Mat material, exhaust gas purification device, and method for manufacturing mat material
By using inorganic fibers and needle punching in the mat material to form interweaving points, and combining inorganic and organic binders, the shear coefficient and retention force of the mat material are improved, and the shear coefficient of the existing mat material under high temperature conditions is solved. The problem of low and insufficient holding force is eliminated, and stable and efficient sealing of the exhaust gas purification device is achieved.
Patent Information
- Application Number
- CN202380023662.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-22
- Publication Date
- 2024-10-15
AI Technical Summary
Existing mats have low shear coefficients and insufficient holding power in high-temperature exhaust gas purification devices, and organic bonding materials are easily thermally decomposed by high temperatures, resulting in reduced holding power.
Inorganic fiber mats are used, and multiple interwoven points are formed through needle punching. The density is in the range of 0.5/cm2≤ρ<18/cm2, and there are no interwoven points in specific areas on the surface or back. Inorganic binders and organic The binder adheres to the fiber surface in a dispersed or agglomerated state, forming a high-friction coating layer to increase the shear coefficient and retention force.
The shear coefficient and retention force of the mat material are improved to ensure that the inorganic binder does not burn out under high temperature conditions, prevent the mat material from shifting, and take into account fiber adhesion to prevent scattering.
Smart Images

Figure CN118786259A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a mat material, an exhaust gas purification device and a method for manufacturing the mat material. Background Art
[0002] Exhaust gas discharged from internal combustion engines such as diesel engines contains particulate matter (hereinafter also referred to as PM), and in recent years, the PM has become a problem of harming the environment and human body. In addition, since the exhaust gas also contains harmful gas components such as CO, HC, and NOx, there is also concern that these harmful gas components will affect the environment and human body.
[0003] Therefore, as an exhaust gas purification device for capturing PM in exhaust gas and purifying harmful gas components, various schemes of exhaust gas purification devices consisting of an exhaust gas treatment body (which is composed of porous ceramics such as silicon carbide and cordierite), a shell for accommodating the exhaust gas treatment body, and a holding sealing material (mat) arranged between the exhaust gas treatment body and the shell. The main purpose of arranging the holding sealing material (mat) is to: prevent the exhaust gas treatment body from contacting with the shell covering its outer periphery and being damaged due to vibration or impact caused by the driving of the car, etc.; prevent exhaust gas from leaking from between the exhaust gas treatment body and the shell; etc.
[0004] Patent Document 1 discloses that the density of interlaced points formed by needle punching is set to 0.5 pieces / cm 2 ≤ρ<20 pieces / cm 2 , thereby having both the required sheet strength and high resilience. In addition, Patent Document 1 discloses that the sheet contains an organic binder to improve the adhesion between fibers and prevent the fibers from flying when the sheet is handled.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2007-292040 Summary of the invention
[0008] Problems to be solved by the invention
[0009] However, in Patent Document 1, since only an organic binder is added, the shear coefficient of the mat is low and the holding force is smaller than expected. In addition, the organic binder contained in the sheet is thermally decomposed and burned by the high-temperature exhaust gas immediately after using the exhaust gas purification device, which has the problem of reduced holding force.
[0010] Means for solving problems
[0011] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a mat material having a high shear coefficient and a high holding force.
[0012] That is, the mat material of the present invention comprises inorganic fibers and has a plurality of interlaced points formed by needle punching on at least one of the surface or the back surface, and the above-mentioned mat material is characterized in that the density ρ of the above-mentioned interlaced points is 0.5 pieces / cm 2 ≤ρ<18 pieces / cm 2 and at least one of the first region and the second region is arranged in an area of 25 mm × 25 mm, the first region is a 4 mm × 4 mm region where the above-mentioned interweaving points do not exist, the second region is a 3 mm × 8 mm region where the above-mentioned interweaving points do not exist, the above-mentioned mat material contains an inorganic binder, the shear coefficient is greater than 0.20, and the back pressure after firing is greater than 50 kPa.
[0013] In the mat material of the present invention, the density of the interlaced points is 0.5 / cm 2 ≤ρ<18 pieces / cm 2 range, and at least one of the first region and the second region is configured, the first region is a 4mm×4mm region where the above-mentioned interweaving points do not exist, and the second region is a 3mm×8mm region where the above-mentioned interweaving points do not exist. If the density ρ of the interweaving points is small, there is a tendency for the shear coefficient to become smaller, but the mat material of the present invention has at least one of the first region and the second region and contains an inorganic binder, so although the density ρ of the interweaving points is small, it also has a high shear coefficient of more than 0.20. Furthermore, even if high-temperature exhaust gas flows into the exhaust gas purification device, the inorganic binder will not burn off, so the retention force is high, and the rear pressure after firing is more than 50kPa. Furthermore, since there is also an inorganic binder on the surface of the mat material, it is possible to suppress the position of the mat material from shifting due to vibration and impact.
[0014] In the mat of the present invention, the weight ratio of the inorganic binder to the mat (weight of the inorganic binder / weight of the mat) is preferably more than 0 wt % and not more than 10 wt %.
[0015] When the weight ratio of the inorganic binder to the mat material is within the above range, the holding force can be sufficiently improved.
[0016] The mat material of the present invention preferably further contains an organic binder.
[0017] By making the mat material further contain an organic binder, the adhesion between the fibers is improved, and the fibers are prevented from scattering during the handling of the mat material.
[0018] In the mat material of the present invention, the weight ratio of the organic binder to the mat material (weight of the organic binder / weight of the mat material) is preferably more than 0 wt % and not more than 10 wt %.
[0019] When the weight ratio of the organic binder to the mat material is within the above range, both the fiber scattering prevention effect and the high holding force can be achieved.
[0020] In the mat material of the present invention, it is preferred that the inorganic binder and the organic binder are respectively attached to the surface of the inorganic fibers in a dispersed state.
[0021] If the inorganic binder and the organic binder are respectively attached to the surface of the inorganic fiber in a dispersed state, the inorganic binder is dispersed in the film formed by the organic binder. The film in this state has excellent mechanical strength, so it can prevent the inorganic fibers from sliding against each other and improve the holding force.
[0022] The mat material of the present invention preferably further contains a polymer dispersant.
[0023] When the mat material further contains a polymer-based dispersant, the organic binder and the inorganic binder can be easily attached to the surface of the inorganic fiber in a dispersed state.
[0024] The mat material of the present invention is preferably formed by adhering aggregates composed of the inorganic binder and the organic binder to the surface of the inorganic fibers.
[0025] The aggregate composed of the inorganic binder and the organic binder can form irregularities on the surface of the inorganic fibers, thereby increasing the friction between the inorganic fibers and improving the holding force.
[0026] In the mat material of the present invention, it is preferred that the covering layer composed of a mixture of the inorganic binder and the organic binder covers at least a part of the surface of the inorganic fibers.
[0027] The coating layer composed of a mixture of an inorganic binder and an organic binder has higher mechanical strength than a coating layer composed of only an organic binder, so that the coating layer is less likely to peel off, and the friction resistance between the inorganic fibers can be increased.
[0028] In the mat material of the present invention, the covering layer is preferably formed by a continuous scaly mixture of the inorganic binder and the organic binder.
[0029] When the covering layer is formed of the scaly mixture, a large number of irregularities derived from the scaly mixture are formed on the surface of the covering layer, and the frictional resistance between the inorganic fibers can be further increased.
[0030] In the mat material of the present invention, the coating layer preferably has a multi-step shape.
