Curing accelerator for anaerobically curable compositions

By using methacrylate, tert-butyl peroxy-3,5,5-trimethylhexanoate, saccharin and 2-(N-ethylanilino)ethanol or 1,2,3 in the anaerobic curing agent , the combination of 4-tetrahydrobenzo(H)quinolin-3-ol solves the health and safety problems of diethyl-p-toluidine and dimethyl-o-toluidine in the existing technology, and achieves higher Sustainability and safety properties while maintaining adhesive performance.

CN118786155APending Publication Date: 2024-10-15HENKEL KGAA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380024523.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-04
Filing Date
2023-02-21
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Diethyl p-toluidine and dimethyl o-toluidine in existing anaerobic curing agents have health and safety issues, and the self-accelerating decomposition temperature and storage temperature of peroxide components such as cumene hydroperoxide limit their use. Application, it is difficult to fully solve the challenges of health and safety characteristics.

Method used

Use a methacrylate component, a first curing agent (such as tert-butyl peroxy-3,5,5-trimethylhexanoate), a second curing agent (such as saccharin) and a curing accelerator 2-(N -Ethylanilino)ethanol and/or 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol compositions to improve the sustainability, health and safety properties of the composition.

Benefits of technology

The composition significantly improves the health and safety properties of the composition without sacrificing adhesive properties and provides better cure properties and stability for adhesives, sealants and thread locking applications Agent applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005018874670000041
    Figure BDA0005018874670000041
  • Figure BDA0005018874670000042
    Figure BDA0005018874670000042
  • Figure BDA0005018874670000051
    Figure BDA0005018874670000051
Patent Text Reader

Abstract

The present invention relates to an anaerobically curable composition comprising: a) a (meth) acrylate component; b) a first curing agent; c) a second curing agent; and d) a curing accelerator comprising 2-(N-ethylanilino) ethanol and / or 1, 2, 3, 4-tetrahydrobenzo (H) quinoline-3-ol, and a method for producing the same. The anaerobically curable composition according to the present invention can be used in adhesives, sealants, thread locking agents and retaining agents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to anaerobically curable (meth)acrylate compositions having improved sustainability, health and safety properties. Background Art

[0002] Anaerobic technology is most widely used in the electrical industry because it provides improvements in equipment reliability, time savings, cost reduction, and improved process safety. Anaerobic adhesives are one-component (1k) systems that contain esters of acrylic acid or methacrylic acid and cure by a redox-initiated free radical mechanism driven by accelerators and initiators. The word anaerobic means that the polymerization occurs in the absence of air. Typical anaerobic adhesives contain (meth)acrylate monomers and / or (meth)acrylate oligomers, stabilizers, form modifiers, and curing agents (such as amines, peroxides, and saccharin).

[0003] Cumene hydroperoxide is widely used as a curing agent in anaerobic products due to its properties such as self-accelerating decomposition temperature (SADT) 70°C and maximum storage temperature 40°C (Ts max). However, due to the properties of this compound and the presence of cumene impurities, its safety label is a category 2 carcinogen. Similarly, diethyl-p-toluidine (DE-pT) and dimethyl-o-toluidine (DM-oT), which are often used and are the most effective curing accelerators in terms of curing speed and strength development of the composition, have poor health and safety characteristics.

[0004] Some attempts have been made to replace diethyl-p-toluidine (DE-pT) and dimethyl-o-toluidine (DM-oT) in anaerobically curable compositions. However, the peroxide component (such as cumene hydroperoxide) is still present in the composition, and thus the problems with health and safety properties have not been completely solved.

[0005] Therefore, there is a need for anaerobically curable compositions that can provide improved sustainability, health and safety properties without sacrificing the technical performance of the adhesive composition. Summary of the invention

[0006] The present invention relates to an anaerobically curable composition, the anaerobically curable composition comprising: a) a (meth) acrylate component; b) a first curing agent; c) a second curing agent; and d) a curing accelerator, wherein the curing accelerator comprises 2-(N-ethylanilino)ethanol and / or 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol.

[0007] The present invention also relates to a cured product of the anaerobically curable composition according to the invention.

[0008] The present invention comprises the use of the anaerobically curable composition or cured product according to the present invention in adhesives, sealants, thread lockers and retainers. DETAILED DESCRIPTION

[0009] The present invention is described in more detail in the following paragraphs. Unless there is a clear contrary indication, each aspect described in this way can be combined with any other one or more aspects. In particular, any feature that is indicated as preferred or advantageous can be combined with any other one or more features that are indicated as preferred or advantageous.

[0010] In the context of the present invention, unless the context dictates otherwise, the terms used should be interpreted according to the following definitions.

[0011] As used herein, the singular forms "a," "an," and "the" include both singular and plural referents unless the context clearly dictates otherwise.

