Water-soluble nanocomposite barrier film
By introducing an integrated water-dispersible nanocomposite barrier layer into the water-soluble membrane, the existing problems of insufficient barrier performance and slow dissolution speed of water-soluble membranes in chemicals and humid environments are solved, and the problem of water-soluble membranes in chemicals and humid environments is solved. Effective barrier and rapid dissolution effects in humid environments.
Patent Information
- Application Number
- CN202380015754.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-27
- Filing Date
- 2023-01-27
- Publication Date
- 2024-10-15
AI Technical Summary
Existing water-soluble membranes are difficult to effectively block the migration of chemical substances when exposed to chemicals or humid environments, resulting in product performance degradation, and their dissolution rate is too slow when immersed in water, making them unable to meet the need for rapid dispersion.
Using an integrated water-dispersible nanocomposite barrier layer, by forming a nanocomposite barrier layer between water-soluble polymer layers, combined with a specific process and material combination, a nanocomposite barrier layer can be prepared without affecting the solubility and mechanical properties of the film. case, a water-soluble film that improves barrier properties.
It achieves effective barrier properties when exposed to chemicals or moisture, ensuring that chemicals do not migrate and quickly dissolve or disperse when immersed in water, meeting product performance and application requirements.
Smart Images

Figure GDA0005033260970000221 
Figure GDA0005033260970000231 
Figure HDA0004915155010000011
Abstract
Description
Technical Field
[0001] The present invention relates to a water-soluble film that can be used in product applications such as pods and tablets, having an integrated water-dispersible nanocomposite barrier that prevents any permeation, providing several advantages over prior art water-soluble film implementations; and a method for preparing a water-soluble film having an integrated water-dispersible nanocomposite barrier that prevents any permeation. Background Art
[0002] The use of water-soluble films in consumer products such as liquid detergent pods and automatic dishwasher dry powder tablets is increasingly widely recognized. In order to be effective, such water-soluble films must maintain properties (strength, penetration barrier) when exposed to chemicals, and disperse or dissolve completely when immersed in water. The multi-compartment pods launched by P&G on the market enable the chemical composition in the top / bottom compartments to be separated via the water-soluble films laid flat in the middle of the pods. The water-soluble films must be thick enough to avoid chemical exchange between the top / bottom compartments or from external contaminants, and must be thin enough to be completely dissolved in water during use.
[0003] Consumers have discovered that pods often become sticky over time, even if they are not prematurely exposed to water or to high humidity. This is because some of the chemical components held within the pod migrate through the outer pod film over time, as today's soluble films offer little barrier to the liquid components held within the package. The barrier properties of today's soluble films also cause other problems, such as the migration of chemicals between separate chambers of multi-chamber packaging, making it difficult to separate reactive materials even if they were initially separated in different chambers. Over time, they will diffuse and react together prematurely prior to use, limiting the ultimate performance of the entire product. Some examples of chemicals present in products where it is desired to limit migration are: Water, Fragrances, Surfactants, Bleach, Hueing Dyes, Highly Migrating Na + Cation, Fe 2+ cation.
[0004] A common method of preparing water-soluble films is via solution casting. An example of a commercially available water-soluble film is M8630 from MonoSol LLC (Gary, Indiana, USA). Other examples of commercially available water-soluble films are commercial products from Aicello Using this current technology, it is only possible to prepare water-soluble films as a layer or monolayer. For those applications in which barrier functionality is desired, the prior art chooses to apply the barrier material on top of an already formed water-soluble film or to disperse the barrier material within a component of the water-soluble film. Examples of barrier materials dispersed within a component of a water-soluble film are given in patent application WO2007 / 027224. If the barrier material is applied on top of an already formed water-soluble film, the sealing ability of the water-soluble film on the coated surface is affected, or the barrier properties are negligible. If the barrier material is dispersed within a component of the water-soluble film, the solubility of the water-soluble film is affected, or the barrier properties are negligible. In both cases, the barrier properties must be balanced with other important film properties, thereby reducing the barrier properties.
[0005] Water-soluble films are also produced via melt extrusion. This process enables the production of water-soluble multilayer films, provided that the rheological properties and interfacial energies between the different layers do not differ substantially. For those applications where barrier functionality is desired, the prior art disperses the barrier material within the composition of the middle layer of the water-soluble film. Again, in this case, water solubility and barrier properties must be balanced together, thus reducing the barrier properties.
[0006] Therefore, there is still an unmet need for water-soluble films and packages made therefrom (such as pouches and sachets) that have improved barrier properties when exposed to vapor and also dissolve or disperse into particles of sufficiently small size quickly when immersed in or exposed to water (such as rinse water or wash water). Small enough and fast enough depends on the specific product application. For single unit dose products (SUD), the time required will be less than the wash cycle of a washing machine. For packaging for shower body or shampoo products, the time is less than the average shower time, and for packaging that may eventually be discarded, the time is less than a day. Dispersion should be to the extent that the material is compatible with the drainage system without compromising product performance. Therefore, one aspect of the present disclosure is to provide a water-soluble film that has improved barrier properties that prevent the diffusion of undesirable chemicals (even water vapor) before being fully immersed in water, and then can be substantially dissolved or dispersed when immersed in water (such as rinse water or wash water). Summary of the invention
[0007] Provided is a water-soluble film with an integrated water-dispersible nanocomposite barrier, the water-soluble film comprising: a first water-soluble polymer layer having a plane; a second water-soluble polymer layer having a plane; and a water-dispersible nanocomposite barrier layer disposed between the first water-soluble polymer layer and the second water-soluble polymer layer.
[0008] A method for making a water-soluble film with an integrated water-dispersible nanocomposite barrier is provided, the method comprising applying a first aqueous solution of a water-soluble polymer composition to the surface of a removable flat carrier (such as a PET film or a steel strip); removing water from the first aqueous solution of the water-soluble polymer composition to obtain a first water-soluble polymer layer; applying an aqueous dispersion of the water-dispersible nanocomposite barrier to the surface of the first water-soluble polymer layer; removing water from the aqueous dispersion of the water-dispersible nanocomposite barrier to obtain a water-dispersible nanocomposite barrier layer; applying a second aqueous solution of the water-soluble polymer composition to the surface of the water-dispersible nanocomposite barrier layer; removing water from the second aqueous solution of the water-soluble polymer composition to obtain a second water-soluble polymer layer; and removing the flat carrier from the resulting water-soluble nanocomposite barrier film. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 A cross section of a water-soluble polymer layer 10 is shown.
[0010] Figure 2 A cross-section of a water dispersible nanocomposite barrier layer 20 coated on a water soluble polymer layer 10 is shown.
[0011] Figure 3 A cross-section of a water-soluble film with an integrated water-dispersible nanocomposite barrier of the present disclosure is shown, the water-soluble film comprising a water-soluble polymer layer 30 coated on a water-dispersible nanocomposite barrier layer 20, which is coated on a water-soluble polymer layer 10.
[0012] Figure 4 A cross-sectional image obtained via scanning electron microscopy (SEM) of a water-soluble film with an integrated water-dispersible nanocomposite barrier of the present disclosure is shown.
[0013] Figure 5 A cross-sectional image obtained via transmission electron microscopy (TEM) of a water-dispersible nanocomposite barrier of the present disclosure is shown, showing nanoscale (<100 nm) ordered spacing of hydrophilic hectorite nanosheets (1 nm thick dark lines) and intercalated polyethylene glycol (PEG) fillers (0.8 nm thick light lines).
[0014] Figure 6 A schematic diagram of a method of making a water-soluble film with an integrated water-dispersible nanocomposite barrier of the present disclosure is shown.
[0015] Figure 7 Schematic diagram showing the application of the disclosed water-soluble film with an integrated water-dispersible nanocomposite barrier. DETAILED DESCRIPTION
[0016] The present invention describes a water-soluble film with an integrated water-dispersible nanocomposite barrier to water vapor permeation that provides several advantages over prior art water-soluble films; and a method for making a water-soluble film with an integrated water-dispersible nanocomposite barrier layer.
[0017] As used herein, the term "water dispersible" means breaking into small fragments less than one tenth of a millimeter in water. These fragments may, but need not, be stably suspended in water.
[0018] As used herein, the term "nanocomposite" refers to a heterogeneous material comprising nanoscale, orderly spaced hydrophilic nanosheets and intercalated polymer fillers; "nanoscale" means less than about 100 nanometers.