[0031] When the coating layer has a multi-step shape, the frictional resistance between the inorganic fibers can be further increased.
[0032] In the mat material of the present invention, it is preferred that a granular mixture of the inorganic binder and the organic binder is adhered to the surface of the covering layer.
[0033] When a particulate mixture of an inorganic binder and an organic binder is attached to the surface of the covering layer, the frictional resistance between the inorganic fibers can be further increased compared to the case of the covering layer alone.
[0034] The mat of the present invention preferably has the shear coefficient of 105% or more of the shear coefficient of a mat under the same conditions except that the inorganic binder is not contained.
[0035] In addition, the mat material under the same conditions except that the inorganic binder is not contained corresponds to the mat material of the present invention except that the inorganic binder is removed.
[0036] The mat of the present invention preferably has a plurality of first regions and / or the second regions arranged in an area of 25 mm×25 mm.
[0037] If a plurality of first regions and / or second regions are arranged in an area of 25 mm×25 mm, the surface pressure of the mat can be increased.
[0038] The mat of the present invention preferably further has a protective sheet provided on at least one surface.
[0039] If the mat further has a protective sheet provided on the surface thereof, it is possible to suppress positional deviation and / or dense wrinkles of the mat when the mat is wound around the exhaust gas treating body, and generation of gaps in the fitting portion.
[0040] The mat material of the present invention is preferably used in an exhaust gas purification device.
[0041] The mat material of the present invention has a high shear coefficient and a high holding force, and therefore can be suitably used in an exhaust gas purification device.
[0042] The exhaust gas purification device of the present invention comprises: an exhaust gas treatment body; a metal shell that accommodates the exhaust gas treatment body; a mat material that is arranged between the exhaust gas treatment body and the metal shell to hold the exhaust gas treatment body; the exhaust gas purification device is characterized in that the mat material is the mat material of the present invention.
[0043] In the exhaust gas purifying device of the present invention, since the mat material of the present invention is disposed between the exhaust gas treating body and the metal casing, the exhaust gas treating body can be stably held.
[0044] The first embodiment of the method for manufacturing a mat material of the present invention is characterized in that it has an attaching step of attaching an inorganic binder to an inorganic fiber aggregate, wherein the inorganic fiber aggregate comprises inorganic fibers, and at least one of the surface or the back surface has a plurality of interlaced points formed by needle punching, and the density ρ of the interlaced points is 0.5 pieces / cm 2 ≤ρ<18 pieces / cm 2In the range of 25mm×25mm, at least one of the first area and the second area is arranged in the area of 25mm×25mm, the first area is a 4mm×4mm area where the above-mentioned interweaving point does not exist, and the second area is a 3mm×8mm area where the above-mentioned interweaving point does not exist.
[0045] The second embodiment of the method for manufacturing a mat material of the present invention is characterized in that it has an attaching step of attaching both an inorganic binder and an organic binder to an inorganic fiber aggregate, wherein the inorganic fiber aggregate comprises inorganic fibers, and at least one of the surface or the back surface has a plurality of interlacing points formed by needle punching, and the density ρ of the interlacing points is 0.5 pieces / cm 2 ≤ρ<18 pieces / cm 2 In the range of 25mm×25mm, at least one of the first area and the second area is arranged in the area of 25mm×25mm, the first area is a 4mm×4mm area where the above-mentioned interweaving point does not exist, and the second area is a 3mm×8mm area where the above-mentioned interweaving point does not exist.
[0046] In a second aspect of the mat production method of the present invention, in the attaching step, preferably, a dispersion in which the inorganic binder and the organic binder are dispersed in a dispersion medium is attached to the inorganic fiber aggregate.
[0047] In a second aspect of the method for producing a mat according to the present invention, in the attaching step, preferably, an aggregated dispersion obtained by aggregating the inorganic binder and the organic binder is attached to the inorganic fiber aggregate.
[0048] According to the method for producing a mat of the present invention, the mat of the present invention can be easily produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 This is a perspective view schematically showing an example of the mat material of the present invention.
[0050] Figure 2 yes Figure 1 AA line cross-section diagram.
[0051] Figure 3 This is a schematic diagram showing an example of the arrangement of interlaced points in the mat of the present invention.
[0052] Figure 4 This is a schematic diagram showing an example of a mat material in which interlacing points are evenly arranged.
[0053] Figure 5 This is an example of an electron microscope image of the mat material of the present invention which is magnified.
[0054] Figure 6 This is another example of an electron microscope image of the mat material of the present invention which is magnified.
[0055] Figure 7 This is another example of an electron microscope image of the mat material of the present invention which is magnified.
[0056] Figure 8 This is another example of an electron microscope image of the mat material of the present invention which is magnified.
[0057] Fig. 9 1 is a conceptual diagram schematically showing a shear failure load test device.
[0058] Fig.10 This is a perspective view schematically showing another example of the mat of the present invention.
[0059] Fig.11 This is a cross-sectional view schematically showing an example of the exhaust gas purification device of the present invention. DETAILED DESCRIPTION
[0060] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and can be applied with appropriate changes within the scope of the gist of the present invention.
[0061] [Material]
[0062] The mat material of the present invention comprises inorganic fibers and has a plurality of interlaced points formed by needle punching on at least one of the surface or the back surface, wherein the density of the interlaced points is 0.5 / cm 2 ≤ρ<18 pieces / cm 2 and at least one of the first region and the second region is arranged in an area of 25 mm × 25 mm, the first region is a 4 mm × 4 mm region where the above-mentioned interweaving points do not exist, the second region is a 3 mm × 8 mm region where the above-mentioned interweaving points do not exist, the above-mentioned mat material contains an inorganic binder, the shear coefficient is greater than 0.20, and the back pressure after firing is greater than 50 kPa.
[0063] Figure 1 is a perspective view schematically showing an example of the mat material of the present invention, Figure 2 yes Figure 1 AA line cross-section diagram.
[0064] like Figure 1 As shown, the mat material 1 of the present invention is composed of a mat having a predetermined length (hereinafter, Figure 1 Indicated by arrow L), width ( Figure 1 Indicated by arrow W) and thickness ( Figure 1 The pad 10 is formed of a substantially rectangular flat plate shape when viewed from above (indicated by arrow T in the figure).
[0065] exist Figure 1In the mat 10 shown, a convex portion 11 is formed at one of the ends on the lengthwise side of the mat 10, and a concave portion 12 is formed at the other end. When the mat 10 is wound around the exhaust gas treatment body for assembling the exhaust gas purification device described later, the convex portion 11 and the concave portion 12 of the mat 10 are shaped to fit into each other. If such a convex portion 11 and a concave portion 12 are provided, the sealing performance is improved when the mat 10 is arranged in the exhaust gas purification device described later.
[0066] A plurality of interlaced points 15 (also referred to as needle punch marks) are formed on the main surface of the mat 10 by needle punching.
[0067] The pad 10 has two main surfaces, one being the front surface and the other being the back surface.
[0068] It should be noted that the mat used in the mat material of the present invention does not necessarily have convex portions and concave portions at the end portions.
[0069] In addition, the shape of the end portions of the mat may be an L-shape, and the end portions may be fitted together when the mat is wrapped around an object.
[0070] The mat itself may be a mat material, or may further include a protective sheet described below on at least one surface of the mat.
[0071] like Figure 2 As shown, each interlacing point 15 is formed on a straight line perpendicular to the thickness direction of the pad 10. The shape of the interlacing point 15 can be a curve or can be inclined relative to the thickness direction of the pad 10. In addition, the interlacing point 15 may not penetrate the pad 10 in the thickness direction.
