temperature intrusion test. The presence or absence of flow marks was evaluated by appearance observation. When no flow marks were observed, it was determined that the gap permeability was good, and when flow marks were observed, it was determined that the gap permeability was poor. Here, if the gap permeability is good, it is considered that the surface-treated silica powder has excellent filling and viscosity characteristics.
[0110] [Example 1]
[0111] Put the silica powder A shown in Table 1 into a mixing container and start stirring. Then, with respect to 100 parts by weight of silica powder A, use a peristaltic pump (SJ-1211II-H manufactured by ATTA) to supply 1.5 parts by weight of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone). Continue stirring after supplying and mix for 15 minutes. After mixing, continue stirring, while raising the temperature from room temperature to 40°C within 20 minutes, and then maintain it at 40°C for 60 minutes. Thereafter, raise the temperature to 100°C within 60 minutes, and then maintain it at 100°C for 180 minutes to terminate the reaction process. After the reaction process is completed, cool it, maintain it at 30°C, and pass nitrogen into the container for drying to obtain surface-treated silica powder. Table 1 shows the properties of silica powder and the preparation conditions of surface-treated silica powder, and Table 2 shows the physical properties of surface-treated silica powder (the same below).
[0112] Table 1
[0113]
[0114]
[0115] Silica powder A: Silfil NSS-40D manufactured by Tokuyama Corporation
[0116] Silica powder B: Silfil NSS-24D manufactured by Tokuyama Corporation
[0117] Silica powder C: Silfil NSS-5N manufactured by Tokuyama Corporation
[0118] Silica powder D: Sunseal SS-10 manufactured by Tokuyama Co., Ltd.
[0119] Silica powder E: HMDS of Sunseal SS-10 manufactured by Tokuyama Co., Ltd.
[0120] Treated product (equivalent to TMS base 0.5 / nm 2 )
[0121] Table 2
[0122]
[0123]
[0124] [Example 2]
[0125] Put silica powder B into a mixing container and start stirring. Then, use a peristaltic pump (SJ-1211II-H manufactured by ATTA) to supply 2.5 parts by weight of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone) relative to 100 parts by weight of silica powder B. Continue stirring after supplying and mix for 15 minutes. After mixing, continue stirring while raising the temperature from room temperature to 40°C within 20 minutes, and then maintain it at 40°C for 60 minutes. Thereafter, raise the temperature to 150°C within 60 minutes, and then maintain it at 150°C for 180 minutes to terminate the reaction process. Next, prepare the surface-treated silica powder in the same manner as in Example 1 and measure it.
[0126] [Example 3]
[0127] Surface-treated silica powder was prepared and measured in the same manner as in Example 1, except that silica powder C was used instead of silica powder A and 8.0 parts by weight of KBM-403 was used as a silane coupling agent based on 100 parts by weight of silica powder C.
[0128] [Example 4]
[0129] Put the silica powder D into the mixing container and start stirring. Then, use a peristaltic pump (SJ-1211 II-H manufactured by ATTA) to supply 0.01 parts by weight of hexamethyldisilazane (SZ-31 manufactured by Shin-Etsu Silicone) relative to 100 parts by weight of silica powder D, and 0.5 parts by weight of silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone) relative to 100 parts by weight of silica powder D. Continue stirring after supplying and mix for 15 minutes. After mixing, continue stirring while raising the temperature from room temperature to 40°C within 20 minutes, and then maintain it at 40°C for 60 minutes. Thereafter, raise the temperature to 100°C within 60 minutes, and then maintain it at 100°C for 180 minutes to terminate the reaction process. After the reaction process is completed, cool it, maintain 30°C, and pass nitrogen into the container for drying to obtain surface-treated silica powder. Determine the physical properties of the obtained silica powder.
[0130] [Example 5]
[0131] Surface-treated silica powder was prepared and measured in the same manner as in Example 1, except that silica powder E was used instead of silica powder A and 0.5 parts by weight of KBM-403 was used as a silane coupling agent based on 100 parts by weight of silica powder E.
[0132] [Example 6]
[0133] Surface-treated silica powder was prepared and measured in the same manner as in Example 4, except that 0.01 parts by weight of hexamethyldisilazane (SZ-31 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder D, and 1.0 parts by weight of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder D.
[0134] [Example 7]
[0135] Surface-treated silica powder was prepared and measured in the same manner as in Example 4, except that 0.01 parts by weight of hexamethyldisilazane (SZ-31 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder D, and 2.0 parts by weight of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder D.
[0136] [Example 8]
[0137] Surface-treated silica powder was prepared and measured in the same manner as in Example 1 except that silica powder D was used instead of silica powder A and 0.5 parts by weight of a silane coupling agent (KBM-573 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of silica powder D.
[0138] [Example 9]
[0139] Surface-treated silica powder was prepared and measured in the same manner as in Example 4, except that 0.01 parts by weight of hexamethyldisilazane (SZ-31 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder D, and 0.5 parts by weight of a silane coupling agent (KBM-303 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder D.