[0019] As used herein, the term "water vapor transmission rate" or "WVTR" refers to the rate at which water vapor is transmitted through a film when measured according to the Water Vapor Transmission Test Method set forth in the Test Methods section.
[0020] As used herein, the term "dissolution time" refers to the time required to dissolve a water-soluble film when measured according to the Dissolution Test Method set forth in the Test Methods section.
[0021] As used herein, the term "copolymer" refers to a polymer formed from two or more types of monomer repeating units. As used herein, the term "copolymer" also encompasses terpolymers, such as terpolymers having a distribution of vinyl alcohol monomer units, vinyl acetate monomer units, and possibly butene glycol monomer units; however, if the copolymer is substantially completely hydrolyzed, the vinyl acetate monomer units may be substantially absent.
[0022] As used herein, the term "degree of hydrolysis" refers to the mole percentage of vinyl acetate units that are converted to vinyl alcohol units when polymerized vinyl alcohol is hydrolyzed.
[0023] As used herein, when the term "about" modifies a particular value, the term refers to a range equal to the particular value plus or minus twenty percent (±20%). For any of the embodiments disclosed herein, in various alternative embodiments, any disclosure of a particular value may also be understood to be a disclosed range approximately equal to the particular value (i.e., ±20%).
[0024] As used herein, when the term "about" modifies a particular value, the term refers to a range equal to the particular value plus or minus fifteen percent (±15%). For any of the embodiments disclosed herein, in various alternative embodiments, any disclosure of a particular value may also be understood to be a disclosed range approximately equal to the particular value (i.e., ±15%).
[0025] As used herein, when the term "substantially" modifies a particular value, the term refers to a range equal to the particular value plus or minus ten percent (±10%). For any of the embodiments disclosed herein, in various alternative embodiments, any disclosure of a particular value may also be understood to be approximately equal to the disclosed range of the particular value (i.e., ±10%).
[0026] As used herein, when the term "almost" modifies a particular value, the term refers to a range equal to the particular value plus or minus five percent (±5%). For any of the embodiments disclosed herein, in various alternative embodiments, any disclosure of a particular value may also be understood as a disclosed range approximately equal to the particular value (i.e., ±5%).
[0027] Figure 1 A cross section of the water-soluble polymer layer 10 is shown. The water-soluble polymer layer 10 has a first surface 12 and a second surface 14 opposite the first surface 12, and a thickness 16 between the first surface 12 and the second surface 14.
[0028] The thickness of the water-soluble polymer layer 10 between the first surface 12 and the second surface 14 may range from about 1 μm to about 1000 μm, preferably from about 10 μm to about 250 μm, more preferably from about 25 μm to about 125 μm.
[0029] The water-soluble polymer layer 10 comprises at least one water-soluble polymer. Depending on the application, the water-soluble polymer can be selected from the available options to dissolve in water at a temperature of 23° C. in seconds, minutes, or hours. A polymer that takes more than 24 hours to dissolve in water at a temperature of 23° C. will not be considered water-soluble.
[0030] Figure 2 A cross-section of a water-dispersible nanocomposite barrier layer 20 is shown, the water-dispersible nanocomposite barrier layer having a first surface 22 and a second surface 24 opposite the first surface 22, and a thickness 18 between the first surface 22 and the second surface 24, the water-dispersible nanocomposite barrier layer being applied to substantially cover at least one of the first surface 12 or the second surface 14 of the water-soluble polymer layer 10.
[0031] The thickness of the water-dispersible nanocomposite barrier layer 20 is in the range of about 0.1 μm to about 20 μm, preferably about 0.1 μm to about 10 μm, and more preferably about 0.1 μm to about 5 μm.
[0032] The water-dispersible nanocomposite barrier layer 20 is a nanocomposite comprising nanoscale ordered spaced hydrophilic nanosheets and intercalated polymer fillers, wherein the basal spacing measured by X-ray diffraction (XRD) is less than Preferably less than More preferably, less than
[0033] Figure 5 A cross-sectional image obtained via transmission electron microscopy (TEM) of one embodiment of a water-dispersible nanocomposite barrier layer of the present disclosure is shown, wherein the basal plane spacing measured via XRD is equal to Showing the ordered spacing of hydrophilic hectorite nanosheets ( Thick dark lines) and intercalated polyethylene glycol (PEG) fillers ( Thick bright lines), which repeat regularly at the nanoscale.
[0034] Nanosheets are flaky nanoparticles characterized by a high aspect ratio between diameter and orthogonal height. The high aspect ratio enables the formation of a "brick wall" in which the nanosheets are laid parallel to the surface of the underlying water-soluble polymer layer, overlapping each other and placed on top of each other, thus significantly reducing the migration of molecules (whether gaseous or liquid) through the nanosheet layer. The higher the aspect ratio, the higher the barrier properties that can be obtained. The typical aspect ratio of montmorillonite exfoliated nanosheets is about 100 or greater (Cadène et al., JCIS 285 (2): 719-30, June 2005).
[0035] The water-dispersible nanocomposite barrier layer 20 of the present disclosure may be optically opaque, preferably translucent, and even more preferably transparent, depending on the nanocomposite (nanosheet exfoliation level, polymer intercalation between nanosheets, impurity levels) and the nanocomposite application process (nanocomposite orientation).
[0036] Preferably, the water-dispersible nanocomposite barrier layer 20 is flexible and stretchable. When the water-soluble film of the present disclosure is converted through a production line for printing, sheeting, cutting, rewinding and other typical converting operations to make an article such as a pouch, the water-soluble film of the present disclosure can be stretched up to 200%. This can cause the water-dispersible nanocomposite barrier layer 20 to break. Therefore, it is preferred that the water-dispersible nanocomposite barrier layer 20 is flexible and stretchable without breaking. Preferably, the water-dispersible nanocomposite barrier layer 20 can be stretched at least 20%, more preferably at least 30%, even more preferably at least 50%, most preferably at least 100% and up to 200% without breaking.
[0037] Figure 3A cross section of a water-soluble film 100 with an integrated water-dispersible nanocomposite barrier is shown that includes a first water-soluble polymer layer 10. The water-soluble polymer layer 10 has a first surface 12 and a second surface 14 opposite the first surface 12, and a thickness 16 between the first surface 12 and the second surface 14. The water-soluble polymer layer 10 can be in the form of a film or a sheet. A water-dispersible nanocomposite barrier layer 20 having a first surface 22 and a second surface 24 opposite the first surface 22 and a thickness 18 between the first surface 22 and the second surface 24 is applied to and substantially covers at least one of the first surface 12 or the second surface 14 of the water-soluble polymer layer 10. A second water-soluble polymer layer 30 having a first surface 112 and a second surface 114 opposite the first surface 112 and a thickness 116 between the first surface 112 and the second surface 114 is applied such that the second surface of the water-soluble polymer layer substantially covers at least one of the first surface 22 or the second surface 24 of the water-dispersible nanocomposite barrier layer 20. The water soluble polymer layer 30 may be in the form of a film or a sheet. Adhesion between the layers is provided by molecular interactions between the water soluble polymer layer and the water dispersible nanocomposite barrier layer.
[0038] The thickness of the water-soluble polymer layer 30 between the first surface 112 and the second surface 114 may be in a range of about 1 μm to about 1000 μm, preferably about 10 μm to about 250 μm, more preferably about 25 μm to about 125 μm.
[0039] The water-soluble polymer layer 30 includes at least one water-soluble polymer. Depending on the application, the water-soluble polymer can be selected from the available options to dissolve in water at a temperature of 23° C. in seconds, minutes, or hours. A polymer that takes more than 24 hours to dissolve in water at a temperature of 23° C. will not be considered water-soluble.
[0040] Each layer of the present disclosure is distinct and separate from one another. By distinct layers, it is meant that the water-dispersible nanocomposite barrier layer 20 within the water-soluble film 100 comprises substantially only nanocomposite barrier material, and that the boundaries between the water-dispersible nanocomposite barrier layer 20 and the surrounding water-soluble polymer layers 10 and 30 are distinguished by large composition changes over a small distance, thereby creating a sharp boundary that is easily seen by microscopy techniques known in the art. The boundary layer, i.e., the intermediate layer of intermediate composition between the water-dispersible nanocomposite barrier layer and the adjacent water-soluble polymer layer, is no more than 2 μm thick, as seen by microscopy techniques known in the art.
