Resin composition, adhesive, sealing material, cured product, semiconductor device and electronic component
By using thermal curing accelerators of (meth)acrylate compounds, multifunctional thiol compounds and azabicyclic compounds in the resin composition, the problem that the light and thermosetting resin compositions do not react during the thermal curing process after curing by UV irradiation is solved. The problem of residual components is eliminated, and dimensional stability and positional deviation are reduced.
Patent Information
- Application Number
- CN202380024718.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-01
- Filing Date
- 2023-02-17
- Publication Date
- 2024-10-15
AI Technical Summary
When the existing light and thermosetting resin compositions are thermally cured after curing by UV irradiation, the remaining unreacted low molecular components may cause bleeding, outgassing and positional deviation problems, especially the size of the cured product due to shrinkage during the additional heating process. instability.
A resin composition containing a (meth)acrylate compound, a multifunctional thiol compound, a photoradical polymerization initiator and a thermal curing accelerator of an azabicyclic compound having a bridgehead nitrogen is used, and thermal curing is accelerated by adjusting the component ratio and adding agent to inhibit the residue of unreacted components.
It effectively suppresses the residue of unreacted components during the thermal curing process after UV curing, prevents leakage and outgassing, maintains dimensional stability during additional heating, and reduces positional deviation and optical axis deviation.
Smart Images

Figure BDA0005020001950000061 
Figure BDA0005020001950000062 
Figure BDA0005020001950000071
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition, an adhesive or a sealing material comprising the resin composition, a cured product thereof, and a semiconductor device and an electronic component comprising the cured product. Background Art
[0002] There are known photo- and thermosetting resin compositions that can be temporarily fixed by light irradiation and can be fully cured by heating. More specifically, adhesives of the type that are temporarily fixed by ultraviolet (UV) irradiation and then fully cured by heat are used in many fields (for example, Patent Documents 1 and 2). This type of adhesive is particularly widely used for image sensor modules.
[0003] Patent document 3 discloses a resin composition having high bonding strength (especially high peel strength) after curing and capable of suppressing the decrease in bonding strength (especially peel strength) after a moisture resistance test after curing. The resin composition is a photo- and thermosetting resin composition and contains (A) an acrylic resin, (B) a thiol compound, and (C) a latent curing accelerator.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-51954
[0007] Patent Document 2: International Publication No. 2005 / 052021
[0008] Patent Document 3: International Publication No. 2018 / 047849 Summary of the invention
[0009] Problems to be solved by the invention
[0010] It has been found that the light and thermosetting resin composition or adhesive cured by the 2-stage curing process of heat curing (stage 2 curing) after UV irradiation curing (stage 1 curing) also has a lot of unreacted low molecular components remaining in the cured product even after the heat curing of the second stage. It can be considered that this is because, generally speaking, in the area cured by UV irradiation curing of the first stage, most of the molecules are fixed, so the molecular motion is suppressed in the heat curing of the second stage, and the thermosetting component needs more heat energy to react compared with the case of only heat curing. The unreacted components (hereinafter also referred to as "residual components") remaining in the cured area may cause the problem of exudation and degassing as time passes. In addition, the curable resin composition or adhesive needs additional heating after the third stage when building the entire module in some cases, but the residual components are cured and the cured product is shrunk during the additional heating, which may cause the problem of position deviation and optical axis deviation.
[0011] Therefore, an object of the present invention is to provide a resin composition and an adhesive which can provide a cured product in which unreacted components are unlikely to remain after a second-step thermal curing subsequent to a first-step UV curing.
[0012] Means for solving problems
[0013] Specific means for solving the above-mentioned problems are as follows.
[0014] A first embodiment of the present invention is the following resin composition.
[0015] (1) A resin composition comprising:
[0016] (A) (meth)acrylate compound,
[0017] (B) a multifunctional thiol compound,
[0018] (C) a photoradical polymerization initiator, and
[0019] (D) A thermal curing accelerator comprising an azabicyclic compound having a bridgehead nitrogen.
[0020] (2) The resin composition according to (1) above, wherein the ratio of the number of (meth)acryloyl group equivalents of the component (A) to the number of thiol group equivalents of the component (B) ([number of (meth)acryloyl group equivalents of the component (A)] / [number of thiol group equivalents of the component (B)]) is 0.25 to 3.0.
[0021] (3) The resin composition according to (1) or (2) above, wherein the (B) polyfunctional thiol compound comprises a trifunctional or higher-functional thiol compound.
[0022] (4) The resin composition according to any one of (1) to (3) above, further comprising (E) an epoxy compound.
[0023] A second embodiment of the present invention is the following adhesive or sealing material.
[0024] (5) An adhesive or a sealing material comprising the resin composition according to any one of (1) to (4) above.
[0025] (6) The adhesive or sealing material according to (5) above, which is used for fixing, bonding or protecting components constituting an image sensor or a camera module.
[0026] The third embodiment of the present invention is the following cured product.
[0027] (7) A cured product obtained by curing the resin composition according to any one of (1) to (4) above or the adhesive or sealing material according to (5) or (6) above.
[0028] A fourth embodiment of the present invention is the following semiconductor device or electronic component.
[0029] (8) A semiconductor device or an electronic component comprising the cured product according to (7) above.
[0030] (9) The semiconductor device or electronic component according to (8) above, which is an image sensor or a camera module.
[0031] Effects of the Invention
[0032] According to the first embodiment of the present invention, a resin composition can be obtained, which can provide a cured product that suppresses the remaining unreacted components after the second stage of thermal curing following the first stage of UV curing, suppresses the occurrence of oozing out and outgassing, and has high dimensional stability when additional heating is applied. In addition, according to the second embodiment of the present invention, an adhesive or sealing material can be obtained, which can provide a cured product that suppresses the remaining unreacted components after the second stage of thermal curing following the first stage of UV curing, suppresses the occurrence of oozing out and outgassing, and has high dimensional stability when additional heating is applied. In addition, according to the third embodiment of the present invention, a cured product can be obtained, which suppresses the occurrence of oozing out and outgassing, and has high dimensional stability when additional heating is applied. According to the fourth embodiment of the present invention, a semiconductor device or electronic component can be obtained, which includes a cured product that suppresses the occurrence of oozing out and outgassing, and has high dimensional stability when additional heating is applied. DETAILED DESCRIPTION
[0033] [Resin composition]
[0034] A resin composition according to a first embodiment of the present invention includes:
[0035] (A) (meth)acrylate compound,
[0036] (B) a polyfunctional thiol compound, and
[0037] (C) a photoradical polymerization initiator, and
[0038] (D) A thermal curing accelerator comprising an azabicyclic compound having a bridgehead nitrogen.
[0039] According to this embodiment, a resin composition can be obtained which can provide a cured product having high dimensional stability when additionally heated while suppressing the remaining unreacted components after the second-stage thermal curing following the first-stage UV curing, suppressing the occurrence of bleed-out and outgassing.
[0040] (A) (Meth)acrylate compound
[0041] The resin composition of the present embodiment contains (A) (meth)acrylate compound (hereinafter also referred to as "component (A)"). (A) (meth)acrylate compound can impart transparency and appropriate hardness to the cured resin composition. The (meth)acrylate compound as component (A) is not particularly limited as long as it has one or more (meth)acryloyl groups. Considering the aspect of ensuring heat resistance, compounds having two or more (meth)acryloyl groups are preferred, compounds having 2 to 6 (meth)acryloyl groups are more preferred, and compounds having 2 (meth)acryloyl groups are further preferred. In addition, in order to adjust the viscosity and physical properties of the cured product (adhesive strength, flexibility, etc.), a compound having one (meth)acryloyl group may be used in addition to a compound having two (meth)acryloyl groups.
[0042] Examples of the (meth)acrylate compound (A) include diacrylate and / or dimethacrylate of tris(2-hydroxyethyl)isocyanurate; tris(2-hydroxyethyl)isocyanurate triacrylate and / or trimethacrylate; trimethylolpropane triacrylate and / or trimethacrylate or oligomers thereof; pentaerythritol triacrylate and / or trimethacrylate or oligomers thereof; polyacrylate and / or polymethacrylate of dipentaerythritol; tri(acryloyloxyethyl)isocyanurate; caprolactone-modified tri(acryloyloxyethyl)isocyanurate; caprolactone-modified tri(methacryloyloxyethyl)isocyanurate; polyacrylate and / or polymethacrylate of alkyl-modified dipentaerythritol; caprolactone Modified dipentaerythritol polyacrylate and / or polymethacrylate; ethoxylated bisphenol A diacrylate and / or ethoxylated bisphenol A dimethacrylate; dihydrocyclopentadiethyl acrylate and / or dihydrocyclopentadiethyl methacrylate and polyester acrylate and / or polyester methacrylate, dimethylol-tricyclodecane diacrylate, poly(meth)acrylate of di(trimethylol)propane, polyurethane having more than 2 (meth)acryloyl groups in 1 molecule, polyester having more than 2 (meth)acryloyl groups in 1 molecule, phenoxyethyl acrylate, isobornyl acrylate, phenoxydiethylene glycol (meth)acrylate, 4-tert-butylcyclohexyl acrylate, epoxy resin semi-acrylate, etc., but are not limited to them. From the viewpoint of reactivity, component (A) preferably does not substantially contain methacrylate compounds, but acrylate compounds.
