Identifying media and article
By adjusting the adhesive force relationship in the identification medium and using a resin layer with cholesteric regularity, the problems of high cost and difficulty in preventing reuse of the identification medium in the existing technology are solved, and authenticity determination without a special observer is achieved. and prevent reuse.
Patent Information
- Application Number
- CN202380024339.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-15
AI Technical Summary
Existing identification media require the use of a special observer when determining authenticity, which is costly and difficult for ordinary users to obtain. Furthermore, identification media attached to transparent items are difficult to prevent from being reused.
An identification medium containing a first layer and a second layer is designed. By adjusting the adhesive force relationship, the first layer and the second layer are separated when peeled off, thereby losing the optical function, preventing reuse, and passing through the cholesteric The regular resin layer achieves specific reflection and transmission effects of circularly polarized light, allowing the naked eye to determine authenticity.
It is possible to determine the authenticity of items without using a special observer, and prevents the reuse of identification media, reducing costs and simplifying the determination process.
Smart Images

Figure CN118786371A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to identification media and articles. Background Art
[0002] In order to determine whether an article is a genuine article provided by a legitimate manufacturer, an identification medium that cannot be easily copied is usually provided on the article. As such an identification medium, an identification medium using a material having a circularly polarized light separation function is known.
[0003] The material having the circularly polarized light separation function has the function of transmitting one of right-handed circularly polarized light and left-handed circularly polarized light and reflecting part or all of the other. When observing the identification medium using such a material through a right-handed circular polarizer and when observing the identification medium using such a material through a left-handed circular polarizer, different images will appear. Therefore, in determining the authenticity of an article provided with such an identification medium, an observer having two circular polarizers, a right-handed circular polarizer and a left-handed circular polarizer, is usually used.
[0004] Since the authenticity determination of the existing identification medium requires a viewer with two circular polarizers as described above, the cost is high. In addition, it is not easy for ordinary users to obtain a viewer, so it is not easy to implement the authenticity determination. The implementation of the authenticity determination is limited to genuine manufacturers, some retail stores, public institutions, etc. Therefore, an identification medium that can implement the authenticity determination even without using the special viewer as described above is required.
[0005] In response to this, the inventors have developed an identification medium comprising: a first layer that can reflect one of the circularly polarized lights and allow the other circularly polarized lights to pass through; and a second layer that is arranged to overlap with the first layer and can reflect circularly polarized light with the same rotation direction as the circularly polarized light reflected by the first layer and allow the circularly polarized light with the opposite rotation direction to the circularly polarized light reflected by the first layer to pass through. By making the reflectivity of the first layer and the reflectivity of the second layer satisfy a specified relationship, the authenticity can be determined by naked eye observation (Patent Document 1).
[0006] Furthermore, although Patent Document 2 does not relate to the invention of an identification medium including the first layer and the second layer, it describes an identification medium to which a reuse prevention function is imparted regarding an identification medium for authenticity identification.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent document 1: International Publication No. 2020 / 004155 (corresponding publication: U.S. Patent Application Publication No. 2021 / 300105);
[0010] Patent Document 2: Japanese Patent No. 6180095 (corresponding publication: specification of U.S. Patent Application Publication No. 2015 / 323898). Summary of the invention
[0011] Problem that the invention aims to solve
[0012] Although the identification medium including the first layer and the second layer is translucent and can be seen through one side from the other side, it is expected to be used as an identification medium to be attached to a transparent adherend such as glass because the second layer can be observed only from the second layer side, but cannot be observed from the side opposite to the second layer side (the first layer side). In the identification medium to be attached to the adherend for use, a function is strongly required to prevent the identification medium once attached to the adherend from being peeled off and reused.
[0013] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide an identification medium that can determine authenticity and prevent reuse without using a special viewer, and an article including the same.
[0014] Solutions for solving problems
[0015] The inventors have conducted in-depth research on the above-mentioned problem and found that when the adhesive layer, the second layer and the first layer of the identification medium are sequentially stacked and attached to the adherend, the adhesive force F1 between the first layer and the second layer is smaller than the adhesive force F2 between the second layer and the adhesive layer, and the adhesive force F1 between the first layer and the second layer is smaller than the adhesive force F3 between the adhesive layer and the adherend, so that when the identification medium is peeled off from the adherend, the first layer and the second layer can be separated, the optical function of the identification medium disappears and reuse can be prevented, thereby completing the present invention. The present invention includes the following contents.
[0016] [1] An identification medium comprising: a first layer; a second layer arranged overlapping the first layer; and an adhesive layer arranged on the second layer; the first layer is a layer capable of reflecting one of right-handed circularly polarized light or left-handed circularly polarized light and allowing the other circularly polarized light to pass through, the first layer comprises a layer of a resin having cholesteric regularity, the second layer is a layer capable of reflecting at least a portion of circularly polarized light having the same rotation direction as the circularly polarized light reflected by the first layer and allowing the circularly polarized light having the opposite rotation direction to the circularly polarized light reflected by the first layer to pass through, the second layer is a layer of a thin sheet of a resin having cholesteric regularity, and when the adhesive layer is adhered to an adherend, the adhesive force F1 between the first layer and the second layer, the adhesive force F2 between the second layer and the adhesive layer, and the adhesive force F3 between the adhesive layer and the adherend satisfy the relationship between the following equations (1) and (2).
[0017] F1<F2(1)
[0018] F1<F3(2)
[0019] [2] The identification medium according to [1], wherein a tension T1 that deforms the adhesive layer and an adhesive force F3 between the adhesive layer and the adherend satisfy the relationship of the following formula (3).
[0020] T 1<F 3(3)
[0021] [3] An identification medium according to [1] or [2], wherein the second layer is a layer provided on a portion of the surface of the first layer, and the adhesive layer is a layer provided on the first layer and the second layer, and when the adhesive layer is adhered to an adherend, the adhesive force F3 between the adhesive layer and the adherend, and the adhesive force F4 between the first layer and the adhesive layer satisfy the relationship of the following formula (4).
[0022] F 4<F 3(4)
[0023] [4] An identification medium according to any one of [1] to [3], wherein the identification medium includes a third layer, the third layer is arranged on the surface of the first layer opposite to the surface on which the second layer is arranged, overlapping with the first layer, the third layer is a layer capable of transmitting circularly polarized light with a rotation direction opposite to that of the circularly polarized light reflected by the first layer, and the third layer is a layer comprising a thin sheet of a resin having cholesteric regularity.
[0024] [5] The identification medium according to any one of [1] to [4], wherein the volume average particle size (D50) of the flakes of the resin having cholesteric regularity is 70 μm or more.
[0025] [6] The identification medium according to any one of [1] to [5], wherein the first layer is a laminate of a layer of the resin having cholesteric regularity and a layer containing a norbornene-based resin.
[0026] [7] The identification medium according to any one of [1] to [6], wherein the adherend is transparent glass.
[0027] [8] The identification medium according to any one of [1] to [7], wherein when the identification medium is peeled off after being attached to the adherend, the laminated portion of the second layer and the adhesive layer is separated from the first layer.
[0028] [9] The identification medium according to [8], wherein when the adhesive layer of the laminated portion separated from the identification medium is peeled off from the adherend, the adhesive layer is deformed and the second layer is destroyed.
[0029]
[10] An article comprising the identification medium according to any one of [1] to [9] and an adherend to which the identification medium is adhered.
[0030] Effects of the Invention
[0031] According to the present invention, it is possible to provide an identification medium that can determine authenticity and prevent reuse without using a special viewer having a right-handed circular polarizing plate and a left-handed circular polarizing plate, and an article including the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a top view schematically showing the identification medium according to the first embodiment of the present invention.
[0033] Figure 2 To schematically illustrate Figure 1 A cross-sectional view of the cross section taken along the X1-X1 direction.
[0034] Figure 3 To schematically illustrate Figure 2 An exploded cross-sectional view of the adhesion between the layers of the identification medium is shown.
[0035] Figure 4 An exploded cross-sectional view schematically showing the optical path when light is irradiated from the second layer side of the identification medium.
[0036] Figure 5 The figure is an exploded cross-sectional view schematically showing the optical path when light is irradiated from the first layer side of the identification medium.
[0037] Figure 6 The figure is a perspective view schematically showing a sheet and the light path irradiating the sheet.
[0038] Figure 7 This is an exploded perspective view schematically showing an identification medium according to Embodiment 2 of the present invention.
[0039] Figure 8 For viewing from the second floor Figure 7 Schematic top view of the identification medium.
[0040] Fig. 9 For viewing from the third floor Figure 7 Schematic top view of the identification medium.
[0041] Fig.10 To schematically illustrate Figure 8 and Fig. 9 A cross-sectional view of the cross section taken along the X2-X2 direction.
[0042] Fig.11 An exploded cross-sectional view schematically showing the optical path when light is irradiated from the second layer side of the identification medium.
[0043] Fig.12 The figure is an exploded cross-sectional view schematically showing the optical path when light is irradiated from the third layer side of the identification medium.
[0044] Fig.13 It is a cross-sectional view schematically showing a method of measuring the adhesive force F1 between the first layer and the second layer in the example.
[0045] Fig.14 It is a cross-sectional view schematically showing a method for measuring the adhesive force F2 between the second layer and the adhesive layer in the example.
[0046] Fig.15 It is a cross-sectional view schematically showing a method for measuring the adhesive force F3 between the adhesive layer and the adherend in the example.
[0047] Fig.16 It is a cross-sectional view schematically showing a method for measuring the adhesive force F4 between the first layer and the adhesive layer in the example.
[0048] Fig.17 This is a cross-sectional view schematically showing a method of measuring the tension T1 for deforming the adhesive layer of the example.
[0049] Fig.18 This is a side view schematically showing a release sheet manufacturing apparatus used when manufacturing a release sheet (sheet) for a cholesteric resin layer in Examples. DETAILED DESCRIPTION
[0050] The present invention will be described in detail below by showing embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and can be arbitrarily modified within the scope of the claims of the present invention and their equivalents.