[0041] When the water-soluble film of the present disclosure is immersed in water (i.e., in applications where the water-soluble film needs to disappear in water), the outer polymer layer dissolves in water, the inner barrier layer is no longer protected and breaks down in water, and the nanocomposite barrier material is dispersed in water, thus enabling the entire film to disappear in water.
[0042] The water-soluble films of the present disclosure including the water-dispersible nanocomposite barrier layer may be opaque, preferably translucent, and even more preferably transparent, depending on the material.
[0043] The water-soluble films of the present disclosure may include a printed area. Printing may be achieved using standard printing techniques such as flexographic printing, gravure printing, or inkjet printing.
[0044] Water dispersible nanocomposites
[0045] The nanocomposite material comprises nanoscale ordered hydrophilic nanosheets and intercalated polymer fillers, wherein the basal spacing measured by XRD is less than Preferably less than More preferably, less than
[0046] Nanosheets are solid flaky nanoparticles characterized by a high aspect ratio between diameter and orthogonal height. The high aspect ratio provides parallel arrangement of nanosheets and a longer diffusion path length for chemicals through the nanosheets, thus providing a barrier function. It is desirable that the nanosheets have no defects such as cracks and holes that reduce barrier properties. It is also desirable that the nanosheets are easily peeled off in water for both application purposes (e.g., wet coating) and end-of-life situations (e.g., wastewater treatment plants), but have high viscosity when dried. Nanosheets are currently used in industry as rheology modifiers, flame retardants, anti-corrosion coatings, and / or chemical barriers. Nanosheets can be obtained from natural sources and used as is, or can be purified and modified from natural sources, or can be synthesized in a furnace for purity and performance reasons.
[0047] Natural phyllosilicates (such as serpentine, clay, chlorite and mica) consist of nanosheets stacked together. Natural clays (such as montmorillonite and vermiculite) consist of nanosheets stacked together and swell in the presence of water. Smectites (such as montmorillonite and hectorite) consist of nanosheets stacked together and swell most easily in the presence of water. Natural montmorillonite can be purified and modified, such as sodium crosette from BYK, which is made of bentonite (a natural mineral containing 60% to 80% montmorillonite) and cation exchanged with monovalent sodium for stripping purposes. Smectites can also be synthesized, such as synthetic hectorite manufactured by BYK and sodium hectorite synthesized at the University of Bayreuth.
[0048] Water soluble polymer
[0049] The water-soluble polymer, copolymer or derivative thereof suitable for use as the water-soluble polymer layer is selected from polyvinyl alcohol (PVOH), copolymers of polyvinyl alcohol (such as butene glycol-vinyl alcohol copolymer (BVOH)), which are produced by copolymerization of butene glycol with vinyl acetate, followed by hydrolysis of vinyl acetate, suitable butene glycol monomers are selected from 3,4-diol-1-butene, 3,4-diacyloxy-1-butene, 3-acyloxy-4-ol-1-butene, 4-acyloxy-3-ol-1-butene, etc.; polyvinyl pyrrolidone; polyalkylene oxides such as polyethylene oxide or polyethylene glycol (PEG); poly(methyl methacrylate) Acrylic acid), polyacrylic acid, polyacrylates, acrylate copolymers, maleic acid / acrylic acid copolymers; polyacrylamide; poly(2-acrylamido-2-methyl-1-propane sulfonic acid (polyAMPS); polyamides, poly-N-vinylacetamide (PNVA); polycarboxylic acids and salts; cellulose derivatives such as cellulose ethers, methylcellulose, hydroxyethylcellulose, carboxymethylcellulose; hydroxypropyl methylcellulose; natural gums such as xanthan gum and carrageenan; sodium alginate; maltodextrin, low molecular weight dextrin; polyamino acids or peptides; proteins such as casein and / or caseinates (e.g., as commercialized by Lactips).
[0050] Preferred water-soluble polymers are polyvinyl alcohol, polyethylene oxide, methylcellulose and sodium alginate. For applications requiring a "plastic-free" product, the majority of the components of the water-soluble polymer layer may be naturally derived polymers, such as sodium alginate. Preferably, the content of polymer in the water-soluble polymer layer is at least 60%.
[0051] The average molecular weight of the water-soluble polymer (measured by gel permeation chromatography) is about 1,000Da to about 1,000,000Da, or any integer value from about 1,000Da to about 1,000,000Da, or any range formed by any of the foregoing values, such as about 10,000Da to about 300,000Da, about 20,000Da to about 150,000Da, etc. More specifically, the molecular weight of polyvinyl alcohol will have a molecular weight in the range of 20,000Da to 150,000Da. The molecular weight of polyethylene oxide will be in the range of 50,000Da to 400,000Da. The molecular weight of methylcellulose will be in the range of 10,000Da to 100,000Da. Methylcellulose can be methoxy-substituted, for example, from about 18% to about 32%, and can be hydroxy-propoxy-substituted, for example, from about 4% to about 12%. The molecular weight of sodium alginate will range from 10,000 Da to 240,000 Da.
[0052] If a homopolymer polyvinyl alcohol is used, the degree of hydrolysis can be from 70% to 100%, or any integer percentage value between 70% and 100%, or any range formed by any of these values, such as 80% to 100%, 85% to 100%, 90% to 100%, 95% to 100%, 98% to 100%, 99% to 100%, 85% to 99%, 90% to 99%, 95% to 99%, 98% to 99%, 80% to 98%, 85% to 98%, 90% to 98%, 95% to 98%, 80% to 95%, 85% to 95%, 90% to 95%, etc.
[0053] Optional Ingredients
[0054] The water-soluble polymer layer of the water-soluble film with an integrated water-dispersible nanocomposite barrier may include disintegrants, plasticizers, surfactants, lubricants / release agents, fillers, extenders, anti-blocking agents, anti-adhesive agents, defoamers or other functional ingredients. In the case of articles comprising compositions for washing, the water-soluble polymer layer may include functional detergent additives to be delivered to the wash water, such as organic polymer dispersants or other detergent additives.
[0055] For some applications, it may be desirable for the water-soluble polymer layer to include a disintegrant to increase the dissolution rate of the water-soluble film with an integrated water-dispersible nanocomposite barrier in water. Suitable disintegrants are, but are not limited to, corn / potato starch, methylcellulose, mineral clay powders, cross-linked carboxymethyl cellulose (cross-linked cellulose), crospovidone (cross-linked polyvinyl N-pyrrolidone or PVP), sodium starch glycolate (cross-linked starch). Preferably, the water-soluble polymer layer includes between 0.1% and 15% by weight, more preferably about 1% to about 15% by weight of a disintegrant.
[0056] Preferably, the water-soluble polymer layer may include a water-soluble plasticizer. Preferably, the water-soluble plasticizer is selected from water, polyols, sugar alcohols and mixtures thereof. Suitable polyols include polyols selected from the group consisting of glycerol, diglycerol, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycols of up to 400Da molecular weight, neopentyl glycol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol, polypropylene glycol, 2-methyl-1,3-propanediol, methylene glycol, trimethylolpropane, hexylene glycol, neopentyl glycol and polyether polyols, or mixtures thereof. Suitable sugar alcohols include sugar alcohols selected from the group consisting of isomalt, maltitol, sorbitol, xylitol, erythritol, ribitol, galactitol, pentaerythritol and mannitol, or mixtures thereof. In some cases, the plasticizer may be selected from the following list: ethanolamine, alkyl citrate, isosorbide, pentaerythritol, glucosamine, N-methylglucosamine or sodium cumene sulfonate. Less mobile plasticizers such as sorbitol or polyethylene oxide may promote the formation of a water-soluble polymer layer with greater barrier properties than a water-soluble polymer layer including a more mobile plasticizer such as glycerol. In some cases, when it is desired to use as much naturally derived materials as possible, the following plasticizers may also be used: vegetable oils, polysorbate, polydimethylsiloxane, mineral oil, paraffin, C1-C3 alcohols, dimethyl sulfoxide, N,N-dimethylacetamide, sucrose, corn syrup, fructose, dioctyl sodium sulfosuccinate, triethyl citrate, tributyl citrate, 1,2-propylene glycol, monoacetate, diacetate or triacetate of glycerol, natural gums, citrates and mixtures thereof. More preferably, the water-soluble plasticizer is selected from glycerol, 1,2-propylene glycol, 20 dipropylene glycol, 2-methyl-1,3-propanediol, trimethylolpropane, triethylene glycol, polyethylene glycol, sorbitol, or mixtures thereof, most preferably selected from glycerol, sorbitol, trimethylolpropane, dipropylene glycol, and mixtures thereof. Preferably, the water-soluble polymer layer comprises between 5 wt % and 50 wt %, preferably between 10 wt % and 40 wt %, even more preferably about 12 wt % to about 30 wt % of plasticizer.