[0140] [Example 10]
[0141] Surface-treated silica powder was prepared and measured in the same manner as in Example 4, except that 0.01 parts by weight of hexamethyldisilazane (SZ-31 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder D, and 0.5 parts by weight of a silane coupling agent (KBM-503 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder D.
[0142] [Example 11]
[0143] Surface-treated silica powder was prepared and measured in the same manner as in Example 4, except that 0.02 parts by weight of hexamethyldisilazane (SZ-31 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder D, and 0.5 parts by weight of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder D.
[0144] [Comparative Example 1]
[0145] A surface-treated silica powder was prepared and measured in the same manner as in Example 2 except that no epoxy silane coupling agent was added, the heat treatment was performed at 150° C., and the drying treatment was performed at 20 hPa and 50° C. for 1 hour.
[0146] [Comparative Example 2]
[0147] Surface-treated silica powder was prepared and measured in the same manner as in Example 1 except that 0.75 parts by weight of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of silica powder A and drying was performed at 20 hPa and 50° C. for 1 hour.
[0148] [Comparative Example 3]
[0149] Surface-treated silica powder was prepared and measured in the same manner as in Example 1 except that 0.5 parts by weight of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone) was used per 100 parts by weight of silica powder A and drying was performed at 20 hPa and 50° C. for 1 hour.
[0150] [Comparative Example 4]
[0151] Silica powder A was put into a mixing container and stirring was started. Then, a peristaltic pump (SJ-1211II-H manufactured by ATTA) was used to supply 0.5 parts by weight of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone) relative to 100 parts by weight of silica powder A. After supplying, stirring was continued and mixing was continued for 15 minutes. Then, nitrogen was introduced into the reaction container for drying without performing a reaction step based on heating, and the surface-treated silica powder obtained was measured.
[0152] [Comparative Example 5]
[0153] A surface-treated silica powder was prepared and measured in the same manner as in Example 1 except that 9 parts by weight of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder A.
[0154] [Comparative Example 6]
[0155] A surface-treated silica powder was prepared and measured in the same manner as in Example 2 except that 18 parts by weight of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone) was used relative to 100 parts by weight of the silica powder A.
[0156] The surface-treated silica powders of Examples 1 to 11, which contain a large amount of non-chemically bonded silane coupling agent components in addition to the chemically bonded silane coupling agent, have good results in terms of viscosity index and gap permeability. This can be said to be the effect that the reactive hydroxyl groups on the surface of the silica particles are separated from the resin by the silane coupling agent components. Comparative Example 1, which does not contain a silane coupling agent component, and Example 3, in which the silane coupling agent component is only chemically bonded and the amount of silane coupling agent component present per unit specific surface area of silica particles in the surface-treated silica powder is small, are poor in both viscosity index and gap permeability. In addition, Comparative Example 2, in which the amount of physically adsorbed silane coupling agent component is small, has good only gap permeability, and Comparative Example 4, in which the amount of silane coupling agent component present per unit specific surface area of silica particles in the surface-treated silica powder is small, and Comparative Example 5, in which the amount of the component is large, has only good viscosity index. In addition, V 90 The surface-treated silica powder of Comparative Example 6 having a value of 100 or more had a low interstitial permeability.
Claims
1. A surface treated silicon dioxide powder, characterized in that: The surface-treated silica powder is a surface-treated silica powder obtained by surface-treating silica particles using a silane coupling agent. The amount of the silane coupling agent component chemically bonded to the surface of the silica particles per unit surface area of the silica particles is defined as C (pieces / nm 2 ), the amount of the silane coupling agent component present per unit specific surface area of the silica particles in the surface treated silica powder is set to T (pieces / nm 2 ), the ratio (C / T) is less than 0.
7.
2. The surface-treated silicon dioxide powder according to claim 1, characterized in that The amount T of the silane coupling agent component is 2.0 to 22.0 per nm. 2 .
3. The surface-treated silicon dioxide powder according to claim 1 or 2, characterized in that: The cumulative 50 volume % particle size (D 50 ) and cumulative 90 volume % particle size (D 90 ), the amount of coarse particles of the surface-treated silicon dioxide powder obtained according to Formula 1 (V 90 ) is greater than 10 and less than 100, V 90 ={(D 90 -D 50 ) / D 50 }×100(1)。 4. The surface-treated silicon dioxide powder according to claim 1 or 2, characterized in that: BET specific surface area is 1~100m 2 / g.
5. A resin composition, which is obtained by dispersing the surface-treated silica powder according to claim 1 or 2 in a resin.
6. A dispersion obtained by dispersing the surface-treated silicon dioxide powder according to claim 1 or 2 in a liquid solvent.
Citation Information
Patent Citations
Dry-process silica fine particle
JP2014152048A
Silica particles, resin composition containing said particles, and use thereof
WO2015119283A1
Electromagnetic wave shielding film
CN110113925A
Surface-modified silica powder and slurry composition
JP2015189638A