[0051] In the following description, unless otherwise specified, "pattern" refers to a planar pattern shape, and the pattern includes, for example, letters, numbers, and figures.
[0052] In the following description, the “visible light region” refers to a wavelength range of 400 nm to 780 nm.
[0053] In addition, in the following description, the in-plane delay of the film or layer shows a value represented by (nx-ny)×d. In addition, the delay in the thickness direction of the film or layer shows a value represented by {(nx+ny) / 2-nz}×d. Here, nx represents the refractive index of the direction of the maximum refractive index in the direction perpendicular to the thickness direction of the film or layer (in-plane direction). In addition, ny represents the refractive index in the direction orthogonal to the direction of nx in the above-mentioned in-plane direction of the film or layer. Furthermore, nz represents the refractive index in the thickness direction of the film or layer. In addition, d represents the thickness of the film or layer. These delays can be measured at a wavelength of 560nm using a commercially available phase difference measuring device (e.g., "WPA-micro" manufactured by Photonic Lattice Co., Ltd.) or the Sennamon method.
[0054] In addition, in the following description, "(meth)acrylic acid" includes acrylic acid, methacrylic acid and combinations thereof. In addition, "(meth)acrylate" includes acrylate, methacrylate and combinations thereof. In addition, "(thio)epoxy" includes epoxy, thioepoxy and combinations thereof. In addition, "iso(thio)cyanate" includes isocyanate, isothiocyanate and combinations thereof.
[0055] In the following description, unless otherwise specified, adhesives are distinguished from each other by the shear modulus. Specifically, unless otherwise specified, an adhesive refers to a material having a shear modulus of 1 MPa to 500 MPa at 23°C after energy ray irradiation or heat treatment. In addition, unless otherwise specified, an adhesive refers to a material having a shear modulus of less than 1 MPa at 23°C.
[0056] [Identification medium]
[0057] [1. Implementation Method 1]
[0058] Below, refer to Figure 1 to Figure 5 The identification medium according to the first embodiment of the present invention will be described.
[0059] Figure 1 It is a top view schematically showing the identification medium according to the first embodiment of the present invention. Figure 2 To schematically illustrate Figure 1 A cross-sectional view of the cross section taken along the X1-X1 direction. Figure 3 To schematically illustrate Figure 2 An exploded cross-sectional view of the adhesion between the layers of the identification medium is shown. Figure 4 An exploded cross-sectional view schematically showing the optical path when light is irradiated from the second layer side of the identification medium. Figure 5 The figure is an exploded cross-sectional view schematically showing the optical path when light is irradiated from the first layer side of the identification medium.
[0060] like Figure 1 to Figure 3 As shown, an identification medium 10 according to one embodiment of the present invention comprises: a first layer 11; a second layer 12, which is provided overlapping with the first layer 11, and an adhesive layer 14, which is provided on the second layer 12. In the present invention, "overlapping" of a certain layer with another certain layer means that when their planar positional relationship is observed from the thickness direction of the identification medium, at least a part of them is in the same planar position.
[0061] The adhesive layer 14 is generally a layer disposed directly (i.e., in contact with) the second layer 12. Figure 1 to Figure 3 As shown, in the case where the second layer 12 is a layer provided on a portion of the surface of the first layer 11, the adhesive layer 14 is a layer provided on the first layer 11 and the second layer 12. In this case, the adhesive layer 14 is generally a layer provided directly (i.e., in a contacting state) on the first layer 11 and the second layer 12, respectively. Hereinafter, in order to distinguish the adhesive layer 14 provided at least on the second layer 12 from the adhesive layers provided at other positions, it is also referred to as "adhesive layer (A)".
[0062] The first layer 11 is a layer capable of reflecting one of right-handed circularly polarized light or left-handed circularly polarized light and allowing the other circularly polarized light to pass through. In addition, the first layer 11 includes a layer 11a of a resin having cholesteric regularity. The first layer 11 can be a layer comprising the layer 11a of a resin having cholesteric regularity and, as required, a layer 11b of a norbornene-based resin and an adhesive layer 11c (or bonding layer). The second layer 12 is a layer capable of reflecting at least a portion of circularly polarized light having the same rotation direction as the circularly polarized light reflected by the first layer 11 and allowing the circularly polarized light having the opposite rotation direction to the circularly polarized light reflected by the first layer 11 to pass through. In addition, the second layer 12 is a layer comprising a thin sheet 12f of a resin having cholesteric regularity. In Figure 1 In the figure, the second layer 12 is a portion of the letter pattern ABCD formed directly on the layer 11b of the first layer 11. The second layer 12 is formed at a position where the entire area thereof completely overlaps with the first layer 11.
[0063] Figure 2 Since it is a schematic diagram, the cross-sectional shape of the second layer 12 is shown as a schematic shape. Specifically, as the second layer 12, the plane shape of the character pattern and the schematic cross-sectional shape of a layer having a certain thickness are shown.
[0064] The identification medium 10 may include a protective layer 16 provided via an adhesive layer 15 (or a bonding layer) on the surface of the first layer 11 opposite to the surface on which the second layer 12 is provided, as necessary.
[0065] Regarding the identification medium 10, when the adhesive layer (A) 14 is adhered to the adherend 20, the adhesive force F1 between the layer 11b in the first layer 11 and the second layer 12, the adhesive force F2 between the second layer 12 and the adhesive layer (A) 14, and the adhesive force F3 between the adhesive layer (A) 14 and the adherend 20 satisfy the relationship between the following equations (1) and (2).
[0066] F1<F2(1)
[0067] F1<F3(2)
[0068] Furthermore, regarding the identification medium 10, when an adhesive layer (A) 14 is provided on layer 11b of the first layer 11, the adhesive force F3 between the adhesive layer (A) 14 and the adherend 20, and the adhesive force F4 between layer 11b of the first layer and the adhesive layer (A) 14 satisfy the relationship of the following formula (4).
[0069] F 4<F 3(4)
[0070] According to this embodiment, when the identification medium is attached to an adherend, the adhesion between the layers of the identification medium and the adhesion F3 between the adhesive layer (A) and the adherend satisfy a prescribed relationship, so that when the identification medium is peeled off after being attached to the adherend, the identification medium can be separated between the first layer and the second layer. In other words, the identification medium of this embodiment can be a structure in which the laminated portion of the second layer and the adhesive layer is separated from the first layer when the identification medium is peeled off after being attached to the adherend.
[0071] The identification medium of this embodiment has an optical function by having a structure in which the first layer and the second layer are stacked, and the authenticity can be determined by utilizing this function even without using a special observer. Therefore, when the first layer and the second layer are separated, the optical function is lost, and the function as the identification medium disappears, so it is possible to prevent the reuse of the identification medium peeled off from the adherend.
[0072] The optical function of the identification medium according to the present embodiment will be described using the drawings.
[0073] Figure 41 is a schematic exploded cross-sectional view showing the optical path when light is irradiated from the second layer 12 side of the identification medium. Figure 5 FIG. 1 is an exploded cross-sectional view schematically showing the optical path when light is irradiated from the first layer 11 side of the identification medium. Figure 4 and Figure 5 In the embodiment, the following case is used as an example: the first layer 11 is a layer capable of reflecting right-handed circularly polarized light and allowing left-handed circularly polarized light to pass through, and the second layer 12 is a layer capable of reflecting at least a portion of right-handed circularly polarized light and allowing left-handed circularly polarized light to pass through, that is, a layer that does not reflect, or hardly reflects, left-handed circularly polarized light.
[0074] like Figure 4 As shown, when non-polarized light A1 such as natural light is irradiated from the second layer 12 side of the identification medium, at least a portion of right-handed circularly polarized light A1R in the non-polarized light A1 is reflected by the thin sheets of the second layer 12. The thin sheets included in the second layer 12 are generally dispersed in the layer in different directions, so the circularly polarized light A1R is observed as backscattered light A2R. On the other hand, left-handed circularly polarized light A1L in the non-polarized light A1 passes through the second layer 12, and the left-handed circularly polarized light A1L that has passed through the second layer 12 passes through the first layer 11.
[0075] When non-polarized light A1 is irradiated from the second layer 12 side toward the first layer 11 where the second layer 12 is not provided, right circularly polarized light A1R in the non-polarized light A1 is specularly reflected by the first layer 11 to become reflected light A3R. On the other hand, left circularly polarized light A1L in the non-polarized light A1 passes through the first layer 11.
[0076] Next, if Figure 5 As shown, when the non-polarized light A1 is irradiated from the first layer 11 side, the right circularly polarized light A1R in the non-polarized light A1 is specularly reflected by the first layer 11 to become the reflected light A3R. On the other hand, the left circularly polarized light A1L in the non-polarized light A1 passes through the first layer 11. Furthermore, in the region where the second layer 12 is provided on the first layer 11, the left circularly polarized light A1L that has passed through the first layer 11 passes through the second layer 12.
[0077] Therefore, when the identification medium is observed from the second layer 12 side, the backscattered light A2R is observed in the area of the identification medium where the second layer 12 is provided, and the reflected light A3R from the specular reflection of the first layer 11 is observed in the area where the second layer 12 is not provided, by the non-polarized light A1 irradiated from the second layer 12 side, so the observer can see the information of the second layer 12 based on the difference between the backscattered light A2R and the reflected light A3R. In addition, when the non-polarized light A1 is irradiated from the first layer 11 side, in the identification medium, the same degree of left-handed circularly polarized light A1L is transmitted in the area where the second layer 12 is provided and the area where the second layer 12 is not provided. Therefore, when the identification medium is observed from the second layer side, the transmitted light A1L from the first layer side can be made not to affect the visibility of the information of the second layer 12, or even if it has an effect, it can be made to be very small.