[0012] As used herein, the terms "comprising / comprises / comprised of" are synonymous with "including / includes" or "containing / contains" and are inclusive or open-ended and do not exclude additional, unrecited members, elements or method steps.

[0013] As used herein, the term "consisting of excludes any elements, ingredients, members or method steps not specified.

[0014] The words "preferred", "preferably", "desirably", and "particularly / especially" are often used herein to refer to embodiments of the present disclosure that may provide specific benefits under certain circumstances. However, the recitation of one or more preferred, preferred, desired, or specific embodiments does not mean that other embodiments are not useful, and is not intended to exclude those other embodiments from the scope of the present disclosure.

[0015] As used throughout this application, the words "may" and "could" are used in a permissive sense (ie, meaning having the possibility), rather than in a mandatory sense.

[0016] The recitation of numerical endpoints includes all numbers and fractions contained within the corresponding ranges, as well as the recited endpoints.

[0017] Unless otherwise specified, all percentages, parts, ratios, etc. mentioned herein are based on weight.

[0018] When an amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper value and a preferred lower value, it should be understood that any range obtained by combining any upper value or preferred value with any lower value or preferred value is specifically disclosed, regardless of whether the obtained range is explicitly mentioned in the context.

[0019] All references cited in this specification are hereby incorporated by reference in their entirety.

[0020] Unless otherwise defined, all terms (including technical and scientific terms) used in disclosing the present invention have the meanings commonly understood by ordinary technicians in the field to which the present invention belongs. By further guidance, term definitions are included to better understand the teachings of the present invention.

[0021] The present invention relates to an anaerobically curable composition, the anaerobically curable composition comprising: a) a (meth) acrylate component; b) a first curing agent; c) a second curing agent; and d) a curing accelerator, wherein the curing accelerator comprises 2-(N-ethylanilino)ethanol and / or 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol.

[0022] Applicants have found that the use of a curing accelerator, particularly a curing accelerator comprising a combination of tert-butyl peroxy-3,5,5-trimethylhexanoate and 2-(N-ethylanilino)ethanol and / or 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol improves the sustainability, health and safety properties of the composition. In addition, the use of 2-(N-ethylanilino)ethanol and / or 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol enables the amount of the first curing agent (peroxide) to be reduced without sacrificing the performance properties of the composition.

[0023] The anaerobically curable composition according to the present invention comprises a (meth)acrylate component. Suitable (meth)acrylate components may be (meth)acrylate monomers, (meth)acrylate oligomers, or (meth)acrylate polymers.

[0024] The (meth)acrylate monomer suitable for use as the (meth)acrylate component in the present invention can be selected from a variety of materials, such as H2C=CGCO2R 8 those represented by, wherein G may be hydrogen, halogen, or an alkyl group having 1 to 4 carbon atoms, and R 8 It can be selected from an alkyl group, cycloalkyl group, alkenyl group, cycloalkenyl group, alkaryl group, aralkyl group, or aryl group having 1 to 16 carbon atoms, any of which can be optionally substituted or interrupted by silane, silicon, oxygen, halogen, carbonyl group, hydroxyl group, ester, carboxylic acid, urea, carbamate, carbonate, amine, amide, sulfur, sulfonate, sulfone, etc. according to the circumstances.

[0025] Additional (meth)acrylate monomers suitable for use herein as the (meth)acrylate component in the present invention or as a component in preparing the reaction product include multifunctional (meth)acrylate monomers, for example, difunctional (meth)acrylates or trifunctional (meth)acrylates, such as polyethylene glycol di(meth)acrylate, tetrahydrofuran (meth)acrylate and tetrahydrofuran di(meth)acrylate, hydroxypropyl (meth)acrylate ("HPMA"), hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate ("TMPTMA"), diethylene glycol dimethacrylate, triethylene glycol dimethacrylate ("TRIEGMA"), ”), tetraethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, di(pentamethylene glycol) di(meth)acrylate, tetraethylene diethylene glycol di(meth)acrylate, diglycerol tetra(meth)acrylate, tetramethylene di(meth)acrylate, ethylene di(meth)acrylate, neopentyl glycol di(meth)acrylate, and bisphenol A mono(meth)acrylate and bisphenol A di(meth)acrylates (such as ethoxylated bisphenol A (meth)acrylate (“EBIPMA”)), and bisphenol F mono(meth)acrylate and bisphenol F di(meth)acrylate (such as ethoxylated bisphenol A (meth)acrylate).

[0026] Other (meth)acrylate monomers that may be used herein include silicone (meth)acrylate moieties ("SiMA") such as those disclosed in US Pat. No. 5,605,999.