[0072] The thickness of the mat is not particularly limited, but is preferably 2 mm to 40 mm. If the thickness of the mat exceeds 40 mm, the mat loses its flexibility, making it difficult to handle when the mat is wound around the exhaust gas treatment body. In addition, the mat is prone to wrinkles and cracks.
[0073] If the thickness of the mat is less than 2 mm, the holding force of the mat material is insufficient and the exhaust gas treatment body is easy to fall off. In addition, when the volume of the exhaust gas treatment body changes, it is difficult for the mat material to absorb the volume change of the exhaust gas treatment body. Therefore, the exhaust gas treatment body is prone to cracks.
[0074] The mat is composed of inorganic fibers.
[0075] The inorganic fibers are not particularly limited, but are preferably composed of at least one selected from the group consisting of alumina fibers, silica fibers, alumina silica fibers, mullite fibers, biosoluble fibers, and glass fibers.
[0076] When the inorganic fiber is at least one of alumina fiber, silica fiber, alumina silica fiber and mullite fiber, the heat resistance is excellent, so even when the exhaust gas treatment body is exposed to a sufficiently high temperature, it will not deteriorate, and the function as a mat material can be fully maintained. In addition, when the inorganic fiber is a biosoluble fiber, when the exhaust gas purification device is made using the mat material, even if the scattered inorganic fiber is inhaled, it will dissolve in the body, so it will not cause harm to the health of the operator.
[0077] The alumina fibers may contain additives such as calcium oxide, magnesium oxide, and zirconium oxide in addition to aluminum oxide.
[0078] The composition ratio of the alumina-silica fibers is preferably Al2O3:SiO2=60:40 to 80:20, more preferably Al2O3:SiO2=70:30 to 74:26 in terms of weight ratio.
[0079] The mats can be produced by needle punching.
[0080] The average fiber length of the inorganic fibers is preferably 1 mm to 150 mm, more preferably 10 mm to 80 mm.
[0081] If the average fiber length of the inorganic fiber is less than 1 mm, the fiber length of the inorganic fiber is too short, so the interweaving of the inorganic fibers becomes insufficient, the entanglement on the exhaust gas treatment body is reduced, and the mat is easily broken. In addition, if the average fiber length of the inorganic fiber exceeds 150 mm, the fiber length of the inorganic fiber is too long, so the number of fibers constituting the mat is reduced, and the density of the mat is reduced. As a result, the shear strength of the mat is reduced.
[0082] Intertwining points are formed on the surface or the back surface of the mat material.
[0083] The density of interlacing points is 0.5 / cm 2 ≤ρ<18 pieces / cm 2 range.
[0084] When interlaced points are formed on both the front and back surfaces of the mat material, the interlaced point density ρ is the density of interlaced points measured on the main surface having a higher density of interlaced points, the front or back surface.
[0085] At least one of the first region and the second region is arranged in a 25 mm×25 mm area on the front or back side of the mat material, the first region is a 4 mm×4 mm area with no interlacing points, and the second region is a 3 mm×8 mm area with no interlacing points.
[0086] In the mat material of the present invention, high surface pressure is achieved by arranging at least one of the first region and the second region.
[0087] It should be noted that the main surface of the mat material on which the first region and / or the second region is arranged is determined to be the same main surface as the main surface on which the density of the interlaced points is measured.
[0088] In the mat of the present invention, it is preferred that both the first region and the second region are arranged in a 25 mm×25 mm region on the front or back surface.
[0089] The first region and the second region may be arranged separately, but it is more preferable that the first region overlaps with the second region. When the first region overlaps with the second region, the area without interlacing points becomes larger, so the surface pressure of the mat can be increased.
[0090] Figure 3 This is a schematic diagram showing an example of the arrangement of interlaced points in the mat of the present invention.
[0091] exist Figure 3 Therefore, it can be said that there is a 4 mm × 4 mm area ( Figure 3 The area indicated by the solid square in the figure) is the first area 17, and the area of 3 mm × 8 mm where there is no interlacing point 15 ( Figure 3 The area represented by the dotted rectangle in the figure is the second area 18.
[0092] It should be noted that Figure 3 Not all of the first regions 17 and the second regions 18 are shown in the figure.
[0093] Figure 4 This is a schematic diagram showing an example of a mat material in which interlacing points are evenly arranged.
[0094] Figure 4 In the embodiment, the interlacing points 15 are evenly arranged at intervals of 2.8 mm.
[0095] Figure 4 The 4 mm×4 mm square and 3 mm×8 mm rectangle shown each include one or more interlacing points. The 4 mm×4 mm square that does not correspond to the first region and the 3 mm×8 mm rectangle that does not correspond to the second region are marked with "×".
[0096] Therefore, in Figure 4 In the mat material shown, both the first area and the second area cannot be configured.
[0097] The method of counting the number of the first area and the second area in the 25 mm×25 mm area is as follows.
[0098] (1) A 4 mm x 4 mm region (first region) where no interlacing point is formed is found. At this time, a plurality of first regions are selected so as not to overlap with each other.
[0099] (2) Find a 3 mm x 8 mm area (second area) where no interlacing points are formed. At this time, multiple second areas are selected so that they do not overlap with each other. The second area may overlap with the first area.
[0100] (3) A 25 mm×25 mm region is selected in which the number of mutually non-overlapping first regions and the number of mutually non-overlapping second regions are the largest.
[0101] The above operation was performed on 10 samples and the average value was taken.
[0102] It should be noted that the above operations can be performed using commercially available image processing software or the like.
[0103] In the area of 25 mm×25 mm, a plurality of first areas and / or second areas are preferably arranged.
[0104] If a plurality of first regions and / or second regions are arranged in an area of 25 mm×25 mm, the surface pressure of the mat can be increased.
[0105] Configuring multiple first areas and / or second areas refers to a situation where the total number of first areas and the number of second areas is greater than 2, including a situation where multiple first areas are configured, a situation where multiple second areas are configured, and a situation where multiple first areas and multiple second areas are configured.
[0106] It is preferable that a third region of 4 mm×4 mm having four or more interlaced points is arranged in a region of 25 mm×25 mm on the front or back surface of the mat.
[0107] When the third region is provided, the inorganic fibers are strongly entangled with each other in the third region, and thus the shear strength of the mat can be increased.
[0108] It should be noted that the method of counting the number of the third regions within the 25 mm×25 mm region is the same as the method of counting the number of the first regions described above.
[0109] The mat material contains an inorganic binder (also called an inorganic bonding material).
[0110] Since the mat material of the present invention contains an inorganic binder, the shear coefficient is high. Furthermore, even if high-temperature exhaust gas flows into the exhaust gas purification device, the inorganic binder will not burn, so the holding force is high. Furthermore, since the inorganic binder is also present on the surface of the mat material, the position of the mat material can be suppressed from shifting due to vibration and impact.
[0111] Examples of the inorganic binder include alumina sol and silica sol.
[0112] The weight ratio of the inorganic binder to the mat material (weight of the inorganic binder / weight of the mat material) is preferably more than 0 wt % and not more than 10 wt %.
[0113] When the weight ratio of the inorganic binder to the mat material is within the above range, the holding force can be sufficiently improved.
[0114] The mat material may further contain an organic binder (also called an organic binding material).
[0115] By making the mat material further contain an organic binder, the adhesion between the fibers is improved, and the fibers are prevented from scattering during the handling of the mat material.