[0078] On the other hand, when the identification medium is observed from the first layer 11 side, the reflected light A3R is observed on the entire surface of the first layer 11 by irradiating the non-polarized light A1 from the first layer 11 side. Furthermore, when the non-polarized light A1 is irradiated from the second layer 12 side, in the identification medium, the same degree of left-handed circularly polarized light A1L is transmitted in the region where the second layer 12 is provided and the region where the second layer 12 is not provided. Therefore, when the identification medium is observed from the first layer 11 side, the reflected light A3R from the first layer 11 and the transmitted light A1L from the second layer 12 side can be observed on the entire surface of the first layer 11 to the same degree regardless of the region where the second layer 12 is provided or the region where the second layer 12 is not provided, so that the information of the second layer 12 can be prevented from being observed.
[0079] As described above, the identification medium of this embodiment can identify the difference in visibility between the front and back sides when the structure in which the first layer and the second layer are stacked is observed from the front and back sides of the identification medium. Therefore, each of the first layer and the second layer does not produce a difference in visibility between the front and back sides, and loses the identification function, thereby preventing the reuse of the identification medium.
[0080] [1.1. Relationship of Adhesion]
[0081] Regarding the identification medium of this embodiment, when the adhesive layer (A) is attached to an adherend, the adhesive force F1 between the first layer and the second layer and the adhesive force F2 between the second layer and the adhesive layer satisfy the relationship of the following formula (1).
[0082] F1<F2(1)
[0083] In the present embodiment, when the first layer includes a plurality of layers, the "adhesive force F1 between the first layer and the second layer" refers to the adhesive force between the layer of the first layer on which the second layer is directly provided and the second layer.
[0084] The difference (F2-F1) between the adhesive force F2 and the adhesive force F1 is usually greater than 0 N / 10 mm, preferably 1 N / 10 mm or more, more preferably 2 N / 10 mm or more, preferably 5 N / 10 mm or less, more preferably 4.5 N / 10 mm or less.
[0085] In the identification medium of this embodiment, when the adhesive layer (A) is attached to an adherend, the adhesive force F1 between the first layer and the second layer and the adhesive force F3 between the adhesive layer (A) and the adherend satisfy the relationship of the following formula (2).
[0086] F1<F3(2)
[0087] The difference (F3-F1) between the adhesive force F3 and the adhesive force F1 is usually greater than 0 N / 10 mm, preferably 1 N / 10 mm or more, more preferably 2 N / 10 mm or more, preferably 7 N / 10 mm or less, more preferably 6.5 N / 10 mm or less.
[0088] The adhesive force F2 between the second layer and the adhesive layer (A), and the adhesive force F3 between the adhesive layer (A) and the adherend can be, for example, any one of the following: the adhesive force F2 is greater than the adhesive force F3 (F2>F3), the adhesive force F3 is greater than the adhesive force F2 (F2<F3), and the adhesive force F2 and the adhesive force F3 are of the same magnitude (F2=F3).
[0089] When the identification medium has an adhesive layer (A) on the first layer, the adhesive force F3 between the adhesive layer (A) and the adherend and the adhesive force F4 between the first layer and the adhesive layer (A) satisfy the relationship of the following formula (4).
[0090] F 4<F 3(4)
[0091] In the present embodiment, when the first layer includes a plurality of layers, "adhesion force F4 between the first layer and the adhesive layer (A)" refers to the adhesion force between the layer on which the adhesive layer (A) is directly provided in the first layer and the adhesive layer (A).
[0092] The difference (F3-F4) between the adhesive force F3 and the adhesive force F4 is usually greater than 0 N / 10 mm, preferably 1 N / 10 mm or more, more preferably 2 N / 10 mm or more, preferably 6 N / 10 mm or less, more preferably 5.5 N / 10 mm or less.
[0093] The adhesive force F1 between the first layer and the second layer and the adhesive force F4 between the first layer and the adhesive layer (A) can be any one of the case where the adhesive force F1 is greater than the adhesive force F4 (F1 > F4), the case where the adhesive force F4 is greater than the adhesive force F1 (F1 < F4), and the case where the adhesive force F1 and the adhesive force F4 have the same magnitude (F1 = F4). In the present embodiment, it is more preferable that the absolute value of the difference between the adhesive force F1 and the adhesive force F4 is small or there is no difference. This is because it can make the separability between the first layer and the second layer and between the first layer and the adhesive layer (A) good. The absolute value of the difference between the adhesive force F1 and the adhesive force F4 (|F2 - F1|) is preferably 1 N / 10 mm or less, more preferably 0.8 N / 10 mm or less, preferably 0 N / 10 mm, and can be 0.1 N / 10 mm or more.
[0094] Regarding the specific magnitudes of the respective adhesive forces F1 to F4, there is no particular limitation, and the magnitudes of the adhesive forces F1 to F4 are each preferably in the range of, for example, 1 N / 10 mm or more and 20 N / 10 mm or less.
[0095] In the identification medium of the present embodiment, when the identification medium is pasted to the adherend, the adhesive forces between the respective layers on the side of the first layer where the second layer is provided and the adhesive force between the adhesive layer (A) and the adherend Figure 3 among the adhesive forces F1 to F4) are each less than the adhesive forces between the respective layers on the side of the first layer opposite to the side where the second layer is provided Figure 3 among the adhesive forces F5 and F6). In addition, when the first layer includes a plurality of layers, the adhesive forces between the respective layers on the side of the first layer where the second layer is provided and the adhesive force between the adhesive layer (A) and the adherend Figure 3 among the adhesive forces F1 to F4) are each less than the adhesive forces between the respective layers of each first layer Figure 3 among the adhesive forces F7 and F8). This is because, by making the adhesive forces F1 to F8 of the respective layers constituting the identification medium have the above relationship, when the identification medium is peeled off after being pasted to the adherend, the first layer and the second layer can be easily separated.
[0096] The adhesive forces between the respective layers of the identification medium and the adhesive force between the adhesive layer (A) and the adherend can be measured by a 90-degree peel test using the following dynamometer.
[0097] Prepare a sample of the identification medium cut into a width of 10 mm, and after attaching the sample to the adherend, sandwich the laminated portion (in the case of the layer on the surface, it is a single layer) from the layer on the opposite side of the adhesive layer to the layer on the surface between the layers to be measured at the front end of a dynamometer (e.g., "Standard Digital Dynamometer ZTS-100N" manufactured by IMONDA Co., Ltd.), pull the laminated portion (or single layer) at a speed of 300 mm / min along the normal direction of the surface of the adherend, and measure the magnitude of the pulling force generated when peeling off as the adhesive force. The measurement can be carried out under conditions such as a temperature of 22°C ± 10°C and a humidity of 50% ± 20%.
[0098] When it is difficult to sandwich the layers of the identification medium with the tip of the force gauge, the adhesive strength can be measured by preparing an evaluation sample using the same constituent material as the two layers located between the layers to be measured and subjecting the evaluation sample to the above-mentioned 90-degree peel test.
[0099] There is no particular restriction on the specific size of the bonding force between each layer of the identification medium and the bonding force between the adhesive layer (A) and the adherend, and it can be adjusted by selecting the materials used in each layer. In the selection of materials, it is preferred to measure the bonding force in advance by the above-mentioned 90 degree peel test and select the material according to the result.
[0100] [1.2. Tension of adhesive layer (A)]
[0101] The identification medium of the present embodiment preferably has a tension T1 that deforms the adhesive layer (A) and an adhesive force F3 between the adhesive layer and the adherend that satisfies the relationship of the following formula (3).
[0102] T 1<F 3(3)
[0103] By making the tension T1 and the adhesive force F3 in the above relationship, when the identification medium is peeled off after being attached to the adherend, when the laminated portion of the second layer separated from the identification medium and the adhesive layer (A) is peeled off from the adherend, the second layer transferred to the adhesive layer (A) cannot be deformed in accordance with the deformation of the adhesive layer and is destroyed because the adhesive layer (A) is soft and easily stretched, thereby further preventing the identification medium from being reused. In other words, the identification medium of this embodiment can be configured such that when the adhesive layer of the laminated portion separated from the identification medium is peeled off from the adherend, the adhesive layer is deformed and the second layer is destroyed.
[0104] The difference between the adhesive force F3 and the tension T1 is usually greater than 0 N / 10 mm, preferably 1 N / 10 mm or more, more preferably 2 N / 10 mm or more, and preferably 5 N / 10 mm or less, more preferably 4.5 N / 10 mm or less.
[0105] The magnitude of the tension T1 is, for example, not less than 1 N / 10 mm and not more than 20 N / 10 mm.
[0106] The tension T1 for deforming the adhesive layer (A) can be measured by a 90-degree peel test using the following dynamometer.
[0107] A 10 mm wide adhesive layer sheet consisting of an adhesive layer (adhesive) for an adhesive layer (A) is prepared, and after being pasted to an adherend with a gap portion at a certain distance from one end of the adhesive layer sheet, the gap portion is sandwiched between the front end of a dynamometer (e.g., "Standard Digital Dynamometer ZTS-100N" manufactured by IMONDA Co., Ltd.), and the adhesive layer is pulled along the normal direction of the surface of the adherend at a speed of 300 mm / min, and the pulling force when the gap portion begins to stretch is measured as the tension. The measurement can be carried out, for example, at a temperature of 22°C ± 10°C and a humidity of 50% ± 20%.
[0108] When selecting the material of the adhesive layer (A), it is preferred to measure the tension in advance by the above-mentioned 90-degree peel test and select the material based on the result.
[0109] [1.3. Identification of the constituent layers of the medium]
[0110] The identification medium of this embodiment includes a first layer, a second layer, and an adhesive layer (A).
[0111] [1.3.1. First layer]
[0112] The first layer is a layer capable of reflecting one of right-handed circularly polarized light or left-handed circularly polarized light and transmitting the other circularly polarized light. The first layer includes a layer of a resin having cholesteric regularity (hereinafter also referred to as a "cholesteric resin layer").