[0027] Other suitable monomers include polyacrylates represented by the formula:

[0028]

[0029] Where R 4 is a group selected from hydrogen, halogen, or an alkyl group having 1 to 4 carbon atoms; q is an integer equal to at least 1, preferably equal to 1 to 4; and X is an organic group containing at least two carbon atoms and having a total bonding capacity of q plus 1. For the upper limit of the number of carbon atoms in X, useful monomers exist in essentially any value. However, in practice, the usual upper limit is 50, preferably 30, and most preferably 20 carbon atoms.

[0030] For example, X can be an organic group of the formula:

[0031]

[0032] where Y 1 and Y 2Each is an organic group, preferably a hydrocarbon group, containing at least 2 carbon atoms, preferably 2-10 carbon atoms, and Z is an organic group, preferably a hydrocarbon group, containing at least 1 carbon atom, preferably 2-10 carbon atoms.

[0033] Other types of useful monomers are the reaction products of dialkanolamines or trialkanolamines (eg, ethanolamine or propanolamine) with acrylic acid, as disclosed in French Patent No. 1,581,361.

[0034] Examples of useful acrylate oligomers include those having the following general formula:

[0035]

[0036] Where R 5 represents a group selected from hydrogen, a lower alkyl group having 1 to 4 carbon atoms, a hydroxyalkyl group having 1 to 4 carbon atoms, and a group of the formula

[0037]

[0038] Where R 4 is a group selected from hydrogen, halogen, or a lower alkyl group having 1 to about 4 carbon atoms; R 6 is a group selected from hydrogen, hydroxyl, and a group of the formula

[0039]

[0040] Or m is an integer equal to at least 1, such as 1 to 15 or more, preferably 1 to 8; n is an integer equal to at least 1, such as 1 to 40 or more, preferably 2 to 10; and p is 0 or 1.

[0041] Typical examples of acrylate oligomers corresponding to the above general formula include diethylene glycol dimethacrylate, triethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate; di(pentamethylene glycol) dimethacrylate; tetraethylene glycol diacrylate; tetraethylene glycol di(chloroacrylate); diglycerol diacrylate; diglycerol tetramethacrylate; butanediol dimethacrylate; neopentyl glycol diacrylate; and trimethylolpropane triacrylate.

[0042] Although diacrylate and other polyacrylates, particularly the polyacrylate described in the preceding paragraph may be desirable, monofunctional acrylates (esters containing an acrylate group) may also be used. When relating to monofunctional acrylates, it is highly preferred to use esters with relatively polar alcohol moieties. The volatility of such materials is lower than that of low molecular weight alkyl esters, and more importantly, the polar groups tend to provide intermolecular attraction during and after curing, thereby producing more desirable curing properties and more durable sealants or adhesives. Desirably, the polar groups are selected from unstable hydrogen, heterocycle, hydroxyl, amino, cyano and halogenated polar groups. Typical examples of compounds in this category are cyclohexyl methacrylate, tetrahydrofurfuryl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, tert-butylaminoethyl methacrylate, cyanoethyl acrylate and chloroethyl methacrylate.

[0043] Another class of useful monomers is prepared by the reaction of monofunctionally substituted alkyl or aryl acrylates containing active hydrogen atoms on the functional substituents. The monofunctional acrylate-terminated material is reacted with an organic polyisocyanate in a suitable ratio to convert all isocyanate groups to carbamate or urea groups. Monofunctional alkyl and aryl acrylates are preferably acrylates and methacrylates containing hydroxyl or amino functional groups on the non-acrylate portion thereof. Suitable acrylates have the formula:

[0044]

[0045] wherein X is selected from -O- or And R 9 is selected from hydrogen or a lower alkyl group having 1 to 7 carbon atoms; R 7 is selected from hydrogen, chlorine or methyl and ethyl; and R 8 is a divalent organic radical selected from lower alkylene, phenylene or naphthylene having 1 to 8 carbon atoms. These radicals, when appropriately reacted with polyisocyanates, produce monomers of the general formula:

[0046]

[0047] wherein n is an integer from 2 to 6; B is a polyvalent organic group selected from substituted and unsubstituted alkyl, alkenyl, cycloalkyl, cycloalkenyl, aryl, aralkyl, alkaryl, or heterocyclic groups; and R 7 , R 8 and X have the meanings given above.

[0048] Examples of suitable hydroxy-functional (meth)acrylates include hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate ("HEMA"), hydroxypropyl methacrylate ("HPMA"), hydroxybutyl methacrylate, and mixtures thereof. Other examples of suitable hydroxy-functional (meth)acrylates include 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate ("HEMA"), pentaerythritol triacrylate ("PETA"), and 4-hydroxybutyl acrylate.

[0049] The number average molecular weight of the hydroxy-functional (meth)acrylate may be from about 80 to about 1,000 g / mole, or from about 100 to about 800 g / mole, or from about 110 to about 600 g / mole.

[0050] Of course, combinations of these (meth)acrylate components may also be used.