[0116] Examples of the organic binder include acrylic resins, acrylate emulsions, rubber emulsions, water-soluble organic polymers such as carboxymethyl cellulose and polyvinyl alcohol, thermoplastic resins such as styrene resins, and thermosetting resins such as epoxy resins.
[0117] The weight ratio of the organic binder to the mat material (weight of the organic binder / weight of the mat material) is preferably more than 0 wt % and not more than 10 wt %.
[0118] When the weight ratio of the organic binder to the mat material is within the above range, both the fiber scattering prevention effect and the high holding force can be achieved.
[0119] The contents of the organic binder and the inorganic binder contained in the mat can be measured, for example, by the following method.
[0120] First, a certain weight of the mat material of which the content is to be measured is collected as a sample. Next, an organic solvent (e.g., tetrahydrofuran) is selected to dissolve the organic binder contained in the sample, and the organic binder is dissolved and separated from the sample using a Soxhlet extractor. At this time, the inorganic binder contained in the dissolved organic binder is also separated from the sample, and the organic binder and the inorganic binder are recovered in the organic solvent.
[0121] Next, an organic solvent containing the organic binder and the inorganic binder is placed in a crucible, and the organic solvent is evaporated and removed by heating. The residue remaining in the crucible is regarded as the total weight of the organic binder and the inorganic binder relative to the mat material, and the content (weight %) relative to the weight of the mat material is calculated.
[0122] Furthermore, the crucible was heated at 600°C for 1 hour to burn off the organic binder. Since the inorganic binder remained in the crucible, it was regarded as the content (weight %) of the inorganic binder relative to the total of the organic binder and the inorganic binder, and the content was calculated. The remainder was the content (weight %) of the organic binder.
[0123] In the mat material, it is preferred that the inorganic binder and the organic binder are attached to the surface of the inorganic fibers in a dispersed state.
[0124] If the inorganic binder and the organic binder are respectively attached to the surface of the inorganic fiber in a dispersed state, the inorganic binder is dispersed in the film formed by the organic binder. The film in this state has excellent mechanical strength, so it can prevent the inorganic fibers from sliding against each other and improve the holding force.
[0125] In the mat material, it is preferred that the covering layer composed of a mixture of an inorganic binder and an organic binder covers at least a part of the surface of the inorganic fibers.
[0126] The coating layer composed of a mixture of an inorganic binder and an organic binder has higher mechanical strength than a coating layer composed of only an organic binder, so that the coating layer is less likely to peel off, and the friction resistance between the inorganic fibers can be increased.
[0127] The covering layer is preferably formed by continuous flake-like mixture (a mixture of an inorganic binder and an organic binder).
[0128] When the covering layer is formed of the scaly mixture, a large number of irregularities derived from the scaly mixture are formed on the surface of the covering layer, and the frictional resistance between the inorganic fibers can be further increased.
[0129] Figure 5 This is an example of an electron microscope image of the mat material of the present invention which is magnified.
[0130] like Figure 5 As shown, the coating layer 30 composed of a mixture of an inorganic binder and an organic binder covers a portion of the surface of the inorganic fiber 20. The coating layer 30 is formed by a continuous scaly mixture of the inorganic binder and the organic binder. A granular mixture 40 of the inorganic binder and the organic binder is attached to the surface of the inorganic fiber 20.
[0131] It should be noted that whether the coating layer or the particles are composed of a mixture of an inorganic binder and an organic binder can be confirmed by combining field observation with an electron microscope and elemental analysis.
[0132] Figure 6 This is another example of an electron microscope image of the mat material of the present invention which is magnified.
[0133] like Figure 6As shown, the coating layer 30 composed of a mixture of an inorganic binder and an organic binder covers a portion of the surface of the inorganic fiber 20. The coating layer 30 is formed by a continuous scaly mixture of the inorganic binder and the organic binder. A granular mixture 40 of the inorganic binder and the organic binder is attached to the surface of the inorganic fiber 20.
[0134] The thickness of the coating layer may be the same or different.
[0135] The shape of the coating layer with non-constant thickness is also called multi-step shape.
[0136] When the shape of the covering layer is multi-step, it can be said that the covering layer has irregularities on the surface, and thus the frictional resistance between the inorganic fibers can be further increased.
[0137] Whether the coating layer has surface irregularities, that is, whether the coating layer has a multi-step shape, is determined by magnifying the surface of the inorganic fiber 3000 times using a scanning electron microscope to check whether the coating layer has surface irregularities.
[0138] Figure 7 This is another example of an electron microscope image of the mat material of the present invention which is magnified.
[0139] like Figure 7 As shown, the coating layer 30 composed of a mixture of an inorganic binder and an organic binder covers a portion of the surface of the inorganic fiber 20. The coating layer 30 has a different thickness and is multi-stepped.
[0140] A granular mixture 40 of an inorganic binder and an organic binder adheres to the surface of the inorganic fibers 20 .
[0141] It is preferred that particles composed of a mixture of an inorganic binder and an organic binder adhere to the surface of the covering layer.
[0142] When particles composed of a mixture of an inorganic binder and an organic binder are attached to the surface of the covering layer, the frictional resistance between the inorganic fibers can be further increased compared to a case where the particles are not attached.
[0143] Figure 8 This is another example of an electron microscope image of the mat material of the present invention which is magnified.
[0144] like Figure 8 As shown, a coating layer 30 composed of a mixture of an inorganic binder and an organic binder covers a portion of the surface of the inorganic fiber 20. The coating layer 30 is formed by a continuous scaly mixture of an inorganic binder and an organic binder. The thickness of the coating layer 30 is different and is multi-stepped. A granular mixture 40 of an inorganic binder and an organic binder is attached to the surface of the coating layer 30.
[0145] The mat material preferably further contains a polymer dispersant.
[0146] When the mat material further contains a polymer-based dispersant, the organic binder and the inorganic binder can be easily attached to the surface of the inorganic fiber in a dispersed state.
[0147] The content of the polymer dispersant is preferably 50 ppm to 1000 ppm based on the weight of the inorganic fibers.
[0148] The mat material preferably has aggregates composed of an inorganic binder and an organic binder attached to the surface of the inorganic fibers.
[0149] The aggregate composed of the inorganic binder and the organic binder can form irregularities on the surface of the inorganic fibers, thereby increasing the friction between the inorganic fibers and improving the holding force.
[0150] The mat material may further contain a coagulant.
[0151] If the mat further contains a coagulant, the organic binder and the inorganic binder can be easily attached to the surface of the inorganic fibers in a coagulated state.
[0152] Whether the inorganic binder and the organic binder attached to the surface of the inorganic fiber are dispersed or aggregated can be confirmed by observing the surface of the inorganic fiber using SEM-EDX or the like.
[0153] The shear coefficient of the mat material of the present invention is 0.20 or more.
[0154] When the shear coefficient is 0.20 or more, the mat material is less likely to be sheared when the exhaust gas treatment body is pressed into a metal casing using the mat material of the present invention.
[0155] The shear coefficient is obtained by dividing the shear failure load by the relaxation surface pressure (relaxation surface pressure).
[0156] The shear failure load can be obtained by Fig. 9 The shear failure load is measured using the test apparatus shown.
[0157] Fig. 9 1 is a conceptual diagram schematically showing a shear failure load test device.
[0158] Fig. 9 The shear failure load test device 70 shown has test pieces 1a and 1b arranged on both sides of a stainless steel plate 73, and the outer sides thereof are clamped by a left clamp 71 and a right clamp 72. A plurality of protrusion members 74 are provided on the surfaces of the left clamp 71, the right clamp 72 and the stainless steel plate 73 on the surfaces in contact with the test pieces.