[0043] (A) (meth)acrylate compound: Any one of the above-mentioned (meth)acrylate compounds may be used, or two or more of them may be used in combination.
[0044] From the viewpoint of preparation and dispensing properties of the resin composition, component (A) preferably has a viscosity of 0.01 to 100 Pa·s. In this specification, viscosity refers to a value measured at a measurement temperature of 25° C. using an appropriate viscometer corresponding to the viscosity range.
[0045] Commercially available products of component (A) include, for example, polyester acrylate (trade name: EBECRYL810) manufactured by Daicel Allnex Co., Ltd., bis(trimethylol)propane tetraacrylate (trade name: EBECRYL140) manufactured by Daicel Allnex Co., Ltd., polyester acrylate (trade name: M7100) manufactured by Toagosei Co., Ltd., dimethylol-tricyclodecane diacrylate (trade name: Light Acrylate DCP-A) manufactured by Kyoeisha Chemical Co., Ltd., and neopentyl glycol-modified trimethylolpropane diacrylate (trade name: KAYARAD R-604) manufactured by Nippon Kayaku Co., Ltd., but are not limited thereto. Component (A) may be used alone or in combination of two or more.
[0046] The content of the component (A) is preferably 10 to 70% by mass, more preferably 20 to 60% by mass, based on the total mass of the resin composition, from the viewpoint of the adhesive strength of the resin composition.
[0047] (B) Multifunctional Thiol Compounds
[0048] The resin composition of the present embodiment contains (B) a polyfunctional thiol compound (hereinafter also referred to as "component (B)"). The polyfunctional thiol compound (B) imparts high photocurability to the resin composition. Component (B) is not particularly limited as long as it is difunctional or higher, i.e., has two or more thiol groups. Component (B) preferably contains trifunctional or higher thiol compounds, and more preferably contains trifunctional and / or tetrafunctional thiol compounds. It should be noted that the so-called trifunctional and tetrafunctional thiol compounds are thiol compounds having three and four thiol groups, respectively.
[0049] Examples of the polyfunctional thiol compound include pentaerythritol tetrakis(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), dipentaerythritol hexa(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, pentaerythritol tetrakis(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane, 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, trimethylolpropane tris(3-mercaptobutyrate), and trimethylolethane tris(3-mercaptobutyrate). However, the present invention is not limited to these.
[0050] Examples of commercially available products of the component (B) include trimethylolpropane tris(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: TMMP), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate (manufactured by SC Organic Chemical Co., Ltd.: TEMPIC), pentaerythritol tetrakis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: PEMP), tetraethylene glycol bis(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: EGMP-4), dipentaerythritol hexa(3-mercaptopropionate) (manufactured by SC Organic Chemical Co., Ltd.: DPMP), pentaerythritol tetrakis(3-mercaptobutyrate) (manufactured by Showa Denko K.K.: KARENZ MT (registered trademark) PE1), 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (manufactured by Showa Denko KK: KARENZ MT (registered trademark) NR1), trimethylolpropane tris(3-mercaptobutyrate) (manufactured by Showa Denko KK: KARENZ MT (registered trademark) TPMB), etc., but are not limited to them.
[0051] In addition, examples of the (B) polyfunctional thiol compound include glycoluril compounds represented by the following general formula (1).
[0052] [Chemistry 1]
[0053]
[0054] In the general formula (1), R 1 and R 2 Each is independently hydrogen, an alkyl group having 1 to 10 carbon atoms, or a phenyl group. n is an integer of 0 to 10.
[0055] In addition, the component (B) may be a compound represented by the following chemical formula (2) or chemical formula (3).
[0056] [Chemistry 2]
[0057]
[0058] [Chemistry 3]
[0059]
[0060] The compound represented by the chemical formula (2) or the chemical formula (3) is more preferably used as the component (B).
[0061] In addition, examples of the (B) polyfunctional thiol compound include polyfunctional thiol compounds represented by the general formula (4).
[0062] [Chemistry 4]
[0063]
[0064] In the general formula (4), R 3 , R 4 , R 5 and R 6 are independently hydrogen or C n H 2n SH (n is 2 to 6). In addition, R 3 , R 4 , R 5 and R 6 At least one of them is C n H 2n SH (n is 2 to 6). Regarding n of the multifunctional thiol compound of component (B) represented by the general formula (4), from the viewpoint of curability, it is preferably 2 to 4. In addition, among the multifunctional thiol compounds, from the viewpoint of the balance between the physical properties of the cured product and the curing speed, a mercaptopropyl group in which n is 3 is more preferred. Component (B) represented by the general formula (4) is effective when it is desired to reduce the elastic modulus of the cured product because it has a sufficiently soft skeleton. By adding component (B) represented by the general formula (4), the elastic modulus of the cured product can be controlled, thereby increasing the adhesive strength (especially the peel strength) after curing.
[0065] Commercially available products of the component (B) include, but are not limited to, thiol glycoluril derivatives manufactured by Shikoku Chemical Industries (trade name: TS-G (equivalent to chemical formula (2), thiol equivalent: 100 g / eq), trade name: C3 TS-G (equivalent to chemical formula (3), thiol equivalent: 114 g / eq)), and thiol compounds manufactured by SC Organic Chemicals (trade name: PEPT (equivalent to general formula (4), thiol equivalent: 124 g / eq)).
[0066] Other examples of the component (B) include 1,3,4,6-tetrakis(mercaptomethyl)glycoluril, 1,3,4,6-tetrakis(mercaptomethyl)-3a-methylglycoluril, 1,3,4,6-tetrakis(2-mercaptoethyl)-3a-methylglycoluril, 1,3,4,6-tetrakis(3-mercaptopropyl)-3a-methylglycoluril, 1,3,4,6-tetrakis(mercaptomethyl)-3a,6a-dimethylglycoluril, 1,3,4,6-tetrakis(2-mercaptoethyl)-3a,6a-dimethylglycoluril, 1,3,4,6-tetrakis(3-mercaptopropyl)-3a,6a-dimethylglycoluril, 1,3,4,6-tetrakis(mercaptomethyl)-3a,6a-diphenylglycoluril, 1,3,4,6-tetrakis(2-mercaptoethyl)-3a ,6a-diphenyl glycoluril, 1,3,4,6-tetrakis(3-mercaptopropyl)-3a,6a-diphenyl glycoluril, pentaerythritol tetrapropanethiol, 1,2,3-tris(mercaptomethylthio)propane, 1,2,3-tris(2-mercaptoethylthio)propane, 1,2,3-tris(3-mercaptopropylthio)propane, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, tetrakis(mercaptomethylthiomethyl)methane, tetrakis(2-mercaptoethylthiomethyl) )methane, tetrakis(3-mercaptopropylthiomethyl)methane, 1,1,3,3-tetrakis(mercaptomethylthio)propane, 1,1,2,2-tetrakis(mercaptomethylthio)ethane, 1,1,5,5-tetrakis(mercaptomethylthio)-3-thiapentane, 1,1,6,6-tetrakis(mercaptomethylthio)-3,4-dithiahexane, 2,2-bis(mercaptomethylthio)ethanethiol, 3 -mercaptomethylthio-1,7-dimercapto-2,6-dithiaheptane, 3,6-bis(mercaptomethylthio)-1,9-dimercapto-2,5,8-trithianonane, 3-mercaptomethylthio-1,6-dimercapto-2,5-dithiahexane, 1,1,9,9-tetrakis(mercaptomethylthio)-5-(3,3-bis(mercaptomethylthio)-1-thiapropyl)-3- , 7-dithianonane, tris(2,2-bis(mercaptomethylthio)ethyl)methane, tris(4,4-bis(mercaptomethylthio)-2-thiabutyl)methane, tetrakis(2,2-bis(mercaptomethylthio)ethyl)methane, tetrakis(4,4-bis(mercaptomethylthio)-2-thiabutyl)methane, 3,5,9,11-tetrakis(mercaptomethylthio)-1,13-dimercapto -2,6,8,12-tetrathiatridecane, 3,5,9,11,15,17-hexa(mercaptomethylthio)-1,19-dimercapto-2,6,8,12,14,18-hexathianonadecane, 9-(2,2-bis(mercaptomethylthio)ethyl)-3,5,13,15-tetra(mercaptomethylthio)-1,17-dimercapto-2,6,8,12,14,18-hexathianonadecane10,12,16-hexathiaheptadecane, 3,4,8,9-tetrakis(mercaptomethylthio)-1,11-dimercapto-2,5,7,10-tetrathiaundecane, 3,4,8,9,13,14-hexa(mercaptomethylthio)-1,16-dimercapto-2,5,7,10,12,15-hexathiahexadecane, 8-[bis(mercaptomethylthio)methyl ]-3,4,12,13-tetrakis(mercaptomethylthio)-1,15-dimercapto-2,5,7,9,11,14-hexathiapentadecane, 4,6-bis[3,5-bis(mercaptomethylthio)-7-mercapto-2,6-dithiaheptylthio]-1,3-dithiane, 4-[3,5-bis(mercaptomethylthio)-7-mercapto-2,6-dithiaheptylthio] 