[0057] Preferably, the water-soluble polymer layer of the present disclosure includes a surfactant. Suitable surfactants may belong to nonionic, cationic, anionic or zwitterionic categories. Suitable surfactants include, but are not limited to, poloxamer (polyoxyethylene polyoxypropylene glycol), alcohol ethoxylates, alkylphenol ethoxylates, tertiary acetylenic glycols and alkanolamides (nonionic), polyoxyethylene amines, quaternary ammonium salts and polyoxyethylene quaternary amines (cationic), and amine oxides, N-alkyl betaines and sulfobetaines (zwitterionic). Other suitable surfactants include sodium sulfosuccinate, acylated fatty acid esters of glycerol and propylene glycol, fatty acid lactyl fat, sodium alkyl sulfate, polysorbate 20, polysorbate 60, polysorbate 65, polysorbate 80, lecithin, glycerol and propylene glycol, and acetylated esters of 5 kinds of fatty acids, and combinations thereof. Preferably, the water-soluble polymer layer includes a surfactant between 0.1% by weight and 2.5% by weight, more preferably about 1% by weight to about 2% by weight.
[0058] Preferably, the water-soluble polymer layer of the present disclosure comprises a lubricant / stripping agent. Suitable lubricants / stripping agents are, but are not limited to, fatty acids and their salts, fatty alcohols, fatty acid esters, fatty amines, fatty amine acetates, and fatty amides. Preferred lubricants / stripping agents are fatty acids, fatty acid salts, fatty amine acetates, and mixtures thereof. Preferably, the water-soluble polymer layer comprises 0.02 wt % to 1.5 wt %, preferably about 0.1 wt % to about 1 wt % of the lubricant / stripping agent.
[0059] Preferably, the water-soluble polymer layer of the present disclosure comprises filler, extender, anti-adhesive agent, release agent. Suitable filler, extender, anti-adhesive agent, release agent are but not limited to starch, modified starch, cross-linked polyvinyl pyrrolidone, cross-linked cellulose, microcrystalline cellulose, silicon dioxide, metal oxide, calcium carbonate, talc and mica. Preferably, the water-soluble polymer layer is included in the filler, extender, anti-adhesive agent, release agent between 0.1 % by weight and 25 % by weight, more preferably about 1 % by weight to about 15 % by weight. In the absence of starch, the water-soluble polymer layer comprises preferably filler, extender, anti-adhesive agent between 1 % by weight and 5 % by weight.
[0060] Preferably, the water-soluble polymer layer of the present disclosure comprises a defoamer. Suitable defoamers are, but are not limited to, polydimethylsiloxane and hydrocarbon blends. Preferably, the water-soluble polymer layer comprises between 0.001 wt % and 0.5 wt %, more preferably between about 0.01 wt % and about 0.5 wt % of the defoamer.
[0061] The benefit agent may also be incorporated into the water-soluble polymer layer. Thus, it is possible to deliver a benefit agent that is incompatible with the product or composition inside the article via the article, such as a pouch. Examples of benefit agents are, but are not limited to, detergents, soil suspending agents, anti-redeposition agents, fluorescent whitening agents, bleaching agents, enzymes, perfume compositions, bleach activators and precursors, brighteners, foam suppressants, fabric care compositions, surface nourishing compositions.
[0062] Bittering agents may also be incorporated into the water-soluble polymer layer, which is a legal requirement in some areas for certain applications (such as pods). Suitable bittering agents are, but are not limited to, naringin, sucrose octaacetate, quinine hydrochloride, denatonium benzyl, or mixtures thereof. Preferably, the water-soluble polymer layer comprises between 1 ppm and 5000 ppm by weight, more preferably about 100 ppm to about 2500 ppm, even more preferably about 250 ppm to about 2000 ppm of the bittering agent.
[0063] The water-soluble film or water-soluble article of the present disclosure may be coated with an anti-blocking agent. Suitable anti-blocking agents are, but are not limited to, talc, zinc oxide, silicon dioxide, siloxane, zeolite, silicic acid, aluminum oxide, sodium sulfate, potassium sulfate, calcium carbonate, magnesium carbonate, sodium citrate, sodium tripolyphosphate, potassium citrate, potassium tripolyphosphate, calcium stearate, zinc stearate, magnesium stearate, starch, modified starch, clay, kaolin, gypsum, cyclodextrin, or mixtures thereof.
[0064] Method for making water-soluble nanocomposite barrier film
[0065] There are many non-limiting embodiments for making the water-soluble films with integrated water-dispersible nanocomposite barriers described herein. Figure 6 As shown, water-soluble films with an integrated water-dispersible nanocomposite barrier can be prepared by multiple steps of coating and drying of aqueous polymer solutions or aqueous nanocomposite dispersions under specific conditions.
[0066] In one non-limiting embodiment of the method, a water-soluble polymer layer 10 is formed on the surface of a flat support (e.g., an untreated PET film, a stainless steel tape, a fluorinated polymer tape, or any other suitable support material); a water-dispersible nanocomposite barrier layer 20 is formed on at least one of the surfaces 12, 14 of the previously formed water-soluble polymer layer 10; then, a second water-soluble polymer layer 30 is formed on at least one of the surfaces 112, 114 of the previously formed water-dispersible nanocomposite barrier layer; and finally, the flat support is removed from the resulting water-soluble nanocomposite barrier film.
[0067] In order to make the water-soluble polymer layer 10 or 30, an aqueous polymer solution is usually formed as follows: a water-soluble polymer in solid form is taken and first dissolved in water using moderate stirring, typically 20% by weight of the water-soluble polymer corresponds to 80% by weight of water. The aqueous polymer solution is then further combined with other additives such as plasticizers at high temperatures by moderate stirring. The aqueous polymer solution is then coated onto a flat surface carrier (e.g., untreated PET film, stainless steel belt, fluorinated polymer belt or any other suitable material), and water is removed via IR, convection or diffusion drying processes.
[0068] Without being limited by theory, it is believed that the most important material properties of the aqueous polymer solution are: a) the solids content at a given temperature between 20°C and 95°C; b) the resulting viscosity of the aqueous polymer solution at that temperature, with higher viscosities being better for maximum distinction / separation between layers; c) the wetting of the aqueous polymer solution on a flat support, or on a layer of water-dispersible nanosheets, or on another layer of water-soluble polymer, with higher wetting being better.
[0069] To make the water-dispersible nanocomposite barrier layer 20, an aqueous nanocomposite dispersion is typically formed by taking water-dispersible nanosheets in solid form and exfoliating them first in water. The aqueous nanosheet dispersion is then further mixed with an aqueous polymer solution under moderate stirring. The resulting aqueous nanocomposite dispersion will typically contain 1% to 10% solids, depending on the coating method selected for the application. The aqueous nanocomposite dispersion is then coated onto a given substrate, and the water is then removed via drying.
[0070] Without being limited by theory, it is believed that the most important material properties of the nanocomposite are: a) the aspect ratio of the nanosheets (higher aspect ratio is better for barrier performance); b) the overall exfoliation and dispersion of the nanosheets in water to maximize barrier properties; c) the choice of polymer filler and the weight ratio between nanosheets and polymer filler to minimize the basal spacing between nanosheets without phase separation, thereby maximizing barrier properties.
[0071] Without being limited by theory, it is also believed that the most important processability properties of the aqueous nanocomposite dispersion are: a) the viscosity of the aqueous nanocomposite dispersion, with higher viscosity favoring maximum differentiation / separation between the layers and, therefore, maximum barrier properties; b) the wetting of the aqueous nanocomposite dispersion on the water-soluble polymer layer or on another water-dispersible nanocomposite barrier layer; c) the shear applied to the aqueous nanocomposite dispersion, with higher shear favoring parallel nanosheet orientation with respect to the barrier plane; and d) the removal of water from the dispersion via diffusion drying without creating defects (such as pinholes or cracks) in the nanocomposite barrier layer.