[0159] The test pieces 1 a and 1 b are fixed to the left jig 71 , the right jig 72 , and the stainless steel plate 73 by being pierced by the protruding members 74 .
[0160] In this state, the test piece was compressed until its bulk density (GBD) reached 0.3 g / cm 3 .
[0161] Next, if the stainless steel plate 73 is moved toward Fig. 9 , the stainless steel plate 73 is fixed to the test pieces 1a and 1b by the protrusion member 74, and therefore cannot be separated from the test pieces 1a and 1b and fall off. Therefore, when a shear force exceeding the shear failure load of the test pieces is applied to the test pieces 1a and 1b, the test pieces 1a and 1b are sheared and broken.
[0162] The shear force applied to the stainless steel plate when the test piece fails in shear was determined.
[0163] The shear failure load (kPa) can be obtained by dividing the obtained shear force by the area of the test piece. It should be noted that the shear failure load can also be measured using a test piece cut out of a part of the mat.
[0164] The relaxed surface pressure can be measured by the following procedure.
[0165] First, at room temperature, the mat was compressed to a bulk density of 0.3 g / cm 3 , measure the load after holding for 20 minutes.
[0166] The obtained load is divided by the area of the test piece to obtain the relaxed surface pressure (kPa). The relaxed surface pressure may be measured using a test piece obtained by cutting out a portion of the mat.
[0167] The back pressure of the mat material after firing is 50 kPa or more.
[0168] The fired back surface pressure of the mat material can be measured by the following method using a hot surface pressure measuring device equipped with a heater at a portion of a plate that compresses the mat material as a test piece.
[0169] First, the test piece (mat) was compressed at room temperature to a bulk density of 0.3 g / cm 3 Then, the test piece was heated at a rate of 45°C to 900°C on one side and 650°C on the other side under compression, and the compression was released until the bulk density reached 0.27 g / cm 3 Then, the plate that compresses the mat material is moved at a speed of 1 inch (25.4 mm) / min to a bulk density of 0.3 / cm 3 . Until the bulk density reaches 0.27g / cm 3The compression is released until the bulk density reaches 0.3 g / cm 3 After the compression was repeated 1000 times, the bulk density was measured to be 0.27 g / cm 3 The load obtained was divided by the area of the test piece to determine the surface pressure (kPa), which was taken as the surface pressure after firing.
[0170] The mat material may further include a protective sheet disposed on at least one surface.
[0171] The protection sheet is disposed on at least one surface of the pad.
[0172] If a protective sheet is provided on the surface of the mat, it is possible to suppress positional deviation and / or dense wrinkles of the mat when the mat is wound around the exhaust gas treating body, and generation of gaps in the fitting portion.
[0173] The material constituting the protective sheet is not particularly limited, but for example, a flexible resin such as polypropylene is preferred.
[0174] The protective sheet may be, for example, a nonwoven fabric composed of flexible resin fibers.
[0175] Furthermore, the protective sheet may be made of two or more different materials in combination.
[0176] The two or more materials may constitute the same nonwoven fabric, or two or more nonwoven fabrics of different types may be laminated to constitute the protective sheet.
[0177] The thickness of the protective sheet is not particularly limited, but is preferably 1 μm to 1 mm.
[0178] When the thickness of the protective sheet is less than 1 μm, the effect of alleviating pad deformation may be insufficient.
[0179] When the thickness of the protective sheet exceeds 1 mm, the handling properties may be reduced.
[0180] The ratio of the thickness of the protective sheet to the thickness of the pad is not particularly limited, but is preferably in the range of about 1:10 to about 1:1000, and more preferably in the range of about 1:50 to about 1:200.
[0181] The method of bonding the protective sheet and the mat is not particularly limited, and an example thereof includes a method of heating and melting hot-melt powder disposed between the protective sheet and the mat.
[0182] The surface on which the protective sheet is provided is preferably the surface that becomes the outer side when the mat is wound around the exhaust gas treating body.
[0183] The protection sheet may have slits formed therein.
[0184] The direction of the slits is not particularly limited, and they may be along the length direction or the width direction of the mat.
[0185] Fig.10 This is a perspective view schematically showing another example of the mat of the present invention.
[0186] Fig.10 The mat material 2 shown includes a mat 10 and a protective sheet 50 provided on one surface of the mat 10 .
[0187] The protective sheet may be provided on only one surface of the pad or on both surfaces.
[0188] [Exhaust gas purification device]
[0189] The exhaust gas purification device of the present invention comprises: an exhaust gas treatment body; a metal shell that accommodates the exhaust gas treatment body; and a mat material that is arranged between the exhaust gas treatment body and the metal shell to hold the exhaust gas treatment body. The exhaust gas purification device is characterized in that the mat material is the mat material of the present invention.
[0190] In the exhaust gas purifying device of the present invention, since the mat material of the present invention is disposed between the exhaust gas treating body and the metal casing, the exhaust gas treating body can be stably held.
[0191] Fig.11 This is a cross-sectional view schematically showing an example of the exhaust gas purification device of the present invention.
[0192] like Fig.11 As shown, the exhaust gas purification device 100 includes: a metal case 120; an exhaust gas treatment body 130 accommodated in the metal case 120; and a mat 1 disposed between the exhaust gas treatment body 130 and the metal case 120. The mat 1 is the mat of the present invention.
[0193] The exhaust gas treatment body 130 is a columnar exhaust gas treatment body having a plurality of channels 131 arranged side by side in the length direction through the channel wall 132. It should be noted that, at the end of the metal shell 120, an inlet pipe for introducing the exhaust gas discharged from the internal combustion engine and an exhaust pipe for discharging the exhaust gas passing through the exhaust gas purification device to the outside are connected as needed.
[0194] It should be noted that in Fig.11 In the exhaust gas purification device 100 shown, an exhaust gas filter (honeycomb filter) in which any one of the cells is sealed with a sealing material 133 is used as the exhaust gas treatment body 130, but a catalyst carrier in which any end surface is not sealed with a sealing material may also be used.
[0195] like Fig.11 As shown, the exhaust gas ( Fig.11130a, and flows through a channel 131 opened at the exhaust gas inlet side end face 130a of the exhaust gas treatment body (honeycomb filter) 130, and passes through the channel wall 132 separating the channel 131. At this time, PM in the exhaust gas is captured by the channel wall 132, and the exhaust gas is purified. The purified exhaust gas flows out from the other channels 131 opened at the exhaust gas outlet side end face 130b and is discharged to the outside.
[0196] [Making method of mat material]
[0197] The first embodiment of the method for manufacturing a mat material of the present invention is characterized in that it has an attaching step of attaching an inorganic binder to an inorganic fiber aggregate, wherein the inorganic fiber aggregate comprises inorganic fibers, and at least one of the surface or the back surface has a plurality of interlaced points formed by needle punching, and the density ρ of the interlaced points is 0.5 pieces / cm 2 ≤ρ<18 pieces / cm 2 In the range of 25mm×25mm, at least one of the first area and the second area is arranged in the area of 25mm×25mm, the first area is a 4mm×4mm area where the above-mentioned interweaving point does not exist, and the second area is a 3mm×8mm area where the above-mentioned interweaving point does not exist.