1-[4-(6-mercaptomethylthio)-1,3-dithianylthio]-1,3-bis(mercaptomethylthio)propane, 1-[4-(6-mercaptomethylthio)-1,3-dithianylthio]-3-[2,2-bis(mercaptomethylthio)ethyl]-7,9-bis(mercaptomethylthio)-2,4, 6,10-tetrathiaundecane, 3-[2-(1,3-dithiacyclobutyl)]methyl-7,9-bis(mercaptomethylthio)-1,11-dimercapto-2,4,6,10-tetrathiaundecane, 9-[2-(1,3-dithiacyclobutyl)]methyl-3,5,13,15-tetrakis(mercaptomethylthio)-1,17-dimercapto-2,6,8,10,12,16-hexathiaheptadecane, 3-[2-(1,3-dithiacyclobutyl)]methyl-7,9,13,15-tetrakis(mercaptomethylthio)-1,17-dimercapto-2,4,6,10,12,16-hexathiaheptadecane, 4,6-bis[4-(6-mercaptomethylthio)-1,3-dithianylthio]-6-[4-(6- 1,3-dithianethio]-1,3-dithiane, 4-[3,4,8,9-tetrakis(mercaptomethylthio)-11-mercapto-2,5,7,10-tetrathiaundecyl]-5-mercaptomethylthio-1,3-dithiolane, 4,5-bis[3,4-bis(mercaptomethylthio)-6-mercapto-2,5-dithiahexylthio]-1, 3-dithiolane, 4-[3,4-bis(mercaptomethylthio)-6-mercapto-2,5-dithiahexylthio]-5-mercaptomethylthio-1,3-dithiolane, 4-[3-bis(mercaptomethylthio)methyl-5,6-bis(mercaptomethylthio)-8-mercapto-2,4,7-trithiaoctyl]-5-mercaptomethylthio-1,3-dithiolane, 2-{ [3,4-bis(mercaptomethylthio)-6-mercapto-2,5-dithiahexylthio]methyl)-1,3-dithiacyclobutane, 2-[3,4-bis(mercaptomethylthio)-6-mercapto-2,5-dithiahexylthio]mercaptomethylthiomethyl-1,3-dithiacyclobutane, 2-[3,4,8,9-tetrakis(mercaptomethylthio)-11-mercapto-2,5,7,10-tetrathiaundecylthio]mercaptomethylthiomethyl-1,3-dithietane, 2-[3-bis(mercaptomethylthio)methyl-5,6-bis(mercaptomethylthio)-8-mercapto-2,4,7-trithiaoctyl]mercaptomethylthiomethyl-1,3-dithietane, 4-{1-[2-(1,3-dithietanyl)]-3-mercapto-2-thiapropylthio}-5-[1,2-bis(mercaptomethylthio)-4-mercapto-3-thiabutylthio]-1,3-dithiolane, etc., but are not limited to them.
[0067] As the component (B), any one kind may be used, or two or more kinds may be used in combination.
[0068] In this specification, the functional group equivalents such as thiol equivalent and (meth)acryloyl equivalent refer to the molecular weight of the compound per one functional group, and the functional group equivalent number such as thiol equivalent number and (meth)acryloyl equivalent number refer to the number (equivalent number) of functional groups per unit compound mass (feed amount).
[0069] In the resin composition, the ratio of the number of (meth)acryloyl equivalents of component (A) to the number of thiol equivalents of component (B) ([number of (meth)acryloyl equivalents of component (A)] / [number of thiol equivalents of component (B)]) is preferably 0.25 to 3.0, more preferably 0.4 to 2.0, and further preferably 0.5 to 1.5. The thiol equivalent of component (B) is theoretically the number obtained by dividing the molecular weight of component (B) by the number of thiol groups in one molecule. The actual thiol equivalent can be determined, for example, by determining the thiol value using a potential difference. This method is well known and is disclosed, for example, in paragraph 0079 of Japanese Patent Application Laid-Open No. 2012-153794. The thiol group equivalent number of the component (B) is the number (equivalent number) of thiol groups per unit mass (feed amount) of the component (B), and is the quotient obtained by dividing the mass (g) of the multifunctional thiol compound (B) by the thiol equivalent of the thiol compound (when a plurality of thiol compounds are included, the sum of such quotients for each thiol compound). The (meth)acryloyl group equivalent of the (meth)acrylate compound (A) is theoretically equal to the number obtained by dividing the molecular weight of the (meth)acrylate compound by the number of acryloyl groups (or methacryloyl groups) in one molecule. The actual (meth)acryloyl group equivalent can be measured, for example, by NMR. The (meth)acryloyl equivalent of component (A) is the number (equivalent number) of (meth)acryloyl groups per unit mass (feed amount) of component (A), and is the quotient obtained by dividing the mass (g) of the (meth)acrylic acid ester compound (A) by the (meth)acrylic acid ester equivalent of the (meth)acrylic acid ester compound (when a plurality of (meth)acrylic acid ester compounds are included, the sum of such quotients for each (meth)acrylic acid ester compound). The reason why [the (meth)acryloyl equivalent of component (A)] / [the thiol equivalent of component (B)] is in the range of 0.25 to 3.0 is that by reacting a certain amount or more of the (meth)acryloyl group with the thiol group, molecular crosslinking can be sufficiently formed, and high adhesive strength can be easily exhibited.
[0070] (C) Photoradical polymerization initiator
[0071] The resin composition of the present embodiment contains (C) a photoradical polymerization initiator (hereinafter also referred to as "component (C)"). By containing (C) a photoradical polymerization initiator, UV curing can be accelerated.
[0072] (C) As a photoradical polymerization initiator, an alkyl phenone type compound, an acylphosphine oxide type compound etc. are mentioned, for example, but it is not limited to these.
[0073] Examples of the alkylphenone compounds include benzyl dimethyl ketal such as 2,2-dimethoxy-1,2-diphenylethane-1-one (Omnirad 651 manufactured by IGM Resins BV as a commercial product); α-aminoalkylphenone such as 2-methyl-2-morpholino (4-thiomethylphenyl) propane-1-one (Omnirad 907 manufactured by IGM Resins BV as a commercial product); α-hydroxyalkylphenone such as 1-hydroxy-cyclohexyl-phenyl-ketone (Omnirad 184 manufactured by IGM Resins BV as a commercial product); 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butane-1-one (Omnirad 907 manufactured by IGM Resins BV as a commercial product); 379EG), 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone (commercially available product: Omnirad 369 manufactured by IGM Resins BV), etc., but the present invention is not limited to these.
[0074] Examples of acylphosphine oxide compounds include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (commercially available as Omnirad TPO H manufactured by IGM Resins BV), bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (commercially available as Omnirad 819 manufactured by IGM Resins BV), etc., but are not limited to these.
[0075] (C) The photoradical polymerization initiator includes, in addition to the above-mentioned photoradical polymerization initiators, 2-hydroxy-2-methyl-1-phenylpropane-1-one, diethoxyacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, 1-(4-dodecylphenyl)-2-hydroxy-2-methylpropane-1-one, 4-(2-hydroxyethoxy)-phenyl(2-hydroxy-2-propyl)ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin The present invention also includes benzoyl ether, benzyl dimethyl ketal, benzophenone, benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3'-dimethyl-4-methoxybenzophenone, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, methyl benzoylformate, benzyl, camphorquinone, etc., but is not limited to them.
[0076] The content of the component (C) is preferably 0.01 to 40% by mass, more preferably 0.1 to 20% by mass, based on the total mass of the resin composition, from the viewpoint of the curing rate and pot life of the resin composition.
[0077] (D) Thermal curing accelerator
[0078] The resin composition of the present embodiment includes (D) a thermal curing accelerator containing an azabicyclic compound having a bridgehead nitrogen (hereinafter also referred to as "component (D)"). By including (D) a thermal curing accelerator containing an azabicyclic compound having a bridgehead nitrogen, a resin composition can be obtained, which can provide a cured product that suppresses the remaining unreacted components after the second stage of thermal curing following the UV curing in the first stage, suppresses the occurrence of exudation and outgassing, and has high dimensional stability during additional heating. Since the occurrence of exudation and outgassing is suppressed in this way, contamination of peripheral components is suppressed. In addition, since the dimensional stability during additional heating is high, position deviation and optical axis deviation are suppressed.
[0079] Examples of the azabicyclic compound having a bridgehead nitrogen contained in the (D) thermal curing accelerator include compounds represented by the following general formula (5).