[0072] Many processes for coating aqueous nanocomposite dispersions were tested: wire rod coating, anilox roll coating, reverse roll coating, slot die extrusion coating, roll-to-roll coating, and spray coating. Aqueous extrusion coating via a customized slot die (e.g., FMP Technology, Coatema) proved to be the most reliable process for providing the correct transverse feed of aqueous nanocomposite dispersions. Coating processes that provide excellent shear of the aqueous nanocomposite dispersions are preferred because the excellent shear provides excellent parallel orientation of the nanosheets within the nanocomposite barrier layer, resulting in excellent barrier properties. However, the barrier properties also depend on the total thickness of the water-dispersible nanocomposite barrier layer. Typically, the thickness of the water-dispersible nanocomposite barrier layer is in the range of 0.1 μm to 10 μm to provide sufficient barrier properties while maintaining sufficient mechanical flexibility and mechanical resistance.
[0073] In another non-limiting embodiment of the method, the water-dispersible nanocomposite barrier layer 20 is obtained by multiple application steps of coating and drying an aqueous nanocomposite dispersion, each nanocomposite sublayer masks the assumed defects in the underlying nanocomposite sublayer, thereby providing maximum barrier properties. To this end, a first water-dispersible nanocomposite barrier sublayer is formed on the water-soluble polymer layer 10 according to any of the above methods; subsequently, one or more additional water-dispersible nanocomposite barrier sublayers can be added until the desired water-dispersible nanocomposite barrier layer thickness is obtained. According to this method, a relatively thick water-dispersible nanocomposite barrier layer can be formed. In the case of increasing optical transparency and mechanical flexibility, additional water-dispersible nanocomposite barrier sublayers can be separated by additional thinner water-soluble polymer sublayers. Various polymer sublayers or barrier sublayers can have substantially the same chemical composition or different chemical compositions to provide different properties to the overall structure. Adhesion between sublayers is provided by molecular interactions between water-soluble polymer sublayers and water-dispersible nanocomposite barrier sublayers. Similarly, cohesion between water-dispersible nanocomposite barrier sublayers is provided solely by molecular interactions between the nanocomposite barrier materials.
[0074] The drying step is usually performed by a conveyor dryer, such as Those sold under the trade name Drytec, those sold by Coatema under the trade name ModulDry and / or those sold by FMP Technologies GmbH (Erlangen, Germany) under the trade name SenDry or PureDry. In some embodiments, the drying substrate is guided through a hot air tunnel by a running belt (belt dryer), by a plurality of idler wheels (roller dryer) or by a plurality of hot air nozzles (contactless hot air dryer). Without being limited by theory, it is believed that the most important parameters of the drying process are: a) the residence time of the drying substrate in the hot air channel, which is typically about 50 s for a 60 μ thick aqueous polymer solution containing 25% solids; b) the temperature profile of the hot air in the tunnel, which is typically up to about 95° C.; c) the flow velocity of the hot air over the substrate, which is typically about 25 m / s. The heating system can be electric, hot oil, steam or gas.
[0075] The water-soluble film of the present disclosure may contain residual moisture, which depends on the hygroscopicity of the water-soluble film components and the isotherm of the water-soluble film measured by Karl Fischer titration under given temperature and humidity conditions. For example, a water-soluble polyvinyl alcohol film may contain about 4% to 8% residual moisture at 23°C and 50% relative humidity.
[0076] Method for making water-soluble product
[0077] The water-soluble film with integrated water-dispersible nanocomposite barrier described herein can be formed into articles, including but not limited to those in which the water-soluble film with integrated water-dispersible nanocomposite barrier is used as packaging material. Such articles include but are not limited to water-soluble pouches, sachets and other containers. Water-soluble pouches and other such containers in combination with the water-soluble film with integrated water-dispersible nanocomposite barrier described herein can be made in any suitable manner known in the art. The water-soluble film with integrated water-dispersible nanocomposite barrier can be provided before or after it is formed into the final article. In either case, in certain embodiments, when making such articles, it is desirable that the surface of the water-soluble polymer layer on which the barrier layer is applied forms the outer surface of the article.
[0078] There are many processes for making water-soluble products. These include but are not limited to processes known in the art, such as: vertical forming filling and sealing process, horizontal forming filling and sealing process and forming a small bag in a mold on a circular drum surface. In the vertical forming filling and sealing process, a vertical tube is formed by folding the substrate. The bottom end of the tube is sealed to form an open small bag. The small bag is partially filled, thereby allowing the top space. The top parts of the open small bag are then sealed together to close the small bag, and the next open small bag is formed. The first small bag is then cut, and the process is repeated. The small bag formed in this way usually has a pillow shape. The horizontal forming filling and sealing process uses a die head with a series of molds. In the horizontal forming filling and sealing process, the substrate is placed in the die head and an open small bag is formed in these molds, which can then be filled, covered with another layer of substrate and sealed. In the third process (forming a small bag in a mold on a circular drum surface), the substrate is circulated on the drum and formed into bags, which are passed under the filling machine to fill the open bag. Filling and sealing occur at the highest point (top) of the circle depicted by the drum, for example, usually, filling is completed just before the drum starts to move in a downward circular motion, and sealing is completed just after the drum starts its downward motion. In any process related to the step of forming an open pouch, the substrate can be initially molded or formed into the shape of an open pouch using thermoforming, vacuum forming or both. Thermoforming involves heating the mold and / or substrate by applying heat in any known manner, such as contacting the mold with a heating element, or heating the mold and / or substrate by blowing hot air or using a heating lamp. In the case of vacuum forming, vacuum assistance is used to help drive the substrate into the mold. In other embodiments, these two technologies can be combined to form a pouch, for example, the substrate can be formed into an open pouch by vacuum forming, and heat can be provided to promote the process. Then, the open pouch is filled with a composition to be included therein. Then, the filled open pouch is closed, which can be accomplished by any method. In some cases, such as in a horizontal pouch forming process, closure is accomplished by continuously feeding a second material or substrate, such as a water-soluble substrate, over and onto the web of the open pouch and then sealing the first and second substrates together. The second material or substrate may include a water-soluble polymer layer 10 as described herein. It may be desirable to orient the surface of the second substrate onto which the barrier layer is applied so that it forms the outer surface of the pouch.
[0079] In this process, the first substrate and the second substrate are typically sealed in the area between the molds, and thus sealed between the pouches formed in adjacent molds. Sealing can be accomplished by any method. Sealing methods include heat sealing, solvent welding, and solvent sealing or wet sealing. The sealed web of the pouch can then be cut by a cutting device that cuts the pouches in the web into individual pouches from each other. The process of forming the water-soluble pouch is further described in U.S. Patent Application Serial No. 09 / 994,533, Publication No. US2002 / 0169092 A1, published in the name of Catlin et al.
[0080] The sealing mechanism may be a heat seal, a water seal, a moisture seal, an ultrasonic seal, an infrared seal, or any other type of seal deemed suitable.
[0081] Products
[0082] like Figure 7 As shown, the present disclosure also includes an article, which includes a product composition 400 and a water-soluble film 100 with an integrated water-dispersible nanocomposite barrier, which can be formed into a container 300, such as a pouch, a sachet, a capsule, a bag, etc., to hold the product composition. The surface of the water-soluble polymer layer opposite to the surface on which the water-dispersible nanocomposite barrier layer is applied can be used to form the outer surface of the container 300. The water-soluble film 100 with an integrated water-dispersible nanocomposite barrier can form at least a portion of the container 300 that provides a unit dose of the product composition 400. For simplicity, the article of interest herein will be described in the form of a water-soluble pouch, but it should be understood that the discussion herein is also applicable to other types of containers.