[0113] (Cholesteric resin layer)
[0114] The cholesteric regularity of the resin layer having cholesteric regularity refers to the following structure: the molecular axes are arranged in a certain direction on one plane, the direction of the molecular axes in the next plane overlapping it is slightly deflected at an angle, and then the angle is further deflected in the next plane, and as the planes arranged overlapping in this way are successively passed through, the angle of the molecular axes in the plane is gradually deflected (twisted). That is, when the molecules in the layer have cholesteric regularity, the molecules are arranged in the resin layer in a manner that forms a layer of multiple molecules. In a certain layer A among the layers of multiple molecules, the molecules are arranged in a manner that the molecular axes are in a certain direction, in the layer B adjacent to it, the molecules are arranged in a direction deflected at an angle to the direction of layer A, and in the layer C adjacent to it, the molecules are arranged in a direction further deflected at an angle to the direction of layer B. In this way, in the layer of multiple molecules, the angle of the molecular axis is continuously deflected, forming a structure in which the molecules are twisted. In this way, the structure in which the direction of the molecular axis is gradually twisted is optically a chiral structure.
[0115] The cholesteric resin layer generally has a circularly polarized light separation function. That is, the cholesteric resin layer has the property of transmitting one of right-handed circularly polarized light and left-handed circularly polarized light and reflecting a part or all of the other circularly polarized light. The reflection in the cholesteric resin layer is reflected in a state where its chirality is maintained.
[0116] The wavelength that exerts the circularly polarized light separation function depends on the pitch of the helical structure in the cholesteric resin layer. The pitch of the helical structure refers to the distance in the normal direction of the plane from the direction angle of the molecular axis gradually shifting as the plane moves forward and then returning to the original molecular axis direction. By changing the size of the pitch of the helical structure, the wavelength that exerts the circularly polarized light separation function can be changed.
[0117] The cholesteric resin layer can be obtained, for example, by providing a film of a cholesteric liquid crystal composition on an appropriate support for forming the resin layer, and curing the film of the cholesteric liquid crystal composition. The obtained layer can be directly used as the cholesteric resin layer. The cholesteric resin layer is a layer composed of a film of a material itself that reflects one of right-handed circularly polarized light and left-handed circularly polarized light and transmits the other circularly polarized light. Thus, the cholesteric resin layer itself can be used as the first layer.
[0118] As a cholesteric liquid crystal composition for forming a cholesteric resin layer, for example, a composition containing a liquid crystal compound and capable of presenting a cholesteric liquid crystal phase when forming a film on a support can be used. Here, as a liquid crystal compound, a liquid crystal compound and a polymerizable liquid crystal compound as a polymer compound can be used. In terms of obtaining high thermal stability, a polymerizable liquid crystal compound is preferably used. By polymerizing the polymerizable liquid crystal compound in a state of cholesteric regularity, the film of the cholesteric liquid crystal composition can be cured, and a non-liquid crystal resin layer cured in a state of cholesteric regularity can be obtained.
[0119] Preferred cholesteric resin layers having high reflectivity in the wavelength region of 420 nm to 650 nm include, for example: (i) a cholesteric resin layer in which the pitch of the helical structure is changed stepwise; and (ii) a cholesteric resin layer in which the pitch of the helical structure is changed continuously.
[0120] (i) The cholesteric resin layer in which the pitch of the helical structure changes in stages can be obtained by forming a plurality of cholesteric resin layers having different pitches of the helical structure. When giving a specific example, such a cholesteric resin layer can be manufactured by pre-fabricating a plurality of cholesteric resin layers having different pitches of the helical structure and then fixing each layer via a binder or adhesive. Alternatively, it can be manufactured by sequentially forming other cholesteric resin layers on the basis of forming a cholesteric resin layer.
[0121] (ii) There is no particular limitation on the method for preparing a cholesteric resin layer in which the pitch of the spiral structure varies continuously. As a preferred example of the method for preparing such a cholesteric resin layer, the following method can be cited: a cholesteric liquid crystal composition containing a polymerizable liquid crystal compound for forming a cholesteric resin layer is preferably applied on other layers such as an orientation film to obtain a layer of the liquid crystal composition, and then the layer is cured by light irradiation and / or heat treatment one or more times so that the pitch of the spiral structure varies continuously. This operation is an operation for expanding the reflection band of the cholesteric resin layer, so it is called broadband treatment. By performing broadband treatment, even a thin cholesteric resin layer, such as a layer with a thickness of less than 5 μm, can achieve a wide reflection band, so it is preferred.
[0122] As a preferred embodiment of the cholesteric liquid crystal composition to be subjected to such broadband widening treatment, there can be mentioned the cholesteric liquid crystal composition (X) described in detail below.
[0123] The cholesteric resin layer that continuously changes the pitch of the helical structure may be used alone or in multiple layers. For example, a cholesteric resin layer that performs a circularly polarized light separation function in a part of the visible light region and a cholesteric resin layer that performs a circularly polarized light separation function in other regions may be used in combination, and a first resin layer that performs a circularly polarized light separation function in a wide region in the visible light region may be used.
[0124] As described above, the cholesteric resin layer may be a resin layer consisting of only one layer, or may be a resin layer consisting of two or more layers. In the case of having more than two layers, the cholesteric resin layer may have two or more layers of the cholesteric resin layer of (i) above, may have two or more layers of the cholesteric resin layer of (ii) above, or may have two or more layers consisting of a combination of the two. From the viewpoint of easy manufacturing, the number of layers constituting the cholesteric resin layer is preferably 1 to 100 layers, and more preferably 1 to 20 layers. The result of the above-mentioned broadband processing is that in the case of obtaining a cholesteric resin layer having a high reflectivity with only one layer, an identification medium of a preferred form can be obtained even if only the layer is used.
[0125] The cholesteric liquid crystal composition (X) contains a compound represented by the following formula (5) and a specific rod-like liquid crystal compound. The compound represented by formula (5) and the rod-like liquid crystal compound may be used alone or in combination of two or more at any ratio.
[0126] Hereinafter, each of these components will be described in sequence.
[0127] R 1 -A 1 -BA 2 -R 2 (5)
[0128] In formula (5), R 1 and R 2 Each is independently a group selected from a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched alkylene oxide group having 1 to 20 carbon atoms, a hydrogen atom, a halogen atom, a hydroxyl group, a carboxyl group, a (meth)acryloyl group, an epoxy group, a mercapto group, an isocyanate group, an amino group, and a cyano group.
[0129] The above-mentioned alkyl and epoxyalkyl groups may be unsubstituted or may be substituted with one or more halogen atoms. Furthermore, the above-mentioned halogen atoms, hydroxyl groups, carboxyl groups, (meth)acryloyl groups, epoxy groups, mercapto groups, isocyanate groups, amino groups, and cyano groups may be bonded to alkyl and epoxyalkyl groups having 1 to 2 carbon atoms.
[0130] As R 1 and R 2Preferred examples of the group include a halogen atom, a hydroxyl group, a carboxyl group, a (meth)acryloyl group, an epoxy group, a mercapto group, an isocyanate group, an amino group, and a cyano group.
[0131] In addition, R 1 and R 2 At least one of them is preferably a reactive group. 1 and R 2 At least one of the above compounds represented by formula (5) is fixed in the cholesteric resin layer during curing, and a stronger layer can be formed. Here, as the reactive group, for example, a carboxyl group, a (meth)acryloyl group, an epoxy group, a mercapto group, an isocyanate group, and an amino group can be cited.
[0132] In formula (5), A 1 and A 2 Each independently represents a group selected from 1,4-phenylene, 1,4-cyclohexylene, 1,4-cyclohexenylene, 4,4'-biphenylene, 4,4'-bicyclohexylene, and 2,6-naphthylene. The above-mentioned 1,4-phenylene, 1,4-cyclohexylene, 1,4-cyclohexenylene, 4,4'-biphenylene, 4,4'-bicyclohexylene, and 2,6-naphthylene may be unsubstituted or substituted with one or more halogen atoms, hydroxyl groups, carboxyl groups, cyano groups, amino groups, alkyl groups having 1 to 10 carbon atoms, halogenated alkyl groups, etc. When A 1 and A 2 When there are two or more substituents in each of the groups, these substituents may be the same or different.
[0133] As A 1 and A 2 Particularly preferred groups include groups selected from 1,4-phenylene, 4,4'-biphenylene, and 2,6-naphthylene. Compared with alicyclic skeletons, these aromatic ring skeletons are relatively rigid, have high affinity with the mesogen of rod-shaped liquid crystal compounds, and have higher alignment uniformity.
[0134] In formula (5), B is selected from a single bond, -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH2-, -OCH2-, -CH=NN=CH-, -NHCO-, -OCOO-, -CH2COO-; and -CH2OCO-.
[0135] Particularly preferred examples of B include a single bond, -OCO-, and -CH=NN=CH-.
[0136] Preferably, at least one of the compounds of formula (5) has liquid crystal properties, and preferably has chirality. In addition, the cholesteric liquid crystal composition (X) preferably contains a mixture of multiple optical isomers as the compound of formula (5). For example, it may also contain a mixture of multiple enantiomers and / or diastereomers. Preferably, at least one of the compounds of formula (5) has a melting point in the range of 50°C to 150°C.
[0137] When the compound of formula (5) has liquid crystal properties, it is preferred that Δn is high. By using a liquid crystal compound with high Δn as the compound of formula (5), Δn of the cholesteric liquid crystal composition (X) can be increased, and a cholesteric resin layer capable of reflecting circularly polarized light in a wide wavelength range can be prepared. Δn of at least one compound of formula (5) is preferably 0.18 or more, more preferably 0.22 or more. The upper limit of Δn can be, for example, 0.50.
[0138] Particularly preferred specific examples of the compound of formula (5) include the following compounds (A1) to (A10):
[0139] [Chemical formula 1]
[0140]
[0141] In the above compound (A3), "*" represents a chiral center.