[0198] The inorganic fiber aggregate used in the first embodiment of the method for manufacturing a mat material of the present invention can be obtained, for example, through the following steps: a spinning step, spinning a spinning mixture containing at least an inorganic compound and an organic polymer to produce an inorganic fiber precursor; a compression step, compressing the above-mentioned inorganic fiber precursor to produce a sheet-like object; a needling step, needling at least one surface of the above-mentioned sheet-like object to produce a needling-treated body; and a firing step, firing the above-mentioned needling-treated body.
[0199] Hereinafter, specific examples of the spinning step, the compression step, the needling step, and the firing step will be described.
[0200] [Spinning process]
[0201] In the spinning step, a spinning mixture containing at least an inorganic compound and an organic polymer is spun to produce an inorganic fiber precursor.
[0202] In the spinning step, for example, a spinning mixture containing basic aluminum chloride aqueous solution and silica sol as raw materials is spun by a blowing method to produce an inorganic fiber precursor having an average fiber diameter of 3 μm to 10 μm.
[0203] [Compression process]
[0204] In the compression step, the inorganic fiber precursor obtained in the spinning step is compressed to produce a continuous sheet of a predetermined size.
[0205] [Acupuncture process]
[0206] In the needling step, at least one surface of the sheet-like object obtained in the compression step is subjected to needling treatment to produce a needling-treated body.
[0207] In the needling step, the needle arrangement density is preferably set to 0.5 needles / cm 2 More than and less than 18 / cm 2 .
[0208] The positions of the needles in the needling process correspond to the interlacing points in the mat material. Therefore, by setting the needle arrangement density to 0.5 needles / cm 2 More than and less than 18 / cm 2 , the density of interlacing points can be obtained by a single needle punching process at 0.5 / cm 2 ≤ρ<18 pieces / cm 2 range of cushion materials.
[0209] However, when the same sheet-like object is subjected to a plurality of needling treatments, the arrangement density of the needles is not limited to the above range.
[0210] In addition, the arrangement of the needles was intentionally made uneven during the needling process, so that the arrangement of the intertwining points formed on the needle-punched body was made sparse and dense, and the density of the intertwining points was set to 0.5 pieces / cm 2 ≤ρ<18 pieces / cm 2 range, and within the 25 mm×25 mm area, a 4 mm×4 mm area (first area) without an interlacing point and / or a 3 mm×8 mm area (second area) without an interlacing point can be formed.
[0211] As a method for intentionally making the arrangement of the interlacing points uneven, for example, the following method can be cited: after the interlacing points are evenly arranged, a part of the interlacing points are additionally subjected to acupuncture treatment. In addition, a method of performing acupuncture treatment multiple times while moving the inorganic fiber precursor, a method of performing acupuncture treatment using a needle plate with needles arranged at unequal intervals, etc. can also be cited.
[0212] In the needling step, the needle may or may not penetrate the sheet-like object in the thickness direction.
[0213] [Firing process]
[0214] In the firing step, the needle-punched body is fired to obtain an inorganic fiber aggregate composed of inorganic fibers.
[0215] The temperature for firing the needle-punched body is not particularly limited, but is preferably 1000°C to 1600°C.
[0216] [Attachment process]
[0217] In the attaching step, an inorganic binder is attached to the inorganic fiber aggregate.
[0218] As a method for attaching the inorganic binder to the inorganic fiber aggregate, for example, there is a method of bringing an inorganic binder mixed liquid obtained by mixing a solvent and an inorganic binder into contact with the inorganic fiber aggregate and then drying the mixed liquid.
[0219] Examples of methods for bringing the inorganic binder mixture into contact with the inorganic fiber aggregate include immersing the inorganic fiber aggregate in the inorganic binder mixture and dropping the inorganic binder mixture onto the inorganic fiber aggregate by curtain coating or the like.
[0220] By attaching an inorganic binder to the inorganic fiber aggregate, a mat constituting a mat material is obtained.
[0221] The content of the inorganic binder in the inorganic binder mixed liquid is preferably 0.05 wt % or more and 5 wt % or less.
[0222] The inorganic binder mixed liquid may contain a polymer dispersant.
[0223] If the inorganic binder mixed solution contains a polymer dispersant, the inorganic binder is dispersed in the inorganic binder mixed solution. By bringing the inorganic binder mixed solution in this state into contact with the inorganic fiber aggregate, the inorganic binder can be attached to the surface of the inorganic fiber in a dispersed state.
[0224] Examples of the polymer dispersant include hydrophilic synthetic polymer substances such as anionic polymer dispersants such as polycarboxylic acids and / or their salts, naphthalenesulfonate formaldehyde condensates and / or their salts, polyacrylic acid and / or their salts, polymethacrylic acid and / or their salts, polyvinylsulfonic acid and / or their salts, and nonionic polymer dispersants such as polyvinyl alcohol, polyvinyl pyrrolidone, and polyethylene glycol; natural hydrophilic polymer substances such as gelatin, casein, and water-soluble starch; and hydrophilic semi-synthetic polymer substances such as carboxymethyl cellulose.
[0225] Among them, hydrophilic synthetic polymer substances are preferred, and anionic polymer-based dispersants are more preferred.
[0226] In addition, these polymeric dispersants may be used alone or in combination of multiple types. In addition, a polymeric dispersant having a structure showing properties as an anionic polymeric dispersant and a structure showing properties as a nonionic polymeric dispersant may also be used.
[0227] The inorganic binder mixed liquid may contain a coagulant.
[0228] If the inorganic binder mixed liquid contains a coagulant, the inorganic binder is coagulated in the inorganic binder mixed liquid. By bringing the inorganic binder mixed liquid in this state into contact with the inorganic fiber aggregate, the inorganic binder can be attached to the surface of the inorganic fiber in a coagulated state.
[0229] The second embodiment of the method for manufacturing a mat material of the present invention is characterized in that it has an attaching step of attaching both an inorganic binder and an organic binder to an inorganic fiber aggregate, wherein the inorganic fiber aggregate comprises inorganic fibers, and at least one of the surface or the back surface has a plurality of interlacing points formed by needle punching, and the density ρ of the interlacing points is 0.5 pieces / cm 2 ≤ρ<18 pieces / cm 2 In the range of 25mm×25mm, at least one of the first area and the second area is arranged in the area of 25mm×25mm, the first area is a 4mm×4mm area where the above-mentioned interweaving point does not exist, and the second area is a 3mm×8mm area where the above-mentioned interweaving point does not exist.
[0230] The second embodiment of the method for producing a mat of the present invention is similar to the first embodiment of the method for producing a mat of the present invention, except that in the attaching step, not only the inorganic binder but also the organic binder is attached to the inorganic fiber aggregate.
[0231] Therefore, the step of adding both the inorganic binder and the organic binder to the inorganic fiber aggregate will be described below.
[0232] As a method of attaching both the inorganic binder and the organic binder to the inorganic fiber aggregate, there is a method of bringing a binder mixed liquid in which a solvent, an inorganic binder, and an organic binder are mixed into contact with the inorganic fiber aggregate and then drying the mixed liquid.
[0233] The content of the inorganic binder in the binder mixture is preferably 0.05 wt % or more and 5 wt % or less.
[0234] The content of the organic binder in the binder mixture is preferably 0.05 wt % or more and 5 wt % or less.
[0235] The binder mixed liquid may contain a polymer dispersant.
[0236] If the binder mixture contains a polymer dispersant, the inorganic binder and the organic binder are dispersed in the binder mixture. That is, the binder mixture becomes a dispersion in which the inorganic binder and the organic binder are dispersed in a dispersion medium. By bringing the binder mixture (dispersion) in this state into contact with the inorganic fiber aggregate, the inorganic binder and the organic binder can be attached to the surface of the inorganic fiber in a dispersed state.