[0083] The pouch 300 formed by the aforementioned method may have any form and shape suitable for containing the composition 400 contained therein until it is desired to release the composition 400 from the water-soluble pouch 300, such as by immersing the water-soluble pouch 300 in water. The pouch 300 may include one compartment, or two or more compartments (i.e., the pouch may be a multi-compartment pouch). In one embodiment, the water-soluble pouch 300 may have two or more compartments that are in a substantially stacked relationship, and the pouch 300 includes substantially opposite upper and lower outer walls, skirt-like side walls forming the sides of the pouch 300, and one or more inner partition walls separating different compartments from each other. If the composition 400 contained in the pouch 300 includes different forms or components, the different components of the composition 400 may be contained in different compartments of the water-soluble pouch 300 and may be separated from each other by a barrier of a water-soluble material.
[0084] The pouch or other container 300 may contain a unit dose of one or more compositions 400 for use as / in a laundry detergent composition, an automatic dishwashing detergent composition, a hard surface cleaner, a stain remover, a fabric enhancer and / or a fabric softener, a hair care composition, a beauty care composition, an oral care composition, a health care composition, a personal cleansing composition, and a household cleaning composition; for example, a shampoo, a conditioner, a mousse, a facial soap, a hand soap, a shower soap, a liquid soap, a bar soap, a moisturizer, a skin lotion, a shaving lotion, a toothpaste, a mouthwash, a hair spray, a hand soap, a laundry detergent composition, a dishwashing detergent, an automatic dishwasher detergent composition, a cosmetic and Over-the-counter medications, razors, absorbent articles, wipes, hair sprays, foods and beverages, animal food products, menstrual cups, exfoliating pads, electrical and electronic consumer devices, brushes, applicators, earplugs, eye masks, eye patches, face masks, agricultural products, plant foods, plant seeds, insecticides, ant killers, alcoholic beverages, animal food products, electronics, medications, confectionery, pet foods, pet health products, CBD-based products, other products derived from drugs other than cannabis, vitamins, non-pharmaceutical natural / herbal "wellness" products, foods and beverages and new product formats where contact with small amounts of water would produce premature pouch dissolution, undesirable pouch leakage and / or undesirable inter-pouch sticking. Typical absorbent articles of the present disclosure include, but are not limited to, diapers, adult incontinence briefs, training pants, diaper holders, menstrual pads, incontinence pads, liners, absorbent inserts, sanitary pads, tampons, menstrual pants, sponges, tissues, paper towels, wipes, flannels, etc. Pouch sticking from migrating chemical components within the formulated product will also be reduced. The composition 400 in the pouch 300 can be in any suitable form, including but not limited to: liquid, gel, paste, cream, solid, granule, powder, capsule, pill, dragee, solid foam, fiber, etc. The different compartments of the multi-compartment pouch 300 can be used to separate incompatible ingredients. For example, it may be desirable to separate bleach and enzyme into separate compartments. Due to the possible improvement of barrier properties, dyes and spices commonly used in some fabrics and household care products should have higher stability in these new pouches. Other forms of multi-compartment embodiments may include liquid-containing compartments combined with powder-containing compartments. Other examples of multi-compartment water-soluble pouches are disclosed in Smith et al., U.S. Patent 6,670,314B2.
[0085] The water-soluble pouch 300 can be dropped into any suitable aqueous solution (such as hot or cold water), and then the water-soluble film 100 with an integrated water-dispersible nanocomposite barrier that forms the water-soluble pouch 300 dissolves to release the contents of the pouch. The water-soluble film 100 with an integrated water-dispersible nanocomposite barrier described herein can also be used for coated products and other articles. Non-limiting examples of such products are laundry detergent tablets or automatic dishwashing detergent tablets. Other examples include coated products in the food and beverage category, where contact with a small amount of water can produce premature dissolution, undesirable leakage and / or undesirable stickiness.
[0086] Additional product forms (articles) include disposable aprons, laundry bags, disposable hospital bedding, skin patches, face masks, disposable gloves, disposable hospital gowns, medical devices, skin wraps, agricultural mulch, shopping bags, sandwich bags, trash bags, emergency blankets and clothing, building / construction wraps and moisture-proof liners, primary packaging for shipping (such as envelopes and mailing promotional materials), non-absorbent clothing articles that can be used to wrap clothing items (e.g., dresses, shirts, suits, and shoes).
[0087] Test Method
[0088] When testing and / or measuring materials, if the relevant test method does not specify a specific temperature, the specimens are tested and / or measured at a temperature of 23°C (±3°C), wherein such specimens are pre-conditioned to such temperature. When testing and / or measuring materials, if the relevant test method does not specify a specific humidity, the specimens are tested and / or measured at a humidity of 35% (±5%), wherein such specimens are pre-conditioned to such humidity. The tests and / or measurements should be performed by trained, skilled and experienced personnel in accordance with good laboratory practice via properly calibrated equipment and / or instruments.
[0089] 1) Dispersion / dissolution of membrane in water
[0090] When tested according to the slide dissolution test, the test method measures the total time for a specific film sample to be completely dissolved, and the slide dissolution test is a test method 205 (MSTM 205) as described in paragraphs 116-131 of the U.S. published patent application US20150093526A1 entitled "Water-soluble film having improved dissolution and stress properties, and packets made therefrom". The entire disclosure is hereby incorporated by reference herein. The dissolution test method used herein is the same as the method described in US20150093526A1, except that the temperature of the distilled water is 23 ° C, the beaker diameter is about 10 cm and the test duration is limited to 24 hours. The results are single and average disintegration time (time to reach film rupture) and single and average dissolution time (time to reach no visible solid residue). Unless otherwise specified, the dissolution test method uses distilled water maintained at 23 ° C. The dissolution test method is not applicable to materials other than films having a total thickness equal to or less than 3 mm. A film of the present disclosure is considered water soluble if the average dissolution time measured according to the Dissolution Test Method is less than 24 hours.
[0091] 2) Water Vapor Transmission Rate (WVTR)
[0092] The test method was carried out according to ASTM F1249-13 under the following test conditions: a temperature of 40°C (±0.56°C) and a relative humidity of 50% (±3%) or 90% (±3%). The water vapor transmission rate was measured by an instrument Permatran-W Model 3 / 33 from Mocon (Minneapolis, USA) and is expressed in [g / m 2 / day] report. For materials outside the scope of ASTM F-1249-13 (§1.1), the water vapor transmission rate test method is not applicable.
[0093] 3) Scanning electron microscopy (SEM)
[0094] SEM images were recorded by an instrument Zeiss Ultra Plus from Carl Zeiss AG (Oberkochen, Germany) operated at 5.0 kV and equipped with an in-lens secondary electron detector.The sample specimens were prepared by cutting cross sections of the film via a surgical scalpel under room temperature conditions.
[0095] 4) Transmission electron microscopy (TEM)
[0096] TEM images of the sandwich film cross sections were recorded using a microscope JEOL-JEM-2200FS (JEOL GmbH, Germany). Cross sections were prepared from the films by applying a JEOL EM-09100IS Cryo Ion Slicer (JEOL GmbH, Germany).
[0097] 5) Basal spacing obtained by X-ray diffraction (XRD)
[0098] The CuKα radiation was used on a Bragg-Brentano-type instrument (Empyrean Malvern Panalytical BV, The Netherlands). X-ray diffraction was measured using a PIXcel-1D detector. The X-ray diffraction patterns were analyzed using Malvern Panalytical's Highscore Plus software to determine the basal spacing (d 001 ).
[0099] 6) Small-angle X-ray scattering (SAXS)
[0100] As a preparatory work, the birefringent optical properties of the dispersion were checked with homemade orthogonal polarizers. SAXS analysis of nematic dispersions was then performed at 23°C in 1 mm glass capillaries (Hilgenberg, Germany) by using the system Ganesha Air (SAXSLAB, Denmark). The system was equipped with a rotating anode copper X-ray source MicroMax 007HF (RigakuCorp., Japan) and a position sensitive detector PILATUS 300K (Dectris, Switzerland). The sample to detector position was adjustable, covering a wide range of scattering vectors q.
[0101] Example
[0102] Preparation of water-soluble polyvinyl alcohol (PVOH) solution (30% solids)
[0103] 700 g of double distilled water was heated to 85° C. in a beaker. 240 g of solid PVOH powder (Selvol 205, purchased from Sekisui Chemical in Japan), 30 g of glycerol (Cremer GLYC 3109921, purchased from Cremer Oleo in Germany) and 30 g of sorbitol ( P 100T, Roquette, France). The solution was kept at reflux for 2 hours at 85°C with stirring at up to 200 rpm to dissolve all solid components. Before use, the PVOH solution was homogenized and defoamed under vacuum (50 mbar) for 10 min with stirring at up to 2500 rpm using a SpeedMixer DAC 400.2VAC-P device from Hauschild (Germany).