[0142] The cholesteric liquid crystal composition (X) generally has a Δn of 0.18 or more and contains a rod-like liquid crystal compound having at least two reactive groups in one molecule.
[0143] Examples of the rod-like liquid crystal compound include compounds represented by formula (6).
[0144] R 3 -C 3 -D 3 -C 5 -MC 6 -D 4 -C 4 -R 4 (6)
[0145] In formula (6), R 3 and R 4 are reactive groups, each independently selected from (meth)acryloyl, (thio)epoxy, oxetanyl, thietanyl, aziridine, pyrrolyl, vinyl, allyl, fumarate, cinnamoyl, The group in oxazoline group, sulfhydryl group, iso(thio)cyanate group, amino group, hydroxyl group, carboxyl group and alkoxysilyl group.By having these reactive groups, when making cholesteric liquid crystal composition solidify, can obtain the solidified material with the film strength that can withstand practical use.Herein, can withstand practical film strength and refer to be usually HB or more, preferably H or more in pencil hardness (JIS K5400).By making film strength so high, can not be easily damaged, therefore can improve operability.
[0146] In formula (6), D 3 and D 4 It represents a group selected from a single bond, a linear or branched alkyl group having 1 to 20 carbon atoms, and a linear or branched alkylene oxide group having 1 to 20 carbon atoms.
[0147] In formula (6), C 3 ~C 6 It represents a group selected from a single bond, -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH2-, -OCH2-, -CH=NN=CH-, -NHCO-, -OCOO-, -CH2COO-, and -CH2OCO-.
[0148] In formula (6), M represents a mesogenic group. Specifically, M represents an unsubstituted or substituted azomethine, azoxy, phenyl, biphenyl, terphenyl, naphthalene, anthracene, benzoate, cyclohexanecarboxylic acid phenyl ester, cyanophenylcyclohexane, cyano substituted phenyl pyrimidine, alkoxy substituted phenyl pyrimidine, phenyl diphenyl ester ... A group in which 2 to 4 skeletons of alkanes, diphenylacetylenes, and alkenylcyclohexylbenzonitriles are bonded by bonding groups such as -O-, -S-, -SS-, -CO-, -CS-, -OCO-, -CH2-, -OCH2-, -CH=NN=CH-, -NHCO-, -OCOO-, -CH2COO-, and -CH2OCO-.
[0149] Examples of the substituent that the mesogenic group M may have include a halogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, a cyano group, a nitro group, a -OR 5 、-OC(=O)-R 5 、-C(=O)-OR 5 、-OC(=O)-OR 5 、-NR 5 -C(=O)-R 5 、-C(=O)-NR 5 R 7 , or -OC(=O)-NR 5 R7 Here, R 5 and R 7 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. 5 and R 7 In the case of an alkyl group, -O-, -S-, -OC(=O)-, -C(=O)-O-, -OC(=O)-O-, -NR 6 -C(=O)-, -C(=O)-NR 6 -、-NR 6 -, or -C(=O)- (excluding the case where two or more -O- are inserted adjacently and two or more -S- are inserted adjacently). 6 It represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0150] As the substituent in the above-mentioned “alkyl group having 1 to 10 carbon atoms which may have a substituent”, there can be mentioned, for example, a halogen atom, a hydroxyl group, a carboxyl group, a cyano group, an amino group, an alkoxy group having 1 to 6 carbon atoms, an alkoxyalkoxy group having 2 to 8 carbon atoms, an alkoxyalkoxyalkoxy group having 3 to 15 carbon atoms, an alkoxycarbonyl group having 2 to 7 carbon atoms, an alkoxycarbonyl group having 2 to 7 carbon atoms, an alkoxycarbonyloxy group having 2 to 7 carbon atoms, and the like.
[0151] In addition, the rod-shaped liquid crystal compound preferably has an asymmetric structure. Here, the asymmetric structure means that in formula (6), the mesogenic group M is the center and R 3 -C 3 -D 3 -C 5 -and-C 6 -D 4 -C 4 -R 4 Different structures: By using a compound with an asymmetric structure as the rod-like liquid crystal compound, the alignment uniformity can be further improved.
[0152] The Δn of the rod-like liquid crystal compound is preferably 0.18 or more, more preferably 0.22 or more. When a rod-like liquid crystal compound having a Δn value of 0.30 or more is used, the absorption end of the long wavelength side of the ultraviolet absorption spectrum sometimes extends to the visible region. However, as long as the optical properties desired by the spectrum are not adversely affected, the rod-like liquid crystal compound whose absorption end of the spectrum extends to the visible region can be used. By using a rod-like liquid crystal compound having such a high Δn, a cholesteric resin layer having high optical properties (such as selective reflection properties of circularly polarized light) can be obtained. The upper limit of Δn can be, for example, 0.50.
[0153] Preferred specific examples of the rod-like liquid crystal compound include the following compounds (B1) to (B14). However, the rod-like liquid crystal compound is not limited to the following compounds.
[0154] [Chemical formula 2]
[0155]
[0156] [Chemical formula 3]
[0157]
[0158] [Chemical formula 4]
[0159]
[0160] In the cholesteric liquid crystal composition (X), the weight ratio of (total weight of the compounds of formula (5)) / (total weight of the rod-shaped liquid crystal compounds) is preferably 0.05 or more, more preferably 0.1 or more, particularly preferably 0.15 or more, preferably 1 or less, more preferably 0.65 or less, particularly preferably 0.45 or less. By making the above-mentioned weight ratio above the lower limit of the above-mentioned range, the orientation uniformity can be improved. In addition, by setting it to below the upper limit, the orientation uniformity can be improved, the stability of the liquid crystal phase can be improved, and then the Δn as a liquid crystal composition can be improved to stably obtain the desired optical properties (such as the property of selectively reflecting circularly polarized light). Here, the total weight represents its weight when using one type, and represents the total weight when using two or more types.
[0161] In the cholesteric liquid crystal composition (X), the molecular weight of the compound of formula (5) is preferably less than 600, and the molecular weight of the rod-shaped liquid crystal compound is preferably not less than 600. Thus, the compound of formula (5) can enter the gaps between the rod-shaped liquid crystal compounds having a larger molecular weight than the compound of formula (5), thereby improving the alignment uniformity.
[0162] In order to improve the film strength after curing and improve durability, the cholesteric liquid crystal composition (X) and other cholesteric liquid crystal compositions may contain a crosslinking agent as desired. As the crosslinking agent, a crosslinking agent that reacts simultaneously with the curing of the film of the cholesteric liquid crystal composition, or is heat-treated after curing to promote the reaction, or reacts naturally by moisture, can be appropriately selected and used, and can increase the crosslinking density of the cholesteric resin layer without deteriorating the orientation uniformity. Therefore, any crosslinking agent that is cured, for example, by ultraviolet rays, heat, moisture, etc. can be appropriately used. Examples of the crosslinking agent include: polyfunctional acrylate compounds such as trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and 2-(2-vinyloxyethoxy)ethyl acrylate; epoxy compounds such as glycidyl (meth)acrylate, ethylene glycol diglycidyl ether, glycerol triglycidyl ether, and pentaerythritol tetraglycidyl ether; aziridine compounds such as 2,2-bis(hydroxymethylbutanol)tris[3-(1-aziridinyl)propionate], 4,4-bis(ethyleneiminocarbonylamino)diphenylmethane, and trimethylolpropane tris-β-aziridinylpropionate; isocyanate compounds such as hexamethylene diisocyanate, isocyanurate-type isocyanates derived from hexamethylene diisocyanate, biuret-type isocyanates, and adduct-type isocyanates; and Oxazoline-based poly Azoline compound; vinyl trimethoxysilane, N-(2-aminoethyl) 3-aminopropyl trimethoxysilane, 3-aminopropyl trimethoxysilane, 3-glycidoxypropyl trimethoxysilane, 3-(methyl)acryloxypropyl trimethoxysilane, N-(1,3-dimethylbutylene)-3-(triethoxysilyl)-1-propylamine and other alkoxysilane compounds. In addition, the cross-linking agent can be used alone or in combination of two or more in any ratio. Furthermore, a known catalyst can also be used according to the reactivity of the cross-linking agent. By using a catalyst, in addition to improving the film strength and durability of the cholesteric resin layer, productivity can also be improved.
[0163] The amount of the crosslinking agent is preferably such that the amount of the crosslinking agent in the cured film obtained by curing the film of the cholesteric liquid crystal composition is 0.1 wt % to 15 wt %. By setting the amount of the crosslinking agent to be above the lower limit of the above range, the crosslinking density can be effectively increased. In addition, by setting it to be below the upper limit, the stability of the film of the cholesteric liquid crystal composition can be improved.
[0164] The cholesteric liquid crystal composition may contain a photoinitiator as desired. As the photoinitiator, a known compound that generates free radicals or acids by ultraviolet light or visible light can be used. Specific examples of the photoinitiator include: benzoin, benzyl dimethyl ketal, benzophenone, biacetyl, acetophenone, Michler's ketone, benzyl, benzyl isobutyl ether, tetramethylthiuram mono(di)sulfide, 2,2-azobisisobutyronitrile, 2,2-azobis-2,4-dimethylvaleronitrile, benzoyl peroxide, di-tert-butyl peroxide, 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, 1-(4-isopropyl)-1-ol phenyl)-2-hydroxy-2-methylpropane-1-one, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-diethylthioxanthone, methyl benzoylformate, 2,2-diethoxyacetophenone, β-ionone, β-bromostyrene, diazoaminobenzene, α-amylcinnamaldehyde, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, 2-chlorobenzophenone, pp'-dichlorobenzophenone, pp'-bis(diethylaminobenzophenone), benzoin ethyl ether, benzoin isopropyl ether, benzoin n-propyl ether, benzoin n-butyl ether, diphenyl sulfide, bis(2,6-methoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, 2,4,6-trimethylbenzoyldiphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2-methyl-1[4-(methylthio)phenyl]-2-morpholinyl-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinyl)propanone 1-[(4-(phenylthio)-2-(o-benzoyl oxime)]], 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanone 1-(o-acetyl oxime) and other carbazole oxime compounds, (4-methylphenyl)[4-(2-methylpropyl)phenyl]iodide Hexafluorophosphate, 3-methyl-2-butynyltetramethylene sulfide Hexafluoroantimonate, diphenyl-(p-phenylphenylthio)sulfide Hexafluoroantimonate, etc. In addition, these may be used alone or in combination of two or more in any ratio. Furthermore, a known photosensitizer or a tertiary amine compound as a polymerization accelerator may be used to control curability as needed.