[0237] The binder mixture may contain a coagulant.
[0238] If the mixed solution contains a coagulant, the inorganic binder and the organic binder are coagulated in the mixed solution. That is, the binder mixed solution becomes a coagulated dispersion solution in which the coagulates formed by the coagulation of the inorganic binder and the organic binder are dispersed in the dispersion medium. By bringing the binder mixed solution (coagulated dispersion solution) in this state into contact with the inorganic fiber aggregate, the inorganic binder and the organic binder can be attached to the surface of the inorganic fiber in a coagulated state.
[0239] The addition of the inorganic binder and the addition of the organic binder may be performed separately.
[0240] As a method for separately attaching an inorganic binder and an organic binder, for example, the following method can be cited: after an inorganic binder mixed liquid containing an inorganic binder is brought into contact with an inorganic fiber aggregate to attach the inorganic binder, the inorganic binder mixed liquid containing an organic binder is further brought into contact with the inorganic fiber aggregate to attach the organic binder. The order of attaching the inorganic binder and the organic binder is not particularly limited, and the inorganic binder may be attached first, or the organic binder may be attached first.
[0241] (Example)
[0242] The following are examples that more specifically disclose the present invention. However, the present invention is not limited to these examples.
[0243] (Example 1)
[0244] (a) Spinning process
[0245] In an alkaline aluminum chloride aqueous solution prepared in such a manner that the Al content is 70 g / l and Al:Cl=1:1.8 (atomic ratio), silica sol is mixed in such a manner that the composition ratio of the fired inorganic fibers is Al2O3:SiO2=72:28 (weight ratio), and an appropriate amount of an organic polymer (polyvinyl alcohol) is further added to prepare a mixed solution.
[0246] The obtained mixed solution was concentrated to prepare a spinning mixture, and the spinning mixture was spun by a blowing method to prepare an inorganic fiber precursor having an average fiber diameter of 5.1 μm.
[0247] (b) Compression process
[0248] The inorganic fiber precursor obtained in the spinning step (a) is compressed to produce a continuous sheet.
[0249] (c) Acupuncture process
[0250] The sheet-like material obtained in the compression step (b) is subjected to a needle punching treatment a plurality of times using a needle plate on which needles are provided at a predetermined density to produce a needle-punched body.
[0251] First, a needle plate with needles mounted at a predetermined density is prepared. Next, the needle plate is disposed above one surface of a sheet-like object, and a needle-punched body is produced by moving the needle plate up and down once in the thickness direction of the sheet-like object multiple times while moving the inorganic fiber precursor. At this time, the needles are penetrated until the barbs formed at the tip of the needles completely penetrate the surface on the opposite side of the sheet-like object.
[0252] (d) Firing process
[0253] The needle-punched body obtained in the above-mentioned needling step (c) was continuously fired at a maximum temperature of 1250°C to produce a fired sheet composed of inorganic fibers containing alumina and silica in a ratio of 72 parts by weight: 28 parts by weight. The average fiber diameter of the inorganic fibers was 5.1 μm, and the minimum fiber diameter was 3.2 μm. The bulk density of the fired sheet obtained in this way was 0.15 g / cm 3 , basis weight is 1400g / m 2 The density of interlacing points is 9 / cm 2 In the area of 25 mm×25 mm, there are arranged 10 areas of 4 mm×4 mm without interlacing points, namely the first area, and 4 areas of 3 mm×8 mm without interlacing points, namely the second area.
[0254] The fired needle-punched body is cut to produce an inorganic fiber aggregate.
[0255] (e) Attachment process
[0256] (e-1) Organic binder mixed solution preparation process
[0257] An acrylic emulsion as an organic binder was diluted with water to prepare an organic binder mixed liquid having a solid content concentration of 2.0 wt %.
[0258] (e-2) Inorganic binder mixed solution preparation process
[0259] Alumina as an inorganic binder was diluted with water, and a polymer dispersant was added and stirred sufficiently to prepare an inorganic binder mixed liquid having a solid content concentration of inorganic particles of 2.0 wt % and a concentration of the polymer dispersant of 1000 ppm.
[0260] (e-3) Binder Mixture Preparation Step
[0261] The organic binder mixture obtained in the above-mentioned (e-1) organic binder mixture preparation step is added to the inorganic binder mixture obtained in the above-mentioned (e-2) inorganic binder mixture preparation step in a manner to form a weight ratio of 1:1, and the mixture is fully stirred to prepare a binder mixture in which the organic binder has a solid content concentration of 1.0 wt%, the inorganic binder has a solid content concentration of 1.0 wt%, and the concentration of the above-mentioned polymer dispersant is 500 ppm.
[0262] (e-4) Contact process
[0263] The binder mixed solution obtained in the above-mentioned (e-3) binder mixed solution preparation step is brought into contact with the inorganic fiber aggregate obtained in the (d) calcination step by curtain coating.
[0264] (e-5) Dehydration process
[0265] The inorganic fiber aggregate to which the binder mixed solution was applied obtained in the contact step (e-4) was dehydrated by suction using a dehydrator, thereby preparing a mat in which 100 parts by weight of the binder mixed solution was applied to 100 parts by weight of the inorganic fibers.
[0266] (e-6) Drying process
[0267] The mat after the dehydration step (e-5) was dried in a dryer to produce the mat material of Example 1.
[0268] (Example 2)
[0269] A mat material of Example 2 was prepared in the same manner as in Example 1 except that the solid content concentration of the organic binder mixed solution prepared in the organic binder mixed solution preparation step (e-1) was changed to 0.2 wt %.
[0270] (Example 3)
[0271] Without carrying out the (e-1) organic binder mixture preparation step, in the (e-3) binder mixture preparation step, the inorganic binder mixture obtained in the (e-2) inorganic binder mixture preparation step is mixed and stirred with water in a weight ratio of 1:1, and the solid content concentration of the inorganic particles is adjusted to 1.0wt%. Except for this, the mat material of Example 3 is prepared according to the same steps as Example 1.
[0272] (Comparative Example 1)
[0273] Without carrying out the (e-2) inorganic binder mixture preparation step, in the (e-3) binder mixture preparation step, the organic binder mixture obtained in the (e-1) organic binder mixture preparation step and water having a polymer dispersant concentration of 500 ppm are mixed and stirred in a weight ratio of 1:1, and the solid content concentration of the organic binder is adjusted to 1.0 wt%. Except for this, the mat material of Comparative Example 1 is prepared according to the same steps as in Example 1.
[0274] (Measurement of back pressure after firing)
[0275] The back surface pressure after firing was measured for the mat materials of Examples 1 to 3 and Comparative Example 1. The method for measuring the back surface pressure after firing is as described in the description of the present invention. The results are shown in Table 1.
[0276] (Determination of shear coefficient)
[0277] The shear failure load and the relaxation surface pressure were measured for the mat materials of each embodiment and comparative example to obtain the shear coefficient. It should be noted that the method for measuring the shear failure strength and the method for measuring the relaxation surface pressure are as described in the description of the present invention. The results are shown in Table 1.
[0278] [Table 1]
[0279]
[0280] As shown in Table 1, it can be seen that the shear coefficient of the mat material of the present invention is as high as 0.20 or more.
[0281] The shear coefficient of the mat of Example 1 is about 132% of the shear coefficient of the mat of Comparative Example 1 which is a mat under the same conditions except that the inorganic binder is not included.