[0051] In a highly preferred embodiment, the (meth)acrylate component is selected from the group consisting of hydroxyethyl methacrylate, hydroxypropyl methacrylate, poly(ethylene glycol) dimethacrylate, and mixtures thereof.

[0052] Commercially available (meth)acrylate components suitable for use in the present invention include, but are not limited to, hydroxyethyl methacrylate and hydroxypropyl methacrylate from Geo Specialty and Sartomer.

[0053] The anaerobically curable composition according to the present invention may have 87-97 wt %, preferably 89-97 wt %, more preferably 90-96.5 wt % of the (meth)acrylate component based on the total weight of the composition.

[0054] The above defined amount range is ideal and provides good strength to the anaerobically curable composition according to the present invention. An amount less than 87% and exceeding 97% may have a direct negative impact on the strength of the anaerobically curable composition.

[0055] The anaerobically curable composition according to the present invention comprises a first curing agent. The first curing agent may be a hydroperoxide, preferably selected from tert-butyl hydroperoxide, alkyl hydroperoxide, tert-butyl perbenzoate, diisopropylbenzene hydroperoxide, tert-butyl peroxy-3,5,5-trimethylhexanoate, diacetyl peroxide, benzoyl peroxide, tert-butyl peracetate, lauryl peroxide, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexyl carbonate, tert-amyl hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, and mixtures thereof, more preferably selected from the group consisting of Alkane hydroperoxide, diisopropylbenzene hydroperoxide, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peracetate, lauryl peroxide, tert-butyl peroxy-2-ethylhexyl carbonate, tert-amyl hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, and mixtures thereof, and even more preferably, the first curing agent is tert-butyl peroxy-3,5,5-trimethylhexanoate.

[0056] In a highly preferred embodiment, the first curing agent is tert-butyl peroxy-3,5,5-trimethylhexanoate. Tert-butyl peroxy-3,5,5-trimethylhexanoate is particularly preferred because it can provide improved health and safety properties and show similar curing performance at lower amounts.

[0057] Commercially available first curing agents suitable for use in the present invention include, but are not limited to, alkyl hydroperoxide, tert-butyl perbenzoate from Nouryon, benzoyl peroxide from Akzo Nobel, and tert-butyl peroxy-3,5,5-trimethylhexanoate from Arkema.

[0058] The anaerobically curable composition according to the present invention may have 0.1-3.0 wt %, preferably 0.15-2.5 wt %, more preferably 0.2-2.3 wt % of the first curing agent based on the total weight of the composition.

[0059] The above range is preferred because it provides good curing characteristics for the composition according to the present invention. When the amount of the first curing agent is less than 0.1%, this results in a slow curing rate and the strength properties of the composition are negatively affected. However, a high amount exceeding 3% results in a fast curing rate and instability of the composition.

[0060] The anaerobically curable composition according to the present invention comprises a second curing agent. The second curing agent is preferably selected from saccharin, di-p-toluylsulfonimide, tert-butylbenzoyltoluoylsulfonamide, methylbenzoyltoluoylsulfonamide, methoxybenzoyltoluoylsulfonamide, and mixtures thereof; more preferably, the second curing agent is saccharin.

[0061] In a highly preferred embodiment, the second solidifying agent is saccharin. Saccharin is particularly preferred because it can also act as a co-accelerator in the composition.

[0062] Commercially available secondary solidifying agents suitable for use in the present invention include, but are not limited to, saccharin from Univar, di-p-toluoylsulfonimide, and t-butylbenzoyltoluoylsulfonamide.

[0063] The anaerobically curable composition according to the present invention may have 0.1-5.0 wt %, preferably 1.0-3.5 wt %, more preferably 1.1-3.0 wt % of the second curing agent based on the total weight of the composition.

[0064] The above range is preferred because it provides good curing characteristics for the composition according to the present invention. When the amount of the second curing agent is less than 0.1%, this results in a slow curing rate and the strength properties of the composition are negatively affected. However, a high amount exceeding 5% results in a fast curing rate and instability of the composition.

[0065] In another highly preferred embodiment, the anaerobically curable composition according to the present invention comprises a first curing agent (tert-butyl peroxy-3,5,5-trimethylhexanoate) and a second curing agent (saccharin).

[0066] The composition according to the present invention comprises a curing accelerator comprising 2-(N-ethylanilino)ethanol and / or 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol (TBHQ-ol).

[0067] 2-(N-ethylanilino)ethanol and 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol (TBHQ-ol) are selected and are preferred because they offer better health and safety properties compared to conventional curing accelerators while showing equal or at least comparable reactivity and stability in the composition according to the invention.

[0068] Commercially available cure accelerators suitable for use in the present invention include, but are not limited to, 2-(N-ethylanilino)ethanol from BASF and 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol (TBHQ-ol) from Vanamali Organics.