[0165] The amount of the photoinitiator is preferably 0.03 wt % to 7 wt % in the cholesteric liquid crystal composition. By setting the amount of the photoinitiator to be above the lower limit of the above range, the degree of polymerization can be increased, thereby increasing the film strength of the cholesteric resin layer. In addition, by setting it below the upper limit, the orientation of the liquid crystal material can be improved, thereby stabilizing the liquid crystal phase of the cholesteric liquid crystal composition.
[0166] The cholesteric liquid crystal composition may contain a surfactant arbitrarily. As a surfactant, a surfactant that does not hinder orientation may be appropriately selected. As such a surfactant, a nonionic surfactant containing siloxane or fluorinated alkyl in the hydrophobic group may be appropriately cited. Among them, oligomers having two or more hydrophobic groups in one molecule are particularly preferred. As specific examples of these surfactants, PF151N, PF-636, PF-6320, PF-656, PF-6520, PF-3320, PF-651, PF-652 of PolyFox of Omnofa; FTX-209F, FTX-208G, FTX-204D of FTERGENT of Neos Co., Ltd.; KH-40 of Surflon of Seimei Chemical Co., Ltd., etc. may be used. In addition, the surfactant may be used alone or in combination of two or more in any ratio.
[0167] The amount of the surfactant is preferably such that the amount of the surfactant in the cured film obtained by curing the cholesteric liquid crystal composition is 0.05 wt % to 3 wt %. By setting the amount of the surfactant to be above the lower limit of the above range, the orientation restriction force of the air interface can be increased, thereby preventing orientation defects. In addition, by setting it below the upper limit, it is possible to prevent the decrease in orientation uniformity caused by excessive surfactant entering between liquid crystal molecules.
[0168] The cholesteric liquid crystal composition may contain a chiral agent at will. Generally, the twisting direction of the cholesteric resin layer can be appropriately selected according to the type and structure of the chiral agent used. When the twisting direction is set to the right direction, it can be achieved by using a chiral agent that imparts right-handedness, and when the twisting direction is set to the left direction, it can be achieved by using a chiral agent that imparts left-handedness. As specific examples of chiral reagents, chiral reagents described in Japanese Patent Laid-Open No. 2005-289881, Japanese Patent Laid-Open No. 2004-115414, Japanese Patent Laid-Open No. 2003-66214, Japanese Patent Laid-Open No. 2003-313187, Japanese Patent Laid-Open No. 2003-342219, Japanese Patent Laid-Open No. 2000-290315, Japanese Patent Laid-Open No. 6-072962, U.S. Patent No. 6468444, International Publication No. 98 / 00428, Japanese Patent Laid-Open No. 2007-176870, etc. can be appropriately used, and for example, Paliocolor LC756 of BASF AG can be obtained. In addition, the chiral reagent can be used alone or in combination of two or more at any ratio.
[0169] The amount of the chiral agent can be arbitrarily set within a range that does not reduce the desired optical properties. The specific amount of the chiral agent is usually 1% to 60% by weight in the cholesteric liquid crystal composition.
[0170] The cholesteric liquid crystal composition may further contain other arbitrary components as required. As the arbitrary components, for example, solvents, polymerization inhibitors for improving the shelf life, antioxidants for improving durability, ultraviolet absorbers, light stabilizers, etc. can be cited. In addition, these arbitrary components can be used alone or in combination of two or more in any ratio. The amount of these arbitrary components can be arbitrarily set within the range of not reducing the desired optical properties.
[0171] The method for producing the cholesteric liquid crystal composition is not particularly limited, and the cholesteric liquid crystal composition can be produced by mixing the above-mentioned components.
[0172] The cholesteric resin layer can be obtained, for example, as follows: on the surface of a support body composed of a film such as a transparent resin, a corona discharge treatment, a rubbing treatment, etc. are performed as needed, and an orientation film is provided as needed, and a film of a cholesteric liquid crystal composition is provided on the surface, and an orientation treatment and / or curing treatment is performed as needed.
[0173] As a support that can be used for forming a cholesteric resin layer, there can be cited, for example, a single layer or laminated film composed of a synthetic resin such as alicyclic olefin polymers, chain olefin polymers such as polyethylene and polypropylene, triacetyl cellulose, polyvinyl alcohol, polyimide, polyarylate, polyesters such as polyethylene terephthalate, polycarbonate, polysulfone, polyethersulfone, modified acrylic polymer, epoxy resin, polystyrene, acrylic resin, etc.
[0174] The alignment film can be formed, for example, by applying a solution obtained by dissolving the material of the alignment film in a solvent onto the surface of the support body after corona discharge treatment or the like as needed, drying the solution, and then performing rubbing treatment.
[0175] As the material of the alignment film, for example, cellulose, silane coupling agent, polyimide, polyamide, polyvinyl alcohol, epoxy acrylate, silanol oligomer, polyacrylonitrile, phenolic resin, polyol, Azoles, cyclized polyisoprene, etc.
[0176] The cholesteric liquid crystal composition can be applied onto the support or the alignment film by a known method such as extrusion coating, direct gravure coating, reverse gravure coating, die coating, or bar coating.
[0177] The alignment treatment can be performed, for example, by heating the film of the cholesteric liquid crystal composition at 50° C. to 150° C. for 0.5 to 10 minutes. By performing the alignment treatment, the cholesteric liquid crystal composition in the film can be well aligned.
[0178] The curing treatment can be performed by a combination of one or more light irradiation and heating treatment.
[0179] The heating conditions are, for example, usually 40°C or higher, preferably 50°C or higher, and usually 200°C or lower, preferably 140°C or lower, and usually 1 second or higher, preferably 5 seconds or higher, and usually 3 minutes or lower, preferably 120 seconds or lower.
[0180] The light used for light irradiation includes not only visible light but also ultraviolet rays and other electromagnetic waves. Light irradiation can be performed by irradiating light having a wavelength of 200 nm to 500 nm for 0.01 seconds to 3 minutes, for example.
[0181] Here, 0.01 mJ / cm 2 ~50mJ / cm 2 The weak ultraviolet irradiation and heating can obtain the circularly polarized light separation function of the helical structure by continuously changing the pitch of the helical structure and widening the reflection band. Furthermore, after the reflection band is expanded by the weak ultraviolet irradiation, 50mJ / cm 2 ~10000mJ / cm 2 Such strong ultraviolet rays completely polymerize the liquid crystal compound, thereby obtaining a cholesteric resin layer. The above-mentioned expansion of the reflection band and irradiation with strong ultraviolet rays can be carried out in air, or part or all of the process can be carried out in an environment with controlled oxygen concentration (such as a nitrogen environment).
[0182] The steps of coating and curing the cholesteric liquid crystal composition on other layers such as the alignment film are not limited to one time, and the coating and curing may be repeated multiple times to form two or more cholesteric resin layers. However, by using a cholesteric liquid crystal composition such as the cholesteric liquid crystal composition (X), a cholesteric resin layer containing a well-oriented rod-shaped liquid crystal compound having a Δn of 0.18 or more and having a thickness of 5 μm or more can be easily formed even by coating and curing the cholesteric liquid crystal composition only once.
[0183] The cholesteric resin layer obtained in this way can be used directly as the first layer together with the support and the alignment film. Alternatively, the support can be peeled off as necessary, and only the cholesteric resin layer can be transferred and used as the first layer.
[0184] The thickness of the first layer is preferably 2 μm or more, more preferably 3 μm or more, preferably 1000 μm or less, more preferably 500 μm or less. By setting the thickness of the first layer to be above the lower limit, it is not easy to see the information of the second layer when observing the second layer from the first layer side, thereby making it possible to make a clearer judgment of authenticity. By setting the thickness of the first layer to be below the upper limit, the transparency can be improved. Here, regarding the thickness of the first layer, when the first layer is a layer of more than two layers, it refers to the total thickness of each layer, and when the first layer is a single layer, it refers to its thickness. When a support is used, the in-plane delay of the support is preferably 20 nm or less, more preferably 10 nm or less, and ideally 0 nm. By setting the delay to be below the upper limit, the circularly polarized light generated by the first and second layers can be maintained, making the authenticity judgment clearer.
[0185] (Layer containing norbornene-based resin)
[0186] The first layer can be a laminate of the above-mentioned cholesteric resin layer and a layer containing a norbornene resin (hereinafter also referred to as a "norbornene resin layer"). The norbornene resin layer tends to have lower adhesion to other layers than the cholesteric resin layer, so by using the surface provided with the second layer as the first layer, the adhesive forces F1 and F4 can be reduced, and thus the adhesive forces F1 to F8 between the layers of the identification medium can be easily adjusted.
[0187] The norbornene-based resin is a resin containing at least one of a norbornene-based polymer and a hydrogenated product thereof, and is generally a thermoplastic resin.
[0188] As examples of norbornene-based polymers and their hydrides, ring-opening polymers of monomers having a norbornene structure and their hydrides; addition polymers of monomers having a norbornene structure and their hydrides. In addition, as examples of ring-opening polymers of monomers having a norbornene structure, ring-opening homopolymers of a monomer having a norbornene structure, ring-opening copolymers of two or more monomers having a norbornene structure, and ring-opening copolymers of a monomer having a norbornene structure and any monomer copolymerizable therewith can be cited. Furthermore, as examples of addition polymers of monomers having a norbornene structure, addition homopolymers of a monomer having a norbornene structure, addition copolymers of two or more monomers having a norbornene structure, and addition copolymers of a monomer having a norbornene structure and any monomer copolymerizable therewith can be cited. As these polymers, for example, polymers disclosed in Japanese Patent Publication No. 2002-321302 can be cited.