[0080] [Chemistry 5]
[0081]
[0082] In the general formula (5), Q is CR (wherein R is a hydrogen atom (H) or a hydrocarbon chain such as an alkyl group), a nitrogen atom (N), or a skeleton of the following formula (6):
[0083] [Chemistry 6]
[0084]
[0085] (In formula (6), each single bond of the carbon atom is bonded to X and Y of formula (5), and the single bond of the nitrogen atom is bonded to Z of formula (5).)
[0086] X, Y and Z are each independently -(CH2) n -(n=0 or 1 or more), and at least two of X, Y and Z are n=1 or more. In addition, the hydrogen atoms on the hydrocarbon chains of Q, X, Y and Z may be substituted by a substituent selected from an alkyl group which may be substituted, a hydroxyl group and an amino group, or may be substituted by an oxygen atom (O) to form a carbonyl group together with the carbon atoms of the hydrocarbon chain. The substituent of the alkyl group which may be substituted is an alkyl group, a hydroxyl group or an amino group.
[0087] In one embodiment, the preferred compound of formula (5) is a saturated azabicyclic compound having a bridgehead nitrogen, namely,
[0088] Q is CR (where R is a hydrogen atom (H) or a hydrocarbon chain such as an alkyl group) or a nitrogen atom (N),
[0089] X, Y and Z are each independently -(CH2) n -(n=2 or more, preferably n=2). In addition, the hydrogen atoms on the hydrocarbon chains of Q, X, Y, and Z may be substituted by a substituent selected from a substituted alkyl, hydroxyl, and amino group, or may be substituted by an oxygen atom (O) to form a carbonyl group together with the carbon atoms of the hydrocarbon chain.
[0090] In a certain embodiment, another preferred compound of the general formula (5) is the following unsaturated azabicyclic compound having a bridgehead nitrogen, namely,
[0091] Q is a skeleton of the following formula (6):
[0092] [Chemistry 7]
[0093]
[0094] (In formula (6), each single bond of the carbon atom is bonded to X and Y of formula (5), and the single bond of the nitrogen atom is bonded to Z of formula (5).)
[0095] X and Z are each independently -(CH2) n -(n=1 or more, preferably 2 to 6.) hydrocarbon chain, Y is -(CH2) n -(n=0). In addition, the hydrogen atoms on the hydrocarbon chains of Q, X, and Z may be substituted by a substituent selected from substituted alkyl, hydroxyl, and amino groups, or may be substituted by oxygen atoms (O) to form a carbonyl group together with the carbon atoms of the hydrocarbon chain.
[0096] The azabicyclic compounds having bridgehead nitrogen also include compounds containing a moiety represented by the general formula (5). The compound containing a moiety represented by the general formula (5) refers to a compound in which the compound represented by the general formula (5) is bonded or linked to a second moiety via a covalent bond. The second moiety is not particularly limited, and examples thereof include saturated or unsaturated cyclic hydrocarbons, saturated or unsaturated heterocycles, aryl groups, heteroaryl groups, and the like.
[0097] Examples of the compound of formula (5) include 1,4-diazabicyclo[2.2.2]octane (DABCO (registered trademark)), 1-azabicyclo[2.2.2]octane-3-ol (common name: 3-quinuclidinol), 1,4-diazabicyclo[2.2.2]octane-2-methanol, 1-azabicyclo[2.2.2]octane-3-one (common name: 3-quinuclidinone), 1,4-diazabicyclo[2.2.2]octane-2-ol, 1,8-diazabicyclo[5.4.0]-undec-7-ene (DBU (registered trademark)), and 1,5-diazabicyclo[4.3.0]non-5-ene (DBN (registered trademark)). Component (D) may be used alone or in combination of two or more.
[0098] In the case of using a thermosetting accelerator containing an imidazole compound widely used as a thermosetting accelerator for a thermosetting resin composition, it is found that sufficient reactivity is shown in the case of only thermosetting, but the reactivity during thermosetting after UV curing is not high, and a lot of low molecular components remain in the cured product. It can be considered that this is because, generally speaking, in the area cured by UV irradiation curing in the first stage, most of the molecules are immobilized, so the molecular motion is suppressed in the thermosetting of the second stage, and the thermosetting component requires more thermal energy for reaction compared with the case of only thermosetting. The inventors and others found that by using the thermosetting accelerator (D) containing an azabicyclic compound with bridgehead nitrogen in the present embodiment, the reactivity during thermosetting after UV curing is also high, and in the cured product after the thermosetting of the second stage after the UV curing in the first stage, the remaining of the unreacted components is suppressed. Its mechanism is not limited, but it can be inferred as shown below.
[0099] In a photo- and thermosetting resin composition or adhesive that is cured by a two-stage curing process, there is an area where UV curing is incomplete after UV irradiation in the first stage. The heat-based curing property of the thermosetting functional group remaining in the incomplete UV curing area depends on the type of thermosetting accelerator. Azabicyclic compounds with bridgehead nitrogen are also prone to react in the thermosetting process after UV curing due to their high alkalinity. In particular, saturated azabicyclic compounds with bridgehead nitrogen are preferred due to the small steric hindrance of the bridgehead nitrogen. In addition, saturated diazabicyclic compounds with bridgehead nitrogen are more preferred due to their high reaction probability due to the two bridgehead nitrogens. On the other hand, for commonly used thermosetting accelerators such as imidazole compounds and their derivatives, they have sufficient curing property as thermosetting accelerators if only the thermosetting process is used, but they are low in alkalinity compared to azabicyclic compounds with bridgehead nitrogen, so thermosetting reactions are not easy to occur after UV curing.
[0100] In addition, the inventors have found that by using (D) a thermal curing accelerator containing an azabicyclic compound having a bridgehead nitrogen, the resin composition can be thermally cured at a lower temperature. For example, when using a thermal curing accelerator containing an imidazole compound, although the low-temperature curability of the resin composition is excellent, the curing under about 80°C is the limit. When using (D) a thermal curing accelerator containing an azabicyclic compound having a bridgehead nitrogen, the resin composition can be thermally cured at a temperature below 80°C, for example, above 50°C and below 80°C. The resin composition of this embodiment can also be thermally cured at a temperature above 80°C. In the case where the resin composition is used in the manufacturing process of a semiconductor device or an electronic component, especially an image sensor module, by using (D) a thermal curing accelerator containing an azabicyclic compound having a bridgehead nitrogen, the resin composition can be thermally cured at a lower temperature, thereby preventing thermal damage to module components (such as lenses, etc.).
[0101] From the viewpoint of curability, the azabicyclic compound with bridgehead nitrogen contained in the (D) thermal curing accelerator is preferably a saturated azabicyclic compound with bridgehead nitrogen. As saturated azabicyclic compounds with bridgehead nitrogen, compounds with a 1,4-diazabicyclooctane skeleton and compounds with a quinuclidine skeleton can be cited. From the viewpoint of increasing the probability of reaction, compounds with a 1,4-diazabicyclooctane skeleton as a compound with two bridgehead nitrogens are preferred. As such compounds, specifically, 1,4-diazabicyclo[2.2.2]octane, 1,4-diazabicyclo[2.2.2]octane-2-methanol, 1,4-diazabicyclo[2.2.2]octane-2-ol, 1,4-diazabicyclo[2.2.2]octane. In addition, from the viewpoint of affinity with the resin, compounds with a quinuclidine skeleton as a compound with one bridgehead nitrogen are preferred. Specifically, from the viewpoint of affinity with a resin having high polarity, 1-azabicyclo[2.2.2]octan-3-ol is preferred, and from the viewpoint of affinity with a resin having low polarity, 1-azabicyclo[2.2.2]octan-3-one is preferred.
[0102] The content of the component (D) is preferably 0.01 to 40% by mass, more preferably 0.05 to 20% by mass, based on the total mass of the resin composition, from the viewpoint of the curing rate and usable life of the resin composition.
[0103] From the viewpoint of latentization, (D) heat curing accelerator can be a substance that disperses the heat curing accelerating compound in the epoxy compound, or a substance carried between the layers of the layered inorganic compound. The so-called latent curing accelerator is a substance that is inactive at room temperature and acts as a curing catalyst after being activated by heating. As a representative example of a commercial product of a latent heat curing accelerator containing component (D), "NOVACURE HXA5945HP" (trade name of Asahi Kasei Corporation) can be cited. As the epoxy compound, the following (E) epoxy compound can be used.
[0104] The resin composition of the present embodiment may also contain a heat curing accelerator other than component (D) as long as the effect of the present invention is not impaired. Examples thereof include imidazole compounds that are solid at room temperature; solid dispersed amine adduct-based latent curing catalysts such as reaction products of amine compounds and epoxy compounds (amine-epoxy adduct systems); reaction products of amine compounds and isocyanate compounds or urea compounds (urea-type adduct systems), etc.