[0069] The anaerobically curable composition according to the present invention may have 0.1-1.5 wt %, preferably 0.2-1.0 wt %, more preferably 0.25-0.75 wt % of a curing accelerator, based on the total weight of the composition.

[0070] In order to obtain good curing and composition stability, the amount of curing accelerator is very important, and the range defined above can provide this. If the amount of curing accelerator is less than 0.1%, the curing rate will be too slow, while an amount greater than 1.5% will have a negative impact on the stability of the composition.

[0071] The anaerobically curable composition according to the invention may further comprise a stabilizer.

[0072] The stabilizer is preferably selected from benzoquinone, 1,4-naphthoquinone, anthraquinone, hydroquinone, methoxyhydroquinone, tert-butylhydroquinone, butylated hydroxytoluene, and mixtures thereof; preferably, the stabilizer is 1,4-naphthoquinone.

[0073] The stabilizers listed above are preferred because they are proven stabilizers and can prevent premature polymerization of the composition, ie they can provide the desired shelf-life stability to the composition according to the invention.

[0074] Commercially available stabilizers suitable for use in the present invention include, but are not limited to, 1,4-naphthoquinone from Sigma Aldrich.

[0075] The anaerobically curable composition according to the present invention may have 0.01-1.0 wt %, preferably 0.05-0.75 wt %, more preferably 0.1-0.4 wt % of the stabilizer, based on the total weight of the composition.

[0076] If the amount of stabilizer is less than 0.01%, this may negatively affect the stability of the composition according to the invention. However, amounts exceeding 1% may not have any significant additional effect on the stability and performance of the composition.

[0077] The anaerobically curable composition according to the present invention may further comprise a chelating agent.

[0078] Preferably, the chelating agent is selected from the sodium salt of ethylenediaminetetraacetic acid, trisodium salt of N-hydroxyethylenediaminetetraacetic acid (HEDTANas), tetrakis(2-hydroxypropyl)ethylenediamine (EDTPA), pentasodium salt of diethylenetriaminepentaacetic acid (DTPA), and mixtures thereof; preferably, the chelating agent is the sodium salt of ethylenediaminetetraacetic acid.

[0079] The sodium salt of EDTA is preferred as it is more effective than other common chelating agents.

[0080] Commercially available chelating agents suitable for use in the present invention include, but are not limited to, the sodium salt of ethylenediaminetetraacetic acid from BASF.

[0081] The anaerobically curable composition according to the present invention may have 0.2-2.0 wt %, preferably 0.3-1.5 wt %, more preferably 0.6-1.2 wt % of the chelating agent, based on the total weight of the composition.

[0082] If the amount of chelating agent is less than 0.2%, this may negatively affect the stability of the composition. However, amounts exceeding 2.0% do not have any significant additional effect on the stability and performance of the composition.

[0083] The anaerobically curable composition according to the invention may also contain pigments.

[0084] Preferably, the pigment is selected from 1-phenylazo-2-naphthol (Solvent Yellow 14), 2,4-dihydro-5-methyl-2-phenyl-4-(phenylazo)-3H-pyrazol-3-one (Sudan Yellow 146) and 1,4-bis(p-tolylamino)anthraquinone (Sudan Green 4B), and mixtures thereof.

[0085] The anaerobically curable composition according to the present invention may have 0.01-0.05 wt % of pigment, based on the total weight of the composition.

[0086] In a preferred embodiment, the anaerobically curable composition according to the present invention comprises: a) a) (meth) acrylate component; b) a first curing agent, wherein the first curing agent is tert-butyl peroxy-3,5,5-trimethylhexanoate; c) a second curing agent; and d) a curing accelerator, wherein the curing accelerator comprises 2-(N-ethylanilino)ethanol and / or 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol.

[0087] In a preferred embodiment, the anaerobically curable composition according to the present invention comprises: a) a) (meth) acrylate component; b) a first curing agent, wherein the first curing agent is tert-butyl peroxy-3,5,5-trimethylhexanoate; c) a second curing agent, wherein the second curing agent is saccharin; and d) a curing accelerator, wherein the curing accelerator comprises 2-(N-ethylanilino)ethanol and / or 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol.

[0088] In another preferred embodiment, the anaerobically curable composition according to the present invention comprises: a) a (meth) acrylate component; b) 0.1-3.0 wt. %, preferably 0.1-2.75 wt. %, more preferably 0.1-2.3 wt. % of a first curing agent, based on the total weight of the composition, wherein the first curing agent is tert-butyl peroxy-3,5,5-trimethylhexanoate; c) a second curing agent; and d) a curing accelerator, the curing accelerator comprising 0.1-1.5 wt. %, preferably 0.2-1.0 wt. %, more preferably 0.25-0.75 wt. % of 2-(N-ethylanilino)ethanol and / or 0.1-1.5 wt. %, preferably 0.2-1.0 wt. %, more preferably 0.25-0.75 wt. % of 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol, based on the total weight of the composition.