[0189] Specific examples of the norbornene-based polymer and its hydrogenated product include “ZEONOR” manufactured by Zeon Corporation; “ARTON” manufactured by JSR Corporation; and “TOPAS” manufactured by TOPAS ADVANCED POLYMERS.
[0190] The thickness of the norbornene-based resin layer is not particularly limited, and can be, for example, 10 μm to 100 μm. The retardation of the norbornene-based resin layer is preferably 20 nm or less, more preferably 10 nm or less, and ideally 0 nm.
[0191] (Adhesive layer or bonding layer)
[0192] When the first layer includes a cholesteric resin layer and a norbornene-based resin layer, the two are bonded together via an adhesive layer or a bonding layer as necessary.
[0193] As the adhesive used for the adhesive layer, for example, as the adhesive, there can be mentioned, for example, acrylic adhesive, epoxy adhesive, polyurethane adhesive, polyester adhesive, polyvinyl alcohol adhesive, modified polyvinyl alcohol adhesive, polyolefin adhesive, modified polyolefin adhesive, polyvinyl alkyl ether adhesive, rubber adhesive, vinyl chloride-vinyl acetate adhesive, SEBS (styrene-ethylene-butylene-styrene copolymer) adhesive, ethylene-styrene copolymer and other ethylene adhesives, ethylene-(meth) methyl acrylate copolymer, ethylene-(meth) ethyl acrylate copolymer and other acrylate adhesives, etc. As the adhesive, from the viewpoint of curing the adhesive in a short time, an ultraviolet curing type adhesive is preferred, and from the viewpoint of making the adhesive layer thinner, a water-based adhesive of polyvinyl alcohol or modified polyvinyl alcohol can also be used.
[0194] The thickness of the adhesive layer is usually larger than 0 μm and preferably 5 μm or less when an ultraviolet curing adhesive is used, and is usually larger than 0 μm and preferably 0.1 μm or less when a water-based adhesive is used.
[0195] The adhesive and thickness used for the adhesive layer may be appropriately selected from those described as the adhesive and thickness of the material of the adhesive layer (A) described later, and may be used.
[0196] The adhesive for the adhesive layer and the adhesive for the bonding layer are usually selected in such a way that the bonding strength ( Figure 3 The adhesion F5) and the adhesion between the norbornene-based resin layer and the adhesive layer (or bonding layer) ( Figure 3 The bonding force F6) is greater than the bonding force between the layers provided on the side of the first layer provided with the second layer and the bonding force between the adhesive layer (A) and the adherend ( Figure 3 Medium, the adhesion force (F1~F4) is large.
[0197] [1.3.2. Second layer]
[0198] The second layer is a layer provided to overlap with the first layer, and is a layer provided to overlap with the first layer directly (ie, in contact with the first layer) or indirectly (ie, separated via another layer or the like).
[0199] like Figure 1 As shown, the second layer 12 can be a layer provided on a portion of the surface of the first layer 11. In addition, although not shown, the second layer can be a layer provided on the entire surface of the first layer. The second layer 12 being a layer provided on a portion of the surface of the first layer 11 means that there are regions with the second layer 12 and regions without the second layer 12 on the same plane of the first layer 11, regardless of the size of each region.
[0200] In the case where the second layer 12 is a layer provided on a part of the surface of the first layer 11, the second layer 12 may have a predetermined pattern shape including, for example, text, numbers, or graphics. In addition, the second layer may form a pattern by repeatedly arranging predetermined shapes such as straight lines and graphics. In the case where the second layer has a predetermined pattern shape, or forms a pattern, the deformation of the second layer when the adhesive layer (A) is peeled off can be easily identified, and reuse of the identification medium can be effectively prevented, which is preferred.
[0201] The second layer is a layer that can reflect at least a portion of circularly polarized light having the same rotation direction as the circularly polarized light reflected by the first layer, and transmits circularly polarized light having a rotation direction opposite to the circularly polarized light reflected by the first layer. In other words, the second layer is a layer that does not reflect or hardly reflects circularly polarized light having a rotation direction opposite to the circularly polarized light reflected by the first layer.
[0202] The second layer is a layer containing flakes of a resin having cholesteric regularity (also referred to as "cholesteric resin"). The cholesteric resin layer suitable as the first layer 11 can reflect one of right-handed circularly polarized light and left-handed circularly polarized light in at least a part of the visible light region and transmit the other circularly polarized light even when it is crushed, so it is preferred to use the crushed material as the flakes of the second layer.
[0203] The volume average particle size (D50) of the thin sheet included in the second layer is preferably 70 μm or more, more preferably 75 μm or more, preferably 300 μm or less, more preferably 200 μm or less, and particularly preferably 150 μm or less. This is because, by making the volume average particle size of the thin sheet above the lower limit, the bottom area of the thin sheet can be relatively increased and the side area can be reduced, so that the viewing of the surface and back of the identification medium can be good. On the other hand, by making the volume average particle size of the thin sheet below the above condition value, the reflected light of the second layer can be scattered well, and the information of the second layer can be easily viewed.
[0204] The present inventors have speculated as follows on the reason why the visibility of the front and back surfaces of the identification medium can be improved by setting the volume average particle size of the sheet within the above range. However, the technical scope of the present invention is not limited to the mechanism described below.
[0205] Figure 6 FIG. 2 is a three-dimensional diagram schematically showing a thin sheet and a light path irradiating the thin sheet. Figure 6 As shown, the thin film 12f included in the second layer generally has a bottom surface (upper surface t and lower surface u) and a side surface s. In such a thin film 12f, at least a portion of one of the circularly polarized lights (e.g., right-handed circularly polarized light A1R) in the non-polarized light A1 irradiated to one bottom surface (upper surface t) is reflected on its surface and inside and emitted from the upper surface u, and the other circularly polarized light (e.g., left-handed circularly polarized light A1L) is transmitted and emitted from the other bottom surface (lower surface u). On the other hand, a portion of the non-polarized light A1 irradiated to the side surface s of the thin film 12f is reflected by the interface between the thin film 12f and its outside, and is reflected as non-polarized reflected light A4. In addition, the non-polarized light A1 incident from the side surface s of the thin film 12f into the interior of the thin film 12f is emitted from the lower surface u of the thin film as an outgoing light A5 with a reduced degree of polarization. Since the first layer can transmit one of the circularly polarized lights that is reflected by the second layer and the other circularly polarized light in the opposite direction, when the identification medium is observed from the first layer side, in the area where the second layer is configured and its vicinity, when the other of the circularly polarized light in the reflected light A4 is non-polarized light and the outgoing light A5 is basically non-polarized light, the other of the circularly polarized light in the non-polarized light can be viewed by the observer through the first layer, thereby making it possible to see through the information of the second layer.
[0206] In this regard, by setting the volume average particle size (D50) of the sheet to a predetermined value or more, the bottom area of one side of the sheet can be relatively increased and the side area of the sheet can be relatively reduced, thereby suppressing the interface reflection of non-polarized light on the side of the sheet and the reduction in the polarization degree of the outgoing light caused by the incidence of non-polarized light from the side of the sheet. As a result, when the identification medium is observed from the first layer side, the information of the second layer can be suppressed from being seen through.
[0207] The particle size of the flakes refers to the diameter of the bottom surface when the flakes are assumed to be disc-shaped. The volume average particle size (D50) of the flakes is the 50% volume average particle size measured and calculated by dry method using a particle size distribution measuring device based on laser scattering and diffraction method (e.g., Laser Diffraction and Scattering Particle Size Distribution Measuring Device "LA-960V Series" manufactured by Horiba, Ltd.). The 50% volume average particle size is the particle size at the position where the cumulative frequency accumulated from the small diameter side becomes 50% in the obtained particle size distribution (volume basis). In the above-mentioned measuring device, it is possible to assume that the diameter of the bottom surface of the flakes is a true sphere with the above-mentioned diameter for measurement.
[0208] The ratio of the bottom area of one side of the sheet to the side area (bottom area / side area, S ratio) is preferably 1.5 or more, more preferably 1.7 or more, preferably 3.0 or less, more preferably 2.7 or less. By making the S ratio above the lower limit, the penetration of the second layer when observing the identification medium from the first layer side can be effectively suppressed. In addition, by making the S ratio below the upper limit, the reflected light of the second layer can be scattered well, and the information of the second layer can be easily viewed.
[0209] The ratio of the bottom area of one side of a sheet to the side area (bottom area / side area, S ratio) refers to the ratio of the bottom area of one side to the side area when the sheet is assumed to be disc-shaped, and is a value calculated by the following formula (7) based on the volume average particle size of the sheet and the thickness of the sheet.
[0210] S ratio = {π(r / 2) 2} / (πrL) (7)
[0211] In the above formula (7), r (μm) is the volume average particle size of the flakes (the diameter of the bottom surface of the flakes), and L (μm) is the thickness of the flakes.
[0212] The thickness of the sheet can be appropriately selected according to the desired volume average particle size of the sheet, and is not particularly limited, but is preferably 2 μm or more, more preferably 3 μm or more, preferably 10 μm or less, and more preferably 7.5 μm or less. The thickness of the sheet can be, for example, the same thickness as the thickness of the first layer, or a different thickness.
[0213] The average refractive index of the sheet can be appropriately selected according to the cholesteric resin used as the material of the sheet, for example, 1.4 or more, preferably 1.5 or more, preferably 1.8 or less, and more preferably 1.7 or less. This is because by setting the average refractive index of the sheet to the above range, the refractive index difference with the binder can be reduced, and the interface reflection with the sheet and its outer side can be suppressed.