[0105] Representative examples of commercially available products of the thermosetting accelerator other than component (D) include, for amine-epoxy adducts (amine adducts), "AMICURE PN-23" (trade name of Ajinomoto Fine-Techno Co., Ltd.), "AMICURE PN-40" (trade name of Ajinomoto Fine-Techno Co., Ltd.), "AMICURE PN-50" (trade name of Ajinomoto Fine-Techno Co., Ltd.), "HARDNER X-3661S" (trade name of ACR Corporation), "HARDNER X-3670S" (trade name of ACR Corporation), "NOVACURE HX-3742" (trade name of Asahi Kasei Corporation), "NOVACURE HX-3721" (trade name of Asahi Kasei Corporation), "NOVACURE HXA3922HP" (trade name of Asahi Kasei Corporation), "NOVACURE HXA9322HP" (trade name of Asahi Kasei E-Materials Co., Ltd.), "FUJICURE FXR-1121" (trade name of T&K TOKA Co., Ltd.), etc., and as for the urea type adduct system, "FUJICURE FXE-1000" (trade name of T&K TOKA Co., Ltd.), "FUJICURE FXR-1030" (trade name of T&K TOKA Co., Ltd.), etc. can be mentioned, but it is not limited to these.
[0106] It should be noted that, when using a thermosetting accelerator provided in the form of a dispersion dispersed in an epoxy compound as component (D) and a thermosetting accelerator other than component (D), it should be noted that the amount of the epoxy compound in which the thermosetting accelerator is dispersed is also included in the amount of component (E) of the resin composition of this embodiment.
[0107] (E) Epoxy compounds
[0108] The resin composition of the present embodiment may further include (E) an epoxy compound (hereinafter also referred to as "component (E)"). The epoxy compound (E) is not particularly limited as long as it is difunctional or more, i.e., has more than two epoxy groups, and conventionally used epoxy resins can be used as component (E). It should be noted that the so-called epoxy resin is a general term for thermosetting resins that can be cured by cross-linking and networking using epoxy groups present in the molecule, including prepolymer compounds before curing. In a certain embodiment of the present embodiment, component (E) includes a difunctional epoxy compound.
[0109] Since the epoxy compound cannot undergo a crosslinking reaction due to the excitation of the (C) photoradical polymerization initiator, it remains in an unreacted state in the cured region after UV irradiation of the resin composition, and the molecular motion is suppressed. Therefore, the curing reaction of the epoxy compound becomes difficult in the second stage of thermal curing. Since the resin composition of the present embodiment includes (D) a thermal curing accelerator including an azabicyclic compound having a bridgehead nitrogen, it is possible to promote the thermal curing of the epoxy compound in a state where the molecular motion is suppressed.
[0110] (E) Epoxy compounds can be roughly divided into aliphatic epoxy compounds and aromatic epoxy compounds. In the present embodiment, (E) epoxy compound preferably includes an aromatic epoxy compound.
[0111] Examples of aliphatic epoxy compounds include:
[0112] - diepoxy compounds such as (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, polytetramethylene ether glycol diglycidyl ether, glycerol diglycidyl ether, neopentyl glycol diglycidyl ether, cyclohexane type diglycidyl ether, and dicyclopentadiene type diglycidyl ether;
[0113] - triepoxy compounds such as trimethylolpropane triglycidyl ether and glycerol triglycidyl ether;
[0114] - alicyclic epoxy compounds such as vinyl (3,4-cyclohexene) dioxide and 2-(3,4-epoxycyclohexyl)-5,1-spiro-(3,4-epoxycyclohexyl)-m-dioxane;
[0115] - glycidylamine-type epoxy compounds such as tetraglycidylbis(aminomethyl)cyclohexane;
[0116] - Hydantoin type epoxy compounds such as 1,3-diglycidyl-5-methyl-5-ethylhydantoin; and
[0117] Epoxy compounds having a silicone skeleton such as -1,3-bis(3-glycidoxypropyl)-1,1,3,3-tetramethyldisiloxane, etc., but are not limited to these.
[0118] Among the above examples, the so-called "cyclohexane type diglycidyl ether" means a compound having a structure in which two glycidyl groups are bonded to a divalent saturated hydrocarbon group having a cyclohexane ring as a parent structure via an ether bond. The so-called "dicyclopentadiene type diglycidyl ether" means a compound having a structure in which two glycidyl groups are bonded to a divalent saturated hydrocarbon group having a dicyclopentadiene skeleton as a parent structure via an ether bond. The aliphatic multifunctional epoxy compound is preferably a compound having an epoxy equivalent of 90 to 450 g / eq. In addition, as a cyclohexane type diglycidyl ether, cyclohexanedimethanol diglycidyl ether is particularly preferred.
[0119] Aromatic epoxy compounds are epoxy compounds having a structure containing an aromatic ring such as a benzene ring. There are many such compounds in conventionally used epoxy resins such as bisphenol A epoxy resins. Examples of aromatic epoxy compounds include:
[0120] -Bisphenol A type epoxy compounds;
[0121] - branched multifunctional bisphenol A type epoxy compounds such as p-glycidyloxyphenyl dimethyl trisphenol A diglycidyl ether;
[0122] -Bisphenol F type epoxy compounds;
[0123] - Novolac epoxy compounds;
[0124] -Tetrabromobisphenol A type epoxy compounds;
[0125] -Fluorene epoxy compounds;
[0126] -biphenyl aralkyl epoxides;
[0127] - Diepoxides such as 1,4-phenylenedimethanol diglycidyl ether;
[0128] - biphenyl type epoxy compounds such as 3,3′,5,5′-tetramethyl-4,4′-diglycidyloxybiphenyl;
[0129] - glycidylamine type epoxy compounds such as diglycidylaniline, diglycidyltoluidine, triglycidyl-p-aminophenol, tetraglycidyl-m-xylylenediamine; and
[0130] -Epoxy compounds containing naphthalene rings, etc., but are not limited to them. In the present embodiment, from the viewpoint of compatibility with thiol compounds, component (E) preferably contains aromatic epoxy compounds compared to aliphatic epoxy compounds. As aromatic epoxy compounds, bisphenol F type epoxy compounds, bisphenol A type epoxy compounds and glycidylamine type epoxy compounds are preferred, among which compounds with an epoxy equivalent of 90 to 300 g / eq are more preferred, compounds with an epoxy equivalent of 110 to 300 g / eq are particularly preferred, and compounds with an epoxy equivalent of 150 to 220 g / eq are most preferred. (E) Epoxy compounds can be used alone or in combination of two or more.
[0131] When the resin composition contains (E) an epoxy compound, in the resin composition, the ratio of the sum of the number of (meth)acryloyl group equivalents of the component (A) and the number of epoxy group equivalents of the component (E) to the number of thiol group equivalents of the component (B) (([number of (meth)acryloyl group equivalents of the component (A)] + [number of epoxy group equivalents of the component (E)]) / [number of thiol group equivalents of the component (B)]) is preferably 0.25 to 3.0, more preferably 0.4 to 2.0, and even more preferably 0.5 to 1.5.
[0132] In addition, when the resin composition contains the (E) epoxy compound, in the resin composition, the ratio of the number of (meth)acryloyl equivalents of the component (A) to the number of epoxy equivalents of the component (E) ([number of (meth)acryloyl equivalents of the component A)] / [number of epoxy equivalents of the component (E)]) is preferably 1 to 100, more preferably 2 to 80, further preferably 3 to 50, particularly preferably 3 to 40, and most preferably 5 to 35.
[0133] The epoxy equivalent of component (E) is theoretically the number obtained by dividing the molecular weight of component (E) by the number of epoxy groups in one molecule. The actual epoxy equivalent can be calculated using the method described in JIS K7236. The epoxy equivalent number of component (E) is the number (equivalent number) of epoxy groups per unit mass (feed amount) of component (E), and is the quotient obtained by dividing the mass (g) of the epoxy compound of component (E) by the epoxy equivalent of the epoxy compound (when multiple epoxy compounds are included, it is the sum of such quotients for each epoxy compound).
[0134] Alternatively, when the resin composition contains the (E) epoxy compound, the content is preferably 1.5 to 40% by mass, more preferably 2 to 30% by mass, and even more preferably 3 to 20% by mass, based on the total mass of the resin composition.
[0135] (F) Filling
[0136] The resin composition of the present embodiment may contain (F) filler (hereinafter also referred to as "component (F)") within the range that does not impair the effect of the present invention. By containing (F) filler in the resin composition, the linear expansion coefficient of the cured product obtained by curing the resin composition can be reduced, and the heat cycle resistance is improved. In addition, if it is a filler with a low elastic modulus, the stress generated in the cured product can be alleviated, and the long-term reliability is improved. (F) Filler can be roughly divided into inorganic fillers and organic fillers.
[0137] The inorganic filler is composed of a granular body formed by an inorganic material, and is not particularly limited as long as it is a material having the effect of reducing the linear expansion coefficient by addition. As inorganic materials, silicon dioxide, talc, aluminum oxide, aluminum nitride, calcium carbonate, aluminum silicate, magnesium silicate, magnesium carbonate, barium sulfate, barium carbonate, lime sulfate, aluminum hydroxide, calcium silicate, potassium titanate, titanium oxide, zinc oxide, silicon carbide, silicon nitride, boron nitride, etc. can be used. Any one of the inorganic fillers can be used, or two or more can be used in combination. As an inorganic filler, a silicon dioxide filler is preferably used from the aspect of being able to increase the filling amount. Silica is preferably amorphous silicon dioxide.