[0282] In addition, in the mats of Examples 1 to 3, the lower the weight ratio of the organic binder, the higher the shear coefficient, and the shear coefficient of Example 3 without an organic binder is the highest. On the other hand, the shear coefficient of the mat of Example 1 is also above 0.20, and the back pressure after firing is above 50 kPa. Therefore, it is believed that both the prevention of fiber scattering and the high holding force brought by the organic binder can be taken into account.
[0283] (Examples 4-5, Comparative Examples 2-3)
[0284] The mat materials of Examples 4 to 5 and Comparative Examples 2 to 3 were prepared in the same manner as in Example 1, except that the type of needle plate used in the needling process (c) and the number of needling treatments were changed, and the density of interlaced points and the number of first and second regions in the 25 mm×25 mm region were changed as shown in Table 2, and the back pressure and shear coefficient after firing were measured. The results are shown in Table 2.
[0285] (Comparative Example 4)
[0286] The mat material of Comparative Example 4 was prepared in the same manner as Comparative Example 1 except that the type of needle plate used in the needling process (c) and the number of needling treatments were changed, and the density of interlaced points and the number of first and second regions in the 25 mm×25 mm region were changed as shown in Table 2, and the back pressure and shear coefficient after firing were measured. The results are shown in Table 2.
[0287] [Table 2]
[0288]
[0289] As shown in Table 2, it can be seen that the mats of Examples 4 to 5 in which at least one of the first region and the second region is configured in an area of 25 mm×25 mm have higher back pressure after firing than the mats of Comparative Examples 2 to 4 in which neither the first region nor the second region is configured in an area of 25 mm×25 mm.
[0290] Explanation of symbols
[0291] 1.2 cushion material
[0292] 1a, 1b test piece
[0293] 10 pads
[0294] 11 convex part
[0295] 12 recesses
[0296] 15 interweaving points
[0297] 17 Area 1
[0298] 18 Area 2
[0299] 20Inorganic fiber
[0300] 30 coating layer
[0301] 40 Granular mixture
[0302] 50 protective film
[0303] 70 Shear failure load test device
[0304] 71 Left side fixture
[0305] 72 Right side clamp
[0306] 73 stainless steel plate
[0307] 74 protruding member
[0308] 100 Exhaust gas purification device
[0309] 120 metal shell
[0310] 130 Exhaust gas treatment body
[0311] 130a Exhaust gas inflow side end face
[0312] 130b Exhaust gas outflow side end surface
[0313] 131 Channel
[0314] 132 Channel wall
[0315] 133 Sealing material
Claims
1. A mat material comprising inorganic fibers and having a plurality of interlaced points formed by needle punching on at least one of the surface or the back surface, The mat material is characterized in that the density of the interlacing points is 0.5 / cm 2 ≤ρ<18 pieces / cm 2 , and at least one of the first area and the second area is arranged in the area of 25 mm×25 mm, the first area is a 4 mm×4 mm area where the interlacing point does not exist, and the second area is a 3 mm×8 mm area where the interlacing point does not exist, The mat material contains an inorganic binder, has a shear coefficient of more than 0.20, and a rear pressure of more than 50 kPa after firing.
2. The mat material according to claim 1, wherein: The weight ratio of the inorganic binder to the mat material, that is, the weight of the inorganic binder / the weight of the mat material, exceeds 0 wt % and is 10 wt % or less.
3. The mat material according to claim 1 or 2, further comprising an organic binder.
4. The mat material according to claim 3, wherein: The weight ratio of the organic binder to the mat material, that is, the weight of the organic binder / the weight of the mat material, exceeds 0 wt % and is 10 wt % or less.
5. The mat material according to claim 3 or 4, wherein: The inorganic binder and the organic binder are attached to the surface of the inorganic fiber in a dispersed state. 6 . The mat material according to claim 1 , further comprising a polymer dispersant.
7. The mat material according to claim 3 or 4, wherein: Aggregates composed of the inorganic binder and the organic binder are attached to the surfaces of the inorganic fibers.
8. The mat material according to claim 7, wherein: The coating layer composed of a mixture of the inorganic binder and the organic binder covers at least a portion of the surface of the inorganic fiber.
9. The mat material according to claim 8, wherein: The coating layer is formed by a continuous scaly mixture of the inorganic binder and the organic binder.
10. The mat material according to claim 8 or 9, wherein: The coating layer has a multi-step shape.
11. The mat material according to any one of claims 8 to 10, wherein A particle-shaped mixture of the inorganic binder and the organic binder adheres to the surface of the coating layer.
12. The mat material according to any one of claims 1 to 11, wherein The shear coefficient is 105% or more of the shear coefficient of a mat material under the same conditions except that the inorganic binder is not contained.
13. The mat material according to any one of claims 1 to 12, wherein A plurality of the first regions and / or the second regions are arranged in an area of 25 mm×25 mm.
14. The mat material according to any one of claims 1 to 13, which is used in an exhaust gas purification device. 15 . The mat material according to claim 1 , further comprising a protective sheet provided on at least one surface.
16. An exhaust gas purification device, comprising: Exhaust gas treatment body; A metal housing that contains the exhaust gas treatment body; A mat material is disposed between the exhaust gas treatment body and the metal shell to hold the exhaust gas treatment body. The exhaust gas purification device is characterized in that The mat material is the mat material according to any one of claims 1 to 15.
17. A method for manufacturing a mat material, characterized in that: The method comprises the step of attaching an inorganic binder to an inorganic fiber aggregate, wherein the inorganic fiber aggregate comprises inorganic fibers, and at least one of the surface or the back surface has a plurality of interlaced points formed by needle punching, and the density of the interlaced points is 0.5 / cm 2 ≤ρ<18 pieces / cm 2 In the range of 25 mm×25 mm, at least one of the first area and the second area is configured, the first area is a 4 mm×4 mm area where the interweaving point does not exist, and the second area is a 3 mm×8 mm area where the interweaving point does not exist.
18. A method for manufacturing a mat material, characterized in that: The method comprises the step of attaching both an inorganic binder and an organic binder to an inorganic fiber aggregate, wherein the inorganic fiber aggregate comprises inorganic fibers, and at least one of the surface or the back surface has a plurality of interlaced points formed by needle punching, and the density of the interlaced points is 0.5 / cm 2 ≤ρ<18 pieces / cm 2 In the range of 25 mm×25 mm, at least one of the first area and the second area is configured, the first area is a 4 mm×4 mm area where the interweaving point does not exist, and the second area is a 3 mm×8 mm area where the interweaving point does not exist.
19. The method for manufacturing a mat material according to claim 18, wherein: In the attaching step, a dispersion in which the inorganic binder and the organic binder are dispersed in a dispersion medium is attached to the inorganic fiber aggregate.
20. The method for manufacturing a mat material according to claim 18, wherein: In the attaching step, an aggregated dispersion liquid in which the inorganic binder and the organic binder are aggregated is attached to the inorganic fiber aggregate.
Citation Information
Patent Citations
Mat, method for manufacturing the mat, and apparatus for purifying exhaust gas
CN102207018A
Mat, holding sealing material, method for producing mat, and exhaust gas purifying apparatus
CN102444452A
Inorganic fiber formed article, mat for exhaust gas cleaning device, and exhaust gas cleaning device
CN107429455A
Catalytic converter
JP2001065337A
Inorganic fiber having carbon particles buried thereon, method for producing the same, assembly of inorganic fibers having carbon particles buried thereon, and exhaust purifying device
JP2016060969A