[0214] The average refractive index of the sheet can be measured as the average refractive index of a cholesteric resin layer having the same thickness as the sheet. The cholesteric resin layer is formed into a spiral structure by arranging the rod-shaped liquid crystal compound contained in the solidified material of the cholesteric liquid crystal composition into a spiral shape, and the molecules of the rod-shaped liquid crystal compound have anisotropy of refractive index. Therefore, by measuring the refractive index of the four directions in the plane of the cholesteric resin layer respectively, and obtaining the average refractive index as the arithmetic average thereof, the refractive index of the cholesteric resin layer as a whole can be evaluated. The average refractive index of the cholesteric resin layer is obtained, for example, as follows: Using a prism coupler (e.g., manufactured by Metricon, model 2010), under the conditions of a measuring wavelength of 560nm, a temperature of 20°C ± 2°C, and a humidity of 60 ± 5%, a single layer of the cholesteric resin layer is measured in four directions (x1, x2, x3, and x4) in the plane, and the arithmetic average of the four refractive indices is calculated. Regarding the four directions x1, x2, x3 and x4 within the plane, when x1 is used as a reference (0°), x2 can be a direction of 45°, x3 can be a direction of 90°, and x4 can be a direction of 135°.
[0215] The area ratio of the sheet group per unit area of the second layer is preferably less than 60%, more preferably 50% or less, preferably 20% or more, and can be 25% or more.
[0216] This is because, by making the area ratio of the thin sheet group per unit area of the second layer less than the above upper limit, it is possible to suppress the overlapping of the thin sheets, and to suppress the bottom surface of the thin sheet from being dispersed obliquely relative to the surface direction of the second layer, thereby suppressing the interface reflection of non-polarized light at the side surface. On the other hand, by making the above area ratio greater than the above lower limit, it is possible to make the visibility of the second layer good.
[0217] The area ratio of the sheet group per unit area of the second layer can be obtained by observing the second layer with a digital microscope (e.g., "VHX-7000" manufactured by Keyence Corporation), performing image analysis on the digital microscope, and measuring the area ratio of the sheet group per unit area of the second layer (1 mm 2 ) and calculate the total area of multiple thin sheets present.
[0218] From the viewpoint of clear authenticity identification and high degree of freedom in design, the cholesteric resin used as the material of the sheet preferably has as high a reflectivity as possible, and as a result, a cholesteric resin having a high reflectivity in the wavelength range to be reflected is preferred.
[0219] The cholesteric resin sheet can be produced by, for example, the method for producing a release sheet described in Japanese Patent No. 6142714.
[0220] A sheet of a material having no polarization property can be used together with the sheet of cholesteric resin. Examples of the sheet having no polarization property include sheets of at least one selected from carbon black, oxides, nitrides, and oxynitrides of metals belonging to Groups 3 to 11 of Period 4 of the Periodic Table of Elements. These can be used alone or in combination of two or more in any ratio.
[0221] In the present embodiment, the second layer can be produced, for example, by applying a sheet consisting of a pulverized product of the cholesteric resin layer, a solvent, a binder, and an ink containing any component as required, on a support and drying the ink.
[0222] As the solvent, inorganic solvents such as water can be used, and organic solvents are generally used. When examples of organic solvents are given, organic solvents such as ketones, alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters, and ethers can be given. Among them, ketones are preferred in consideration of the burden on the environment. In addition, the solvent can be used alone or in combination of two or more in any ratio.
[0223] The amount of the solvent is usually 40 parts by weight or more, preferably 60 parts by weight or more, more preferably 80 parts by weight or more, and usually 1000 parts by weight or less, preferably 800 parts by weight or less, more preferably 600 parts by weight or less, relative to 100 parts by weight of the ground product of the cholesteric resin layer. By setting the amount of the solvent to the above range, the coating property of the ink can be improved.
[0224] As the binder, a polymer is generally used. Examples of the polymer include polyester polymers, acrylic polymers, polystyrene polymers, polyamide polymers, polyurethane polymers, polyolefin polymers, polycarbonate polymers, polyethylene polymers, etc. The binder may be used alone or in combination of two or more in any ratio.
[0225] The refractive index of the binder is preferably 1.4 or more, preferably 1.5 or more, preferably 1.8 or less, and more preferably 1.7 or less. In addition, the absolute value of the difference between the refractive index of the binder and the average refractive index of the sheet is preferably 0.2 or less, more preferably 0.1 or less, particularly preferably 0.05 or less, ideally 0, and can be 0.001 or more. This is because, by making the refractive index of the binder and the absolute value of the difference between the average refractive index of the sheet and the refractive index of the binder within the above range, the refractive index difference with the binder can be reduced, and the interface reflection with the sheet and its outer side can be suppressed.
[0226] The refractive index of the adhesive can be measured using a prism coupler (for example, model 2010 manufactured by Metricon) under the conditions of a measurement wavelength of 560 nm, a temperature of 20° C.±2° C., and a humidity of 60±5%.
[0227] The amount of the binder is usually 20 parts by weight or more, preferably 40 parts by weight or more, more preferably 60 parts by weight or more, and usually 1000 parts by weight or less, preferably 800 parts by weight or less, more preferably 600 parts by weight or less, relative to 100 parts by weight of the pulverized product of the cholesteric resin layer. By setting the amount of the binder to the above range, the coating property of the ink can be improved. In addition, the pulverized product of the cholesteric resin layer can be stably fixed in the second layer.
[0228] As optional components that can be contained in the ink, there can be mentioned, for example, antioxidants, ultraviolet absorbers, light stabilizers, bluing agents, etc. These may be used alone or in combination of two or more at any ratio.
[0229] The second layer can be obtained as a layer including flakes composed of a pulverized product of the cholesteric resin layer by printing the above-mentioned ink on the first layer in a predetermined pattern and drying the printed ink.
[0230] The ink described above may replace the polymer as a binder, or may contain a monomer of the polymer in combination with the polymer. In this case, after the ink is applied to a support and dried, the monomer is polymerized, thereby making it possible to manufacture a sheet consisting of a crushed product of the cholesteric resin layer and a second layer of the binder. In the case of containing the monomer, the ink preferably contains a polymerization initiator.
[0231] [1.3.3. Adhesive layer (A)]
[0232] The adhesive layer is a layer provided on the second layer. When the identification medium has a layer provided on a part of the surface of the first layer as the second layer, the adhesive layer is a layer provided between the first layer and the second layer.
[0233] As the adhesive of the material of the adhesive layer, for example, rubber adhesive, acrylic adhesive, polyvinyl ether adhesive, polyurethane adhesive, silicone adhesive, polyolefin adhesive and the like can be cited. Among them, acrylic adhesive and polyolefin adhesive are preferred from the viewpoint of heat resistance and productivity, and acrylic adhesive is particularly preferred. In addition, the adhesive can be used alone or in combination of two or more in any ratio.
[0234] The refractive index of the adhesive layer (A) is preferably 1.4 or more, preferably 1.5 or more, preferably 1.8 or less, and more preferably 1.7 or less. In addition, the absolute value of the difference between the refractive index of the adhesive layer (A) and the refractive index of the adhesive in the second layer is preferably 0.2 or less, more preferably 0.1 or less, particularly preferably 0.05 or less, ideally 0, and can be 0.001 or more. This is because, by setting the absolute value of the difference between the refractive index of the adhesive layer (A) and the adhesive in the second layer to be below the above upper limit, the interface reflection between the second layer and the adhesive layer (A) can be suppressed.
[0235] The refractive index of the adhesive layer (A) can be measured using a prism coupler (for example, model 2010 manufactured by Metricon) under the conditions of a measurement wavelength of 560 nm, a temperature of 20° C.±2° C., and a humidity of 60±5%.
[0236] The thickness of the adhesive layer is not particularly limited, and can be, for example, 1 μm or more and 200 μm or less.
[0237] [1.3.4. Arbitrary structure]
[0238] As an optional structure, the identification medium may include a protective layer provided via an adhesive layer or a bonding layer on the surface of the first layer opposite to the surface on which the second layer is provided.
[0239] As the protective layer, for example, a transparent substrate can be used. As the substrate that can be used as the material of the protective layer, for example, a plastic film and sheet such as a vinyl chloride sheet and an acrylic resin sheet, and a glass substrate can be mentioned. The thickness of the protective layer can preferably be 50 μm or more and 1000 μm or less.
[0240] The visible light transmittance of the protective layer is preferably 80% or more, more preferably 85% or more. From the viewpoint of maintaining the circularly polarized light state of the first layer 11, the retardation in the in-plane direction of the protective layer is preferably 20 nm or less, more preferably 10 nm or less, and ideally 0. The visible light transmittance can be measured using an ultraviolet-visible spectrophotometer.
[0241] The haze value of the protective layer is preferably 1.0% or less, and more preferably 0.5% or less. The haze value is ideally 0%. The haze can be measured using a haze meter (turbidimeter) in accordance with JIS K7361-1997.
[0242] The adhesive and thickness of the adhesive layer and the adhesive and thickness of the adhesive layer can be appropriately selected from the materials described above as the materials of the adhesive layer and the adhesive layer.
[0243] [1.4. Physical properties of identification medium]
[0244] In the identification medium 10 of the present embodiment, usually, the ratio (Ssf2 / S2) of Ssf2 defined by the following formula (9) to S2 defined by the following formula (8) is larger than 0.7.
[0245] [Mathematical formula 1]
[0246]
[0247] In formula (8), λ represents wavelength (nm), and Rf2(λ) represents the reflectivity of the second layer at wavelength λ. The S2 value defined by formula (8) is the integral value of the reflectivity Rf2 of the second layer at wavelengths of 400nm to 780nm.
[0248] [Mathematical formula 2]
[0249]
[0250] In formula (9), λ represents wavelength (nm), and Rs(λ) represents the reflectivity of the first layer at wavelength λ. The Ssf2 value defined by formula (9) is the integrated value of the square root of the product of the reflectivity Rs of the first layer and the reflectivity Rf2 of the second