[0138] The inorganic filler is preferably a material whose surface is surface-treated with a coupling agent such as a silane coupling agent. Thereby, the viscosity of the resin composition can be adjusted to an appropriate range.
[0139] Examples of the organic filler include polytetrafluoroethylene (PTFE) fillers, silicone fillers, acrylic fillers, styrene fillers, etc. The organic filler may be surface treated.
[0140] The shape of the filler is not particularly limited, and may be any of spherical, flaky, needle-shaped, and irregular shapes.
[0141] In one embodiment, the average particle size of the filler is preferably 5.0 μm or less, more preferably 4.0 μm or less, and further preferably 3.0 μm or less. In this specification, the average particle size refers to the volume-based median particle size (d 50), or as a value obtained by the number average of 50 measured values arbitrarily selected from an observation image obtained by a transmission electron microscope (TEM) or a scanning electron microscope (SEM). By setting the average particle size of the filler to below the upper limit, the sedimentation of the filler can be suppressed, and the formation of coarse particles can be suppressed, and the clogging of the nozzle of the dispensing machine can be suppressed. The lower limit of the average particle size of the filler is not particularly limited, but from the perspective of the viscosity of the resin composition, it is preferably 0.005μm or more, and more preferably 0.1μm or more. In a certain mode of the present embodiment, the average particle size of the CF) filler is preferably 0.01μm to 5.0μm, and more preferably 0.1μm to 3.0μm. Fillers with different average particle sizes can also be used in combination. For example, a filler with an average particle size of 0.005μm or more and less than 0.1μm and a filler with an average particle size of 0.1μm to 5.0μm can be used in combination.
[0142] The content of the filler (F) in the resin composition of the present embodiment is preferably 0.5 to 80% by mass, more preferably 1 to 70% by mass, relative to the total mass of the resin composition. By setting the content of the filler (F) to the above range, the heat cycle resistance is improved, and the viscosity of the resin composition is set to an appropriate range, thereby improving the applicability in the dispensing machine.
[0143] (G) Stabilizer
[0144] The resin composition of the present embodiment may contain (G) a stabilizer (hereinafter also referred to as "component (G)") within a range that does not impair the effects of the present invention. The (G) stabilizer is a substance used to improve the stability of the resin composition during storage, and is added to suppress the occurrence of polymerization reactions caused by unexpected free radicals and alkaline components. Typically, as the (G) stabilizer, free radical inhibitors and anionic inhibitors can be cited.
[0145] As the free radical inhibitor, a known inhibitor can be used, for example, N-nitroso-N-phenylhydroxylamine aluminum, triphenylphosphine, p-methoxyphenol and hydroquinone etc. can be mentioned, but it is not limited to them. In addition, the known free radical inhibitors disclosed in Japanese Unexamined Patent Publication No. 2010-117545 and Japanese Unexamined Patent Publication No. 2008-184514 etc. can also be used. Any one of the free radical inhibitors can be used, or two or more can be used in combination.
[0146] When a radical polymerization inhibitor is contained, the content of the radical polymerization inhibitor is preferably 0.0001 to 5% by mass, more preferably 0.001 to 3% by mass, based on the total mass of the resin composition, from the viewpoint of usable time.
[0147] As anionic polymerization inhibitor, known polymerization inhibitors can be used, for example, borate compounds and strong acids can be used. As specific examples of anionic polymerization inhibitors, trimethyl borate, triethyl borate, tri-n-propyl borate, triisopropyl borate, trifluoromethanesulfonic acid, maleic acid, methanesulfonic acid, barbituric acid, difluoroacetic acid, trichloroacetic acid, phosphoric acid, dichloroacetic acid, etc. can be cited, but are not limited to them. Among them, preferred anionic polymerization inhibitors are at least one selected from tri-n-propyl borate, triisopropyl borate and barbituric acid. In addition, anionic polymerization inhibitors can also use known polymerization inhibitors disclosed in Japanese Patent Publication No. 2010-117545, Japanese Patent Publication No. 2008-184514, Japanese Patent Publication No. 2017-171804, etc. Anionic polymerization inhibitors can use any one, or two or more can be used in combination.
[0148] When an anionic polymerization inhibitor is contained, the content of the anionic polymerization inhibitor is preferably 0.001 to 5% by mass, more preferably 0.01 to 3% by mass, based on the total mass of the resin composition.
[0149] (H) Thermal radical polymerization initiator
[0150] The resin composition of the present embodiment may contain (H) a thermal radical polymerization initiator (hereinafter also referred to as "component (H)") within a range that does not impair the effects of the present invention. By containing a thermal radical polymerization initiator in the resin composition, the resin composition can be cured by heating for a short time. The thermal radical polymerization initiator that can be used is not particularly limited. Well-known materials can be used. Specific examples of the thermal radical polymerization initiator include diisopropylbenzene peroxide, tert-butylisopropylbenzene peroxide, 1,3-bis(2-tert-butylperoxyisopropyl)benzene, or dialkyl peroxides such as 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 1,1-bis(tert-butylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy) Cyclohexane, 2,2-bis(tert-butylperoxy)butane, 4,4-bis(tert-butylperoxy)butyl valerate, or peroxy ketal such as ethyl 3,3-(tert-butylperoxy)butyrate, and peroxy alkyl esters such as tert-butyl peroxy-2-ethylhexanoate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, tert-butyl peroxymaleate, or tert-butyl peroxybenzoate, but are not limited thereto. As the thermal free radical polymerization initiator, a single substance may be used, or two or more substances may be used in combination.
[0151] When (H) a thermal radical polymerization initiator is contained, the content of the (H) thermal radical polymerization initiator is preferably 0.01 to 5% by mass, more preferably 0.1 to 3% by mass, based on the total mass of the resin composition.
[0152] (I) Other additives
[0153] In the resin composition, carbon black, titanium black, silane coupling agent, ion trapping agent, leveling agent, antioxidant, defoaming agent, or other additives can be combined in the range of not damaging the characteristics of the resin composition of the present embodiment and as needed. In addition, in the resin composition, viscosity modifiers, flame retardants, or solvents can also be combined. Here, carbon black and titanium black can be used as light-shielding materials. From the perspective of achieving both light-shielding and UV curing (curing depth), titanium black can be used appropriately. As an example of titanium black, titanium black 12S (Mitsubishi Materials Electronic Chemicals Co., Ltd.), titanium black 13M (Mitsubishi Materials Co., Ltd.) and titanium black 13M-C (Mitsubishi Materials Co., Ltd.), TilackD (Ako Chemical Co., Ltd.) can be cited, but it is not limited to them. Titanium black 13M is particularly preferred. The type and amount of each additive are as shown in the usual method.
[0154] The method for manufacturing the resin composition of the present embodiment is not particularly limited. The resin composition can be obtained by, for example, stirring, melting, mixing and dispersing component (A) to component (D), component (E), component (F), component (G), component (H) and / or (I) other additives, etc., simultaneously or separately, as required, applying heat treatment. The devices used for these mixing, stirring and dispersing are not particularly limited. A crusher, Henschel mixer, three-roll mill, ball mill, planetary mixer, or bead mill equipped with a stirring device and a heating device can be used. In addition, these devices can also be used in combination as appropriate.
[0155] The resin composition obtained in this way is photocurable and thermosetting. Regarding the thermosetting temperature of the resin composition, when used in an image sensor module, it is preferably 50 to 120°C, more preferably 50 to 90°C, further preferably 50 to 80°C, and particularly preferably 50 to 70°C. By making the resin composition of this embodiment contain component (D), during the thermosetting of the second stage after the UV curing of the first stage, not only the thermosetting under 80°C but also the thermosetting under 60°C can be performed.
[0156] The resin composition of the present embodiment can be used as an adhesive, sealing material, dam agent and raw materials thereof for fixing, bonding or protecting parts, and is suitable for being set as a one-liquid type. Here, the dam agent is pre-formed on the periphery of the substrate before sealing multiple semiconductor chips with a low-viscosity filler on the substrate. By forming a dam based on the dam agent, the outflow of the low-viscosity filler that seals multiple semiconductor chips can be suppressed. In addition, the adhesive containing the resin composition of the present embodiment can also achieve good bonding to engineering plastics, ceramics and metals.
[0157] [Adhesive or sealing material]
[0158] The adhesive or sealing material of the second embodiment of the present invention comprises the resin composition of the first embodiment. The adhesive or sealing material can achieve good bonding to engineering plastics, ceramics and metals. The adhesive or sealing material of this embodiment is preferably used for fixing, bonding or protecting components constituting an image sensor or camera module.