[0104] Preparation of water dispersible hectorite dispersion (6% solids)
[0105] Sodium hectorite [Na 0.5 ] inter [Mg 2.5 Li 0.5 ] oct [Si4] tet O 10 F2: The high purity reagents SiO2 (Merck, fine particles, washed and calcined quartz), LiF (ChemPur, 99.9%, powder), MgF2 (ChemPur, 99.9%, 3 mm to 6 mm blocks, molten), MgO (Alfa Aesar, 99.95%, 1 mm to 3 mm molten agglomerates) and NaF (Alfa Aesar, 99.995%, powder) were carefully weighed according to the composition in the recipe. Crucibles made of molybdenum (25 mm outer diameter, 21 mm inner diameter, 180 mm long) were provided by Plansee SE (Reutte, Austria). For cleaning purposes, these crucibles were first heated to 1600° C. in a quartz tube placed in a copper-based high-frequency induction heating coil. The reagents were then added to the crucible under an argon atmosphere (glove box) and heated to 1200° C. under vacuum to remove any residual water. The crucible was then sealed with a molybdenum lid by heating both parts to the melting point of the molybdenum. Therefore, the sealed crucible was placed horizontally in a graphite heating furnace under an argon atmosphere and rotated at 1750°C for 80 minutes. Then, the crucible was opened, the resulting sodium hectorite was collected, ground via a planetary ball mill, and dried in a clean crucible at 250°C under an argon atmosphere for 14 hours. Then, the crucible was sealed with a molybdenum lid and annealed in a graphite heating furnace at 1045°C for 6 weeks to increase the homogeneity of the sodium hectorite. Then, the material was placed in a desiccator at (23°C, 43% relative humidity) to achieve a hydrated form [Na 0.5 ] inter [Mg 2.5 Li 0.5 ] oct [Si4] tet O 10F2·[H2O]2. Then, double distilled water was added to reach a 6% hectorite dispersion in water. Finally, the dispersion was placed at 23°C for 1 week to allow the hectorite nanosheets to spontaneously delaminate, thereby obtaining the maximum aspect ratio of the hectorite nanosheets. The aspect ratio ranged between 400 and 40,000.
[0106] Preparation of water dispersible hectorite / PEG nanocomposite dispersion (1% solids)
[0107] First, 117g of 6% hectorite water dispersion was diluted with 583g of double distilled water at 23°C to obtain 700g of 1% hectorite water dispersion. 3g of PEG 10,000g / mol provided by Sigma-Aldrich was dissolved separately with 297g of double distilled water at 23°C to obtain 300g of 1% PEG 10000 solution. The dispersion and solution were mixed together at 23°C to obtain 1000g of 1% hectorite / PEG 10000 water dispersion (ratio 70:30). The birefringent optical properties indicate that the hectorite nanosheets are self-oriented parallel to each other in the dispersion. 1D small angle X-ray scattering (SAXS) analysis confirmed the nematic liquid crystal state of the dispersion.
[0108] Preparation of water dispersible hectorite / PEO nanocomposite dispersion (1% solids)
[0109] First, 117g of 6% hectorite water dispersion was diluted with 583g of double distilled water at 23°C to obtain 700g of 1% hectorite water dispersion. 3g of PEO 2000000g / mol provided by Sigma-Aldrich was dissolved separately with 297g of double distilled water at 80°C under stirring to obtain 300g of 1% PEO 2000000 solution. The dispersion and solution were mixed together at 23°C to obtain 1000g of 1% hectorite / PEO 2000000 water dispersion (ratio 70:30). The birefringent optical properties indicate that the hectorite nanosheets are self-oriented parallel to each other in the dispersion. 1D small angle X-ray scattering (SAXS) analysis confirmed the nematic liquid crystal state of the dispersion.
[0110] Preparation of water dispersible hectorite / PVOH nanocomposite dispersion (5% solids)
[0111] First, 333 g of 6% hectorite aqueous dispersion was diluted with 67 g of double distilled water at 23 ° C to obtain 400 g of 5% hectorite aqueous dispersion. 30 g of PVOH grade Poval 10-98 provided by Kuraray was dissolved separately with 570 g of double distilled water at 80 ° C under stirring to obtain 600 g of 5% PVOH solution. The dispersion and solution were mixed together at 23 ° C to obtain 1000 g of 5% hectorite / PVOH aqueous dispersion (ratio 40:60). The birefringent optical properties indicate that the hectorite nanosheets are self-oriented parallel to each other in the dispersion. 1D small angle X-ray scattering (SAXS) analysis confirmed the nematic liquid crystal state of the dispersion.
[0112] Laboratory-scale fabrication of water-soluble films with integrated water-dispersible nanocomposite barriers
[0113] All aqueous solutions / dispersions were homogenized at 2500 rpm using a SpeedMixer DAC 400.2VAC-P from Hauschild & Co KG (Hamm, Germany) and degassed at (23° C., 50 mbar) for 5 minutes (before using them). A 36 μ thick polyethylene terephthalate (PET) film grade purchased from Bleher Folientechnik GmbH (Germany) was placed on a 501 was used as a carrier and further surface treated. As a next step, the carrier film (as previously described) was coated with a 30% PVOH solution using an automatic knife coating device (ZAA 2300, Zehntner GmbH Testing Instruments, Switzerland). The speed was set to 15 mm / s and the blade height was set to 250 μm. The wet coating was dried at 60° C. for 30 min, and the resulting dry layer was about 28 μm thick and consisted of 80% PVOH grade Selvol 205, 10% glycerol, 10% sorbitol.
[0114] 1) Water-soluble membrane with integrated water-dispersible hectorite / PEG nanocomposite barrier
[0115] In one embodiment, the hectorite / PEG nanocomposite barrier is applied by spraying using a fully automatic spraying system (SATA 4000LAB HVLP1.0mm spray gun purchased from SATA, Germany). The distance between the nozzle and the PET film coated with PVOH is set to 17cm. Subsequently, 1% hectorite / PEG nanocomposite dispersion (as previously described) is fed into the nozzle under a constant 4bar pressure and applied to the PET film coated with PVOH. The wet coating is dried at 50°C for 30min, and the resulting dried layer is 40nm thick. The spraying and drying cycle is repeated 100 times, and the resulting dried layer is 4 μm thick and is composed of 70% hectorite and 30% PEG 10000g / mol. As a next step, the nanocomposite barrier was coated with a 30% PVOH solution (as previously described) using an automated knife coating apparatus (as previously described), and the resulting dry layer was approximately 26 μm thick and consisted of 80% PVOH, 10% glycerol, 10% sorbitol. At this point, the carrier PET film was removed, resulting in a water-soluble film with an integrated nanocomposite barrier.
[0116] 2) Water-soluble membrane with integrated water-dispersible hectorite / PEO nanocomposite barrier
[0117] In one embodiment, the hectorite / PEO nanocomposite barrier is applied by spraying using a fully automatic spraying system (SATA 4000LAB HVLP1.0mm spray gun purchased from SATA, Germany). The distance between the nozzle and the PET film coated with PVOH is set to 17cm. Subsequently, 1% hectorite / PEO nanocomposite dispersion (as previously described) is fed into the nozzle under a constant 4bar pressure and applied to the PET film coated with PVOH. The wet coating is dried at 50°C for 30min, and the resulting dried layer is 40nm thick. The spraying and drying cycle is repeated 100 times, and the resulting dried layer is 4 μm thick and is composed of 70% hectorite and 30% PEO 2000000g / mol. As a next step, the nanocomposite barrier was coated with a 30% PVOH solution (as previously described) using an automated knife coating apparatus (as previously described), and the resulting dry layer was approximately 26 μm thick and consisted of 80% PVOH, 10% glycerol, 10% sorbitol. At this point, the carrier PET film was removed, resulting in a water-soluble film with an integrated nanocomposite barrier.