[0089] In another preferred embodiment, the anaerobically curable composition according to the present invention comprises: a) a (meth) acrylate component; b) 0.1-3.0 wt. %, preferably 0.1-2.75 wt. %, more preferably 0.1-2.3 wt. % of a first curing agent, based on the total weight of the composition, wherein the first curing agent is tert-butyl peroxy-3,5,5-trimethylhexanoate; c) a second curing agent, wherein the second curing agent is saccharin; and d) a curing accelerator, the curing accelerator comprising 0.1-1.5 wt. %, preferably 0.2-1.0 wt. %, more preferably 0.25-0.75 wt. % of 2-(N-ethylanilino)ethanol and / or 0.1-1.5 wt. %, preferably 0.2-1.0 wt. %, more preferably 0.25-0.75 wt. % of 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol, based on the total weight of the composition.

[0090] The present invention also relates to a cured product of the anaerobically curable composition according to the invention.

[0091] The present invention relates to the use of the anaerobically curable composition or the cured product according to the present invention in adhesives, sealants, threadlockers and retaining agents.

[0092] Example

[0093] Example 1

[0094] Four anaerobic compositions were prepared in which the concentration of 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol (THBQ-ol) was maintained at 0.5% w / w while the concentration of tert-butyl peroxy-3,5,5-trimethylhexanoate (TBPTH) was varied from 0.25 to 1.0% w / w. The formulation details are provided in Table 1 below.

[0095] Table 1

[0096]

[0097] All four prepared formulations were tested for compressive shear strength, break torque, and prevail torque on mild steel and stainless steel. The bonded pins and collars, as well as nuts and bolts, were cured at room temperature for 1 hour and 24 hours, and the results were recorded and compared to the control formulations. To further understand the durability, mild steel pins and collars were bonded and cured at room temperature for 24 hours, then exposed to 100°C for 1000 hours, and compared to the strength properties of the control.

[0098] Compressive shear strength was measured on mild and stainless steel, rods and rod rings (P&C) according to ASTM D 4562-001.

[0099] The compressive shear strengths of all four formulations are reported in Tables 2 and 3. Table 2 illustrates 1 hour room temperature cure compressive shear strength (rod and rod ring) N / mm 2 Results and Table 3 exemplify 24-hour room temperature cured compressive shear strength (rod and rod ring) N / mm 2 .

[0100] Table 2

[0101]

[0102] Table 3

[0103]

[0104] From the above test results, it is observed that Examples 2 and 3 exhibit similar 1 hour and 24 hour room temperature cure and similar compressive shear strength on mild steel and stainless steel.

[0105] Breakaway torque is measured on mild and stainless steel, nuts and bolts (N&B) according to ASTM D 5649-01.

[0106] The breakaway torques for all four formulations are reported in Tables 4 and 5. Table 4 illustrates the 1 hour room temperature cure breakaway torque (M10 N&B) in Nm, and Table 5 illustrates the 24 hour room temperature cure breakaway torque (M10 N&B) in Nm.

[0107] Table 4

[0108]

[0109] Table 5

[0110]

[0111] According to the above test results, all Examples 1-4 show improvement in breaking torque on mild steel, while they are comparable on stainless steel.

[0112] Pull-out torque is measured on mild steel and stainless steel according to ASTM D 5649-01.

[0113] The pull-out torques for all four formulations are reported in Tables 6 and 7. Table 6 illustrates the 1 hour room temperature cure pull-out torque (N&B) in Nm, and Table 7 illustrates the 24 hour room temperature cure pull-out torque (N&B) in Nm.

[0114] Table 6

[0115]

[0116] Table 7

[0117]

[0118] According to the above test results, Formulation Examples 5 and 6 show an increase in 1 hour room temperature cure pull-out torque on mild steel and stainless steel compared to the comparative example, while the 24 hour room temperature cure pull-out torque on mild steel and stainless steel is similar.

[0119] Heat aging

[0120] All four formulations as well as the control were used to bond mild steel rods and rod rings and allowed to cure at room temperature for 24 hours and then exposed to 100°C for 1000 hours. After completion of 1000 hours at 100°C, the bonded rods and rod rings were cooled to room temperature and tested for compressive shear strength to measure retention of bond strength. Heat aging testing was performed according to ASTM D 4562-001.

[0121] Heat aged compressive shear strength on mild steel (rod and rod ring) N / mm 2 The test results are shown in Table 8.

[0122] Table 8

[0123]

[0124] The heat aging results show that Example 1 and Example 2 show comparable retention in compressive shear strength compared to the control, while Example 3 and Example 4 show a 9% decrease in compressive shear strength. In summary, all four examples show comparable retention in compressive shear strength to the comparative example.