[0159] [Cured product of resin composition, adhesive or sealing material]
[0160] The cured product according to the third embodiment of the present invention is a cured product obtained by curing the resin composition according to the first embodiment or the adhesive or sealing material according to the second embodiment.
[0161] [Semiconductor devices, electronic components]
[0162] The semiconductor device or electronic component of the fourth embodiment of the present invention includes the cured product of the third embodiment described above. Here, the so-called semiconductor device refers to all devices that can function by utilizing semiconductor characteristics, including electronic components, semiconductor circuits, modules assembled with them, electronic equipment, etc. Semiconductor devices or electronic components can include, for example, HDDs, semiconductor elements, sensor modules such as image sensor modules, camera modules, semiconductor modules, integrated circuits, etc., but are not limited to them. In a certain embodiment, the semiconductor device or electronic component can be an image sensor or a camera module.
[0163] Example
[0164] Hereinafter, the present invention will be described in further detail using Examples and Comparative Examples, but the present invention is not limited to these Examples. It should be noted that in the following Examples, parts and % represent parts by mass and % by mass unless otherwise indicated.
[0165] [Examples 1 to 15, Comparative Examples 1 to 2]
[0166] A resin composition was prepared by mixing the given amounts of the components using a three-roll mill according to the formulation shown in Table 1. In Table 1, the amount of each component is expressed in parts by mass (unit: g). The components used in Examples and Comparative Examples are as follows.
[0167] (A) (Meth)acrylate compound (ingredient (A))
[0168] (A-1): dimethylol-tricyclodecane diacrylate (trade name: Light Acrylate DCP-A, manufactured by Kyoeisha Chemical Co., Ltd., acryloyl equivalent: 152 g / eq)
[0169] (A-2): Neopentyl glycol-modified trimethylolpropane diacrylate (trade name: KAYARAD R-604, manufactured by Nippon Kayaku Co., Ltd., acryloyl equivalent: 163 g / eq)
[0170] (A-3): Bis(trimethylol)propane tetraacrylate (trade name: EBECRYL 140, manufactured by Daicel Allnex Co., Ltd., acryloyl equivalent: 117 g / eq)
[0171] (B) Polyfunctional thiol compound (component (B))
[0172] (B-1): Pentaerythritol tetrakis(3-mercaptopropionate) (trade name: PEMP, manufactured by SC Organic Chemicals, thiol equivalent: 122 g / eq)
[0173] (B-2): a polyfunctional thiol compound of the general formula (4) (trade name: PEPT, manufactured by SC Organic Chemicals, thiol equivalent: 124 g / eq)
[0174] (B-3): A polyfunctional thiol compound of the chemical formula (3) (trade name: C3 TS-G, manufactured by SC Organic Chemicals, thiol equivalent: 114 g / eq)
[0175] (B-4): Pentaerythritol tetrakis(3-mercaptobutyrate) (trade name: KARENZ MT (registered trademark) PE1, manufactured by Showa Denko K.K., mercaptan equivalent: 136 g / eq)
[0176] (C) Photoradical initiator (ingredient (C))
[0177] (C-1): 1-Hydroxy-cyclohexyl-phenyl-ketone (trade name: Omnirad 184, manufactured by IGM Resins Co., Ltd.)
[0178] (C-2): 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (trade name: Omnirad TPO H, manufactured by IGM Resins BV)
[0179] (D) A thermal curing accelerator comprising an azabicyclic compound having a bridgehead nitrogen (ingredient (D))
[0180] (D-1): A heat curing accelerator containing 1,4-diazabicyclo[2.2.2]octane (DABCO (registered trademark)) (trade name: NOVACURE HXA5945HP, manufactured by Asahi Kasei Corporation)
[0181] (D-2): A thermal curing accelerator containing 1,4-diazabicyclo[2.2.2]octane (DABCO (registered trademark)) (1,4-diazabicyclo[2.2.2]octane itself, obtained from Tokyo Chemical Industry Co., Ltd.)
[0182] (D-3): A thermal curing accelerator comprising 1-azabicyclo[2.2.2]octan-3-ol (common name: 3-quinuclol) (1-azabicyclo[2.2.2]octan-3-ol itself, obtained from Tokyo Chemical Industry Co., Ltd.)
[0183] (D-4): A thermal curing accelerator containing 1,8-diazabicyclo[5.4.0]-undec-7-ene (DBU (registered trademark)) (1,8-diazabicyclo[5.4.0]-undec-7-ene itself, obtained from Tokyo Chemical Industry Co., Ltd.)
[0184] (D') Thermal curing accelerator other than component (D) (component (D'))
[0185] (D'-1): A heat curing accelerator containing an imidazole compound (trade name: NOVACURE HXA3922HP, manufactured by Asahi Kasei E-Materials Co., Ltd.)
[0186] (D'-2): A thermal curing accelerator containing 2-ethyl-4-methylimidazole (trade name: CURESOLE 2E4MZ, manufactured by Shikoku Chemical Industry Co., Ltd.)
[0187] Components (D-1) and (D'-1) among the above-mentioned thermal curing accelerators (D) and (D') are provided in the form of a dispersion in which a particulate curing accelerating compound is dispersed in an epoxy compound (a mixture of a bisphenol A type epoxy compound and a bisphenol F type epoxy compound). The mass parts of components (D-1) and (D'-1) in Table 1 are the mass parts of the components after removing the mass parts of the epoxy compound mixture from the mass parts of the dispersion. The epoxy compound constituting the dispersion is treated as a compound forming a part of component (E), and the epoxy compound in (D-1) is set as component (E-1), and the epoxy compound in (D'-1) is set as component (E-2). The mass parts of (E-1) and (E-2) in Table 1 are the mass parts of the epoxy compounds in components (D-1) and (D'-1).
[0188] ·Epoxy compound (ingredient (E))
[0189] (E-1) A mixture of a bisphenol A epoxy compound and a bisphenol F epoxy compound (epoxy equivalent: 180 g / eq)
[0190] (E-2): A mixture of a bisphenol A epoxy compound and a bisphenol F epoxy compound (epoxy equivalent: 180 g / eq)
[0191] (E-3) A mixture of a bisphenol A epoxy compound and a bisphenol F epoxy compound (trade name: EXA-835LV, manufactured by DIC Corporation, epoxy equivalent: 165 g / eq)
[0192] Filler (ingredient (F))
[0193] (F-1): Silica filler (trade name: SE2300, average particle size 0.6 μm, manufactured by ADMATECHS Co., Ltd.)
[0194] (F-2): Calcium carbonate filler (trade name: CS4NA, average particle size: <0.5 μm, manufactured by Ube Materials Co., Ltd.)
[0195] (F-3): Hydrophobic fumed silica (trade name: CAB-O-SIL (registered trademark) TS720, manufactured by CABOT, average particle size: 12 nm)
[0196] Stabilizer (ingredient (G))
[0197] (G-1): triisopropyl borate (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0198] (G-2): N-nitroso-N-phenylhydroxylamine aluminum (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0199] In Examples and Comparative Examples, the properties of the resin compositions and cured products were measured as follows.
[0200] [Residual heat storage obtained by DSC (differential scanning calorimetry)]
[0201] The resin compositions of the examples and comparative examples were degassed in a vacuum and irradiated with UV at a dose of 2000 mJ / cm 2 (UV wavelength: 365nm, LED lamp) After UV curing, heat curing was performed at 80°C / 60 minutes in a blower dryer to obtain a cured resin. 5 mg of the cured resin was collected and heated from 30°C to 250°C at a heating rate of 10°C / minute under nitrogen conditions using DSC to obtain an exothermic curve. In the case of a residual exothermic peak, the exothermic peak was integrated to calculate the residual heat storage. The case where the residual heat storage is less than 25 J / g is judged as the residual unreacted components being suppressed and is set to "A", and the case where it is greater than 25 J / g is judged as the residual unreacted components being more and is set to "F".
[0202] [Evaluation of curability at 60°C]
[0203] The 60°C curability of the prepared resin composition was evaluated by dropping one drop of the resin composition to prepare a sample and observing the state of the sample when heated at 60°C for 60 minutes. If the sample was solid and had no stringing, it was judged to be fully cured and set to "A", and if there was stringing even if it became solid, it was judged to be worse than "A" and set to "B", and if the hemispherical sample did not become solid, it was judged to be uncured and set to "F". The results are shown in Table 1.
[0204] [Table 1-1]
[0205]
[0206] [Table 1-2]
[0207]
[0208] [Table 1-3]
[0209]
[0210] The resin compositions of Examples 1 to 15 contain (D) a thermal curing accelerator containing an azabicyclic compound having a bridgehead nitrogen, and thus can suppress the remaining unreacted components in the cured product after the second stage thermal curing following the first stage UV curing, and the resin compositions can be thermally cured at 60°C.
[0211] On the other hand, in Comparative Examples 1 and 2 in which the resin composition contained a thermosetting accelerator other than component (D), more unreacted components remained in the cured product after the second step of thermal curing following the first step of UV curing, and the resin composition could not be cured at 60°C.