[0118] 3) Water-soluble membrane with integrated water-dispersible hectorite / PVOH nanocomposite barrier
[0119] In one embodiment, the hectorite / PVOH nanocomposite barrier is applied by a blade coating device (ZAA 2300, Zehntner GmbH TestingInstruments, Switzerland). The speed is set to 15 mm / s and the blade height is set to 100 μm. A 5% hectorite / PVOH nanocomposite dispersion (as previously described) is applied to a PVOH-coated PET film. The wet coating is dried at 60° C. for 4 hours and consists of 40% hectorite and 60% PVOH grade Poval 10-98. As a next step, the nanocomposite barrier is coated with a 30% PVOH solution (as previously described) using the same equipment, and the resulting dry layer is about 26 μm thick and consists of 80% PVOH, 10% glycerol, 10% sorbitol. At this point, the carrier PET film is removed to obtain a water-soluble film with an integrated nanocomposite barrier.
[0120] Table 1
[0121]
[0122] Comparative Example
[0123] The following comparative examples consist of a water-soluble film with an integrated barrier layer made of a barrier material that is non-dispersible in water and is therefore not suitable for this application.
[0124] Preparation of PVDC solution (20% solids)
[0125] 1000g methyl ethyl ketone (MEK) and ethyl acetate (EA) solvent mixture (60:40) was heated to 50°C in a glass beaker in a protective fume hood. 200g polyvinylidene chloride (powder grade Resin F310, deriving from Asahi Kasei) was added under magnetic stirring. Once completed, the stirring level was increased to the maximum level and heating was turned off. After continuous stirring for about 2 hours at the maximum level, the PVDC powder was completely dissolved. The solution was stored overnight at room temperature (RT) to eliminate any residual foam.
[0126] A. Water-soluble film with integrated water-insoluble PVDC barrier
[0127] In one embodiment, the first water-soluble polymer layer is formed by coating a 50 μm aqueous PVOH solution (30% solids) onto an untreated PET carrier film (Hostaphan RN 50-350, available from Mitsubishi) via an anilox roll at 80° C. and removing the water via a convection dryer from Drytec set at 95° C. The second and third water-soluble polymer layers are added to the first water-soluble polymer layer via the same process. The resulting dried layer is 39 μm thick and has a composition of 80% PVOH grade Selvol 205 (available from Sekisui Chemicals), 9.5% glycerol, 9.5% sorbitol, and 1% Hecostat (available from Hecoplast). Then, a non-dispersible PVDC barrier was added by coating a 30μ PVDC solution in MEK / EA onto the water-soluble polymer layer via an anilox roll at 50°C and removing the MEK / EA solvent via a convection dryer from Drytec set at 95°C. The resulting dry layer was 3μ thick and its composition was 100% PVDC grade F310 (available from Asahi Kasei). One further water-soluble polymer layer was added by coating a 50μ aqueous PVOH solution onto the non-dispersible PVDC barrier layer via an anilox roll at 80°C and removing the water via a convection dryer from Drytec set at 95°C. The resulting dry layer was 15μ thick and its composition was 80% PVOH grade Selvol 205 (available from Sekisui Chemicals), 10% glycerol, 10% sorbitol.
[0128] Table 2
[0129]
[0130] As shown in Table 2 above, although the PVDC barrier layer provides a low WVTR, the water-insoluble PVDC does not meet the inventive requirements according to the present disclosure.
[0131] The dimensions and values disclosed herein are not to be understood as being strictly limited to the exact numerical values cited. Instead, unless otherwise indicated, each such dimension is intended to represent the stated value and a functionally equivalent range around that value. For example, a dimension disclosed as "40 mm" is intended to mean "about 40 mm".
[0132] Unless expressly excluded or otherwise limited, each document cited herein, including any cross-referenced or related patent or patent application and any patent application or patent to which this application claims priority or the benefit of, is hereby incorporated by reference in its entirety. The citation of any document is not an admission that it is prior art to any of the present invention disclosed or claimed herein, or an admission that it, by itself or in combination with any one or more of the references, proposes, suggests, or discloses any such invention. In addition, to the extent that any meaning or definition of a term in this invention conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this invention shall govern.
[0133] Although specific embodiments of the present invention have been illustrated and described, it will be apparent to those skilled in the art that various other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended that all such changes and modifications within the scope of the present disclosure be covered in the appended claims.
Claims
1. A water-soluble film, comprising: a) A first water-soluble polymer layer having a surface b) A second water-soluble polymer layer having a surface c) a water-dispersible nanocomposite barrier layer disposed between the first layer and the second layer.
2. The water-soluble film of claim 1, wherein the WVTR of the water-soluble film is about 0.01 g / m when measured according to ASTM test method F1249-13 at a temperature of 40°C and a relative humidity of 50%. 2 / day to about 100g / m 2 / sky. 3 . The water-soluble film according to claim 1 , wherein the average thickness of the water-soluble polymer layer is from about 1 μm to about 1000 μm. 4 . The water-soluble film according to claim 1 , wherein the first water-soluble polymer layer and the second water-soluble polymer layer comprise different water-soluble polymers.
5. The water-soluble film of any preceding claim, wherein at least one of the first water-soluble polymer layer or the second water-soluble polymer layer comprises more than one water-soluble polymer sublayer.
6. The water-soluble film according to any one of the preceding claims, wherein the water-soluble polymer layer comprises a water-soluble polymer, and the water-soluble polymer is at least one of polyvinyl alcohol, polyethylene oxide, methylcellulose or sodium alginate, preferably, wherein the water-soluble polyvinyl alcohol is a partially or completely hydrolyzed homopolymer or copolymer.
7. The water-soluble polymer layer of claim 6, wherein the water-soluble polyvinyl alcohol is a homopolymer having a degree of hydrolysis of about 70% to about 100%.
8. The water-soluble polymer layer of claim 6, wherein the water-soluble methylcellulose is from about 18% to about 32% methoxy substituted and from about 4% to about 12% hydroxy-propoxy substituted.
9. The water-soluble film according to any one of the preceding claims, wherein the water-soluble polymer layer comprises at least one water-soluble plasticizer, preferably wherein the plasticizer is at least one of water, glycerol, sorbitol, propylene glycol (PG), trimethylene glycol (PDO), trimethylolpropane (TMP), methylpropanediol (MPD), 2-methyl-1,3 propanediol (MPO) or a mixture thereof.
10. The water-soluble film of any preceding claim, wherein the water-dispersible nanocomposite barrier layer is distinct from the water-soluble polymer layer when observed via optical microscopy or scanning electron microscopy.
11. The water-soluble film according to any one of the preceding claims, wherein the water-dispersible nanocomposite barrier layer is a nanocomposite comprising nanoscale ordered spaced hydrophilic nanosheets and intercalated polymer fillers, wherein the basal spacing measured via XRD is less than Preferably, the average aspect ratio of the hydrophilic nanosheets is greater than about 100, more preferably greater than about 1000, and most preferably greater than about 10000.
12. The water-dispersible nanocomposite barrier layer of claim 11, wherein the average aspect ratio of the hydrophilic nanoplatelets is from about 400 to about 40,000.
13. The water-dispersible nanocomposite barrier layer of claim 11, wherein the hydrophilic nanosheets are clay nanosheets.
14. The water-dispersible nanocomposite barrier layer of claim 13, wherein the hydrophilic nanoplatelets are natural, modified or synthetic smectite or natural, modified or synthetic vermiculite.
15. The water-dispersible nanocomposite barrier layer of claim 13, wherein the hydrophilic nanoplatelets are trioctahedral montmorillonite, such as synthetic hectorite [Na 0.5 ] inter [Mg 2.5 Li 0.5 ] oct [Si4] tet O 10 F2.
16. A method for making a water-soluble film, the method comprising: a) applying a first aqueous solution of a water-soluble polymer composition onto the surface of a removable flat carrier such as a PET film or a steel tape b) removing water from the first aqueous solution of the water-soluble polymer composition to obtain a first water-soluble polymer layer c) applying an aqueous dispersion of a water-dispersible nanocomposite material onto the surface of the first water-soluble polymer layer d) removing water from the aqueous dispersion of the water-dispersible nanocomposite material to obtain a water-dispersible nanocomposite barrier layer e) applying a second aqueous solution of a water-soluble polymer composition onto the surface of the water-dispersible nanocomposite barrier layer f) removing water from the second aqueous solution of the water-soluble polymer composition to obtain a second water-soluble polymer layer g) removing the flat support from the resulting water-soluble nanocomposite barrier film.