[0125] Example 2

[0126] Four different formulations were prepared by maintaining the same concentration of common ingredients such as methacrylate monomer (PEGDMA), stabilizers, chelating agents and saccharin. As shown in Table 9, in Examples 5, 6, 7 and 8, the concentration of EtOH amine was maintained at 0.5% w / w, and the concentration of peroxy-3,5,5-trimethylhexanoic acid tert-butyl ester (TBPTH) was varied between 0.5, 1.0, 1.5 and 2.0% w / w, respectively. The formulation containing the new curing agent was compared with Comparative Example 2, which contained conventional curing agents CHP (1.5%) and DE-pT, DM-oT (0.5%). All components were mixed together for an appropriate time until completely dissolved.

[0127] Table 9

[0128]

[0129] Shear strength properties

[0130] The above formulations were tested for shear strength, breaking torque and pull-out torque on reactive mild steel (MS) substrates and non-reactive stainless steel (SS) substrates after 1 hour and 24 hours of curing at ambient temperature (25°C). The substrate rods and rod rings for shear strength testing were cleaned according to standard practice, and five different specimens were bonded by each of the above formulations according to the standard and tested for shear strength properties after 1 hour and 24 hours of room temperature curing.

[0131] Shear strength properties were measured according to ASTM D 4562-001.

[0132] The results for Comparative Example 2, Example 5, Example 6, Example 7 and Example 8 on both substrates were recorded after 1 hour of curing and are shown in Table 2.

[0133] Table 10 illustrates the shear strength properties on mild steel substrates and stainless steel substrates after 1 hour cure.

[0134] Table 10

[0135]

[0136] The results obtained mean that the shear strength performance of all four Examples 5-8 after 1 hour of curing is comparable to that of Comparative Example 2.

[0137] In a similar manner, all examples were tested for shear strength properties on both mild steel substrates and stainless steel substrates after 24 hours of curing. The results are shown in Table 11.

[0138] Table 11

[0139]

[0140] The shear strength performance of all formulations after 24 hours of cure on mild steel and stainless steel substrates was comparable to the control.

[0141] Breaking torque performance

[0142] Torque properties were measured after 1 hour and 24 hours of curing on mild steel substrates and stainless steel substrates at room temperature. The initial torque gives a reduced axial load measurement and is referred to as the breaking torque. Five specimens of degreased black oxide nuts and bolts were assembled to evaluate the breaking torque and pull-out torque properties of Comparative Example 2 and Examples 5-8, respectively.

[0143] Breaking torque properties were measured according to ASTM D 5649-01.

[0144] After 1 hour of curing, the breaking torque was measured on mild steel substrates and stainless steel substrates as shown in Table 12.

[0145] Table 12

[0146]

[0147] It was observed that the torque at break results recorded for all examples according to the invention after 1 hour of curing on mild steel substrates and stainless steel substrates were comparable to those of Comparative Example 2.

[0148] Table 13 illustrates the breaking torque performance on mild steel substrates and stainless steel substrates after 24 hours of cure.

[0149] Table 13

[0150]

[0151] In a similar manner, it was observed that the breaking torque strength performance of all formulations was comparable to that of Comparative Example 2 on both mild steel and stainless steel substrates.

[0152] Pull-out torque performance

[0153] The pull-out torque performance was measured by rotating the nut 360° after initial failure of the bond. The pull-out torque performance of the formulations is reported in Tables 14 and 15 below, and it is observed that the examples according to the invention exhibited substantially similar performance to Comparative Example 2 on both mild steel and stainless steel substrates after 1 hour and 24 hours of cure at room temperature.

[0154] Pull-out torque properties were measured according to ASTM D 5649-01.

[0155] Table 14 illustrates the pull-out torque on mild steel substrates and stainless steel substrates after 1 hour of cure, and Table 15 illustrates the pull-out torque on mild steel substrates and stainless steel substrates after 24 hours of cure.

[0156] Table 14

[0157]

[0158] Table 15

[0159]

[0160] Heat aging properties

[0161] After curing for 24 hours and aging for 1000 hours at 100°C, the heat aged shear strength performance was evaluated. After the heat treatment, the rods and rod rings were cooled to room temperature and tested for shear strength. The results obtained show that the strength performance of the examples according to the present invention is comparable to that of Comparative Example 2, as shown in Table 16.

[0162] Heat aging tests were performed according to ASTM D 4562-001.

[0163] Table 16

[0164]

Claims

1. An anaerobically curable composition, the anaerobically curable composition comprising: a) (meth)acrylate component; b) a first curing agent; c) a second curing agent; and d) a curing accelerator, the curing accelerator comprising 2-(N-ethylanilino)ethanol and / or 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol.