[0212] [Rate of increase in strength of cured product due to additional heating]
[0213] The resin composition obtained in Example 1 and Comparative Example 1 was stencil printed on an LCP (LAPEROS (registered trademark) E463i) plate with a size of φ2 mm and a thickness of 125 μm. A 1.5 mm×3 mm×0.5 mm alumina chip was placed on the printed resin composition with the 1.5 mm×3 mm surface facing downward to prepare a test piece (n=10). The curing conditions at this time were to use a UV LED irradiation device AC475 manufactured by Excelitas Technologies from the opposite side (back side) of the alumina chip mounting surface (front side) with a cumulative light dose of 2000 mJ / cm 2 After curing (measured using UIT-250 (connected to UVD-365 light receiver) manufactured by USHIO Electric Co., Ltd.), it was heated at 80°C for 60 minutes in an air dryer. The alumina chip on the LCP board was pushed from the side using a MODEL-1605HTP strength tester manufactured by AIKOH ENGINEERING, and the shear strength was calculated based on the numerical value when the alumina chip was peeled off, and was set as shear strength A. On the other hand, the test piece prepared in the same manner was additionally heated at 120°C for 1 hour in an air dryer, and the shear strength was calculated using the same method, and was set as shear strength B. The change in the strength increase rate of the cured product caused by additional heating was calculated using the following formula. The results are shown in Table 2.
[0214] The strength increase rate of the cured product due to additional heating = shear strength B / shear strength A
[0215] As the rate of increase in strength due to additional heating increases, it is shown that unreacted components in the cured product are cured by additional heating, that is, more unreacted components remain in the cured product after thermal curing following UV curing.
[0216] [Table 2]
[0217]
[0218] [Measurement of shrinkage change due to additional heating]
[0219] The volume shrinkage of the resin composition obtained in Example 1 and Comparative Example 1 was measured by a specific gravity method. Specifically, the liquid specific gravity ρL was calculated using a specific gravity bottle with a liquid specific gravity of about 10 mL, and the specific gravity of the cured product was determined by measuring the weight in water and the weight in air to obtain the cured product specific gravity ρS. Using these values, the shrinkage was calculated using the following calculation formula (1).
[0220] Volume shrinkage (%) = (1 / pL-1 / ρS) / (1 / ρL)…(1)
[0221] The resin composition was irradiated with a UV LED irradiation device AC475 manufactured by Excelitas Technologies at a cumulative light intensity of 2000 mJ / cm 2 (Measured using UIT-250 (connected to UVD-365 light receiver) manufactured by USHIO Electric Co., Ltd.) UV curing was performed by UV irradiation, and the obtained product was placed in a blast dryer and heated at 80°C for 60 minutes. The specific gravity of the cured product at this time was set to ρS1. Thereafter, the test piece prepared in the same manner was additionally heated in a blast dryer at 120°C for 1 hour, and the specific gravity of the cured product at this time was set to ρS2. Using these values, the change in shrinkage due to additional heating was measured using the following calculation formula (2). The results are shown in Table 3.
[0222] Change in shrinkage due to additional heating (%) = (1 / ρL-1 / ρS2) / (1 / ρL)-(1 / ρL-1 / ρS1) / (1 / ρL)…(2)
[0223] [Table 3]
[0224] Example 1 Comparative Example 1 Changes in shrinkage due to additional heating 0.0% 0.2%
[0225] The cured product obtained in Example 1 had almost no change in shrinkage due to additional heating, while the cured product obtained in Comparative Example 1 had a 0.2% increase in shrinkage due to additional heating. From this result, it can be considered that the Example had a small change due to time, and problems such as positional deviation were less likely to occur.
[0226] [Measurement of gas release due to additional heating]
[0227] The resin compositions obtained in Example 1 and Comparative Example 1 were prepared by irradiating the resin compositions with a UV dose of 2000 mJ / cm 2The cured resin was cured by UV curing (UV wavelength: 365 nm, LED lamp). 10 mg of the cured resin was collected and measured using a differential thermogravimetric simultaneous measuring device (TG8120 manufactured by Rigaku Corporation) to measure the outgassing generated when heated at 80°C for 60 minutes under air conditions (outgassing generated by normal curing), and the outgassing generated from the initial heating at 80°C for 60 minutes until reaching 120°C when the temperature was increased from 80°C to 120°C at 10°C / min as additional heating (outgassing that may be generated due to additional heating).
[0228] When the outgassing amount was less than 100 ppm, the outgassing resistance was judged to be good and designated as “A”, and when the outgassing amount was 100 ppm or more, the outgassing resistance was judged to be poor and designated as “F”.
[0229] [Table 4]
[0230] Example 1 Comparative Example 1 Outgassing resistance A F
[0231] [Thermosetting of insufficient UV curing areas]
[0232] It has been found that when an adhesive containing a photo- and thermosetting resin composition is used in the assembly process of a semiconductor module (e.g., an image sensor module or a camera module), during UV irradiation curing, since UV irradiation is performed from the outside of the semiconductor module, it is difficult for the inside of the semiconductor module to be irradiated with UV light, and although a portion of the adhesive is UV-cured, there may be a UV-undercured region where UV curing is not completely performed. The unreacted components remaining in the UV-undercured region do not promote the curing reaction even during the subsequent thermal curing, and are particularly likely to remain as residual components.
[0233] In this evaluation test, the above-mentioned insufficient UV curing area of the adhesive was reproduced, and the thermosetting property in the insufficient UV curing area was evaluated. In order to reproduce the insufficient UV curing area, the UV irradiation amount was set low.
[0234] Comparative Example 3 is an example in which the component (D-2) in the resin composition of Example 13 was replaced with the component (D′-2).
[0235] The resin compositions of Example 13 and Comparative Example 3 were degassed in a vacuum and irradiated with UV at a dose of 40 mJ / cm 2After UV curing (UV wavelength: 365nm, LED lamp), heat curing was performed in a blast dryer at 60°C / 60 minutes and 80°C / 60 minutes to obtain a cured resin. 5 mg of the cured resin was collected and heated from 30°C to 250°C under nitrogen conditions at a heating rate of 10°C / minute using DSC to obtain an exothermic curve. In the case of a residual exothermic peak, the exothermic peak was integrated to calculate the residual heat storage. The results are shown in Table 5.
[0236] [Table 5]
[0237]
[0238] The cured product of the resin composition obtained in Example 13 has substantially no residual heat, whereas the cured product of the resin composition obtained in Comparative Example 3 has a large residual heat. From this result, it can be confirmed that the Examples containing component (D) exhibit high thermosetting properties even in the incompletely cured region of the UV-cured region that reproduces the region that is difficult to be irradiated with UV, and therefore have a small amount of unreacted components. It is believed that the small amount of unreacted components has the effect of suppressing the positional deviation and outgassing described above.
[0239] Industrial Applicability
[0240] The present invention is a resin composition that can suppress the remaining unreacted components in the cured product after the second-stage thermal curing following the first-stage UV curing and can be thermally cured at 60°C. The resin composition is particularly useful as an adhesive or sealing material for fixing, bonding or protecting components constituting image sensors or camera modules.
[0241] The entire contents of the disclosure of Japanese Patent Application No. 2022-030685 (filing date: March 1, 2022) are incorporated into this specification by reference.
[0242] All documents, patent applications, and technical standards described in this specification are incorporated herein by reference to the same extent as if each individual document, patent application, or technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A resin composition comprising: A (meth)acrylate compound, B. Multifunctional thiol compounds, C. a photoradical polymerization initiator, and D is a thermal curing accelerator comprising an azabicyclic compound having a bridgehead nitrogen.
2. The resin composition according to claim 1, wherein The ratio of the number of (meth)acryloyl groups equivalent of component A to the number of thiol groups equivalent of component B, that is, [the number of (meth)acryloyl groups equivalent of component A] / [the number of thiol groups equivalent of component B], is 0.25 to 3.
0.
3. The resin composition according to claim 1 or 2, wherein The B multifunctional thiol compound includes a thiol compound having three or more functional groups. 4 . The resin composition according to claim 1 , further comprising an E epoxy compound. 5 . An adhesive or a sealing material comprising the resin composition according to claim 1 . 6 . The adhesive or sealing material according to claim 5 , which is used for fixing, bonding or protecting components constituting an image sensor or a camera module. 7 . A cured product obtained by curing the resin composition according to claim 1 , or the adhesive or sealing material according to claim 5 . 8 . A semiconductor device or an electronic component comprising the cured product according to claim 7 . 9 . The semiconductor device or electronic component according to claim 8 , which is an image sensor or a camera module.
Citation Information
Patent Citations
Ultraviolet curable resin composition, cured product thereof, and various kinds of articles derived therefrom
JP2008184514A
Photo and heat curable composition, and cured product using the same
JP2009051954A
Photosensitive resin composition and application thereof
JP2010117545A
Resin composition, adhesive, cured product, and semiconductor device
JP2017171804A
Body wash implement and manufacturing method thereof
JP2022030685A