2. The anaerobically curable composition according to claim 1, wherein the (meth)acrylic monomer accounts for 87-97 wt%, preferably 89-97 wt%, more preferably 90-96.5 wt%, of the total weight of the composition.

3. The anaerobically curable composition according to claim 1 or 2, wherein the first curing agent is a hydroperoxide, preferably selected from tert-butyl hydroperoxide, alkyl hydroperoxide, tert-butyl perbenzoate, diisopropylbenzene hydroperoxide, tert-butyl peroxy-3,5,5-trimethylhexanoate, diacetyl peroxide, benzoyl peroxide, tert-butyl peracetate, lauryl peroxide, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexyl carbonate, tert-amyl hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, and mixtures thereof, more preferably selected from the group consisting of Alkane hydroperoxide, diisopropylbenzene hydroperoxide, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peracetate, lauryl peroxide, tert-butyl peroxy-2-ethylhexyl carbonate, tert-amyl hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, and mixtures thereof, and even more preferably the first curing agent is tert-butyl peroxy-3,5,5-trimethylhexanoate.

4. The anaerobically curable composition according to any one of claims 1 to 3, wherein the first curing agent accounts for 0.1-3.0 wt%, preferably 0.15-2.5 wt%, more preferably 0.2-2.3 wt%, of the total weight of the composition.

5. The anaerobically curable composition according to any one of claims 1 to 4, wherein the second curing agent is selected from saccharin, di-p-toluoylsulfonimide, tert-butylbenzoyltoluoylsulfonamide, methylbenzoyltoluoylsulfonamide, methoxybenzoyltoluoylsulfonamide, and mixtures thereof, preferably the second curing agent is saccharin.

6. The anaerobically curable composition according to any one of claims 1 to 5, wherein the second curing agent accounts for 0.1-5.0 wt%, preferably 1.0-3.5 wt%, more preferably 1.1-3.0 wt%, of the total weight of the composition.

7. The anaerobically curable composition according to any one of claims 1 to 6, wherein the curing accelerator accounts for 0.1-1.5 wt%, preferably 0.2-1.0 wt%, more preferably 0.25-0.75 wt%, of the total weight of the composition.

8. The anaerobically curable composition according to any one of claims 1 to 7, comprising: a) (meth)acrylate component; b) a first curing agent, wherein the first curing agent is tert-butyl peroxy-3,5,5-trimethylhexanoate; c) a second curing agent; and d) a curing accelerator, the curing accelerator comprising 2-(N-ethylanilino)ethanol and / or 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol.

9. The anaerobically curable composition according to claim 8, wherein tert-butyl peroxy-3,5,5-trimethylhexanoate accounts for 0.1-3.0 wt%, preferably 0.1-2.75 wt%, more preferably 0.1-2.3 wt%, of the total weight of the composition, and 2-(N-ethylanilino)ethanol accounts for 0.1-1.5 wt %, preferably 0.2-1.0 wt %, more preferably 0.25-0.75 wt %, of the total weight of the composition. and / or 1,2,3,4-tetrahydrobenzo(H)quinolin-3-ol accounts for 0.1-1.5 wt%, preferably 0.2-1.0 wt%, more preferably 0.25-0.75 wt%, of the total weight of the composition.

10. The anaerobically curable composition according to any one of claims 1 to 9, wherein the composition further comprises a stabilizer, preferably selected from benzoquinone, 1,4-naphthoquinone, anthraquinone, hydroquinone, methoxyhydroquinone, tert-butylhydroquinone, butylated hydroxytoluene, and mixtures thereof; preferably the stabilizer is 1,4-naphthoquinone.

11. The anaerobically curable composition according to claim 10, wherein the stabilizer accounts for 0.01-1.0 wt%, preferably 0.05-0.75 wt%, more preferably 0.1-0.4 wt%, based on the total weight of the composition.

12. An anaerobically curable composition according to any one of claims 1 to 11, wherein the composition further comprises a chelating agent, the chelating agent is preferably selected from the group consisting of sodium salt of ethylenediaminetetraacetic acid, trisodium salt of N-hydroxyethylenediaminetetraacetic acid, tetrakis(2-hydroxypropyl)ethylenediamine, pentasodium salt of diethylenetriaminepentaacetic acid, and mixtures thereof; preferably, the chelating agent is sodium salt of ethylenediaminetetraacetic acid.

13. The anaerobically curable composition according to claim 12, wherein the chelating agent accounts for 0.2-2.0 wt%, preferably 0.3-1.5 wt%, more preferably 0.6-1.2 wt%, based on the total weight of the composition.

14. A cured product of the anaerobically curable composition according to any one of claims 1 to 13.

15. Use of the anaerobically curable composition according to any one of the preceding claims 1 to 13 or the cured product according to claim 14 in adhesives, sealants, threadlockers and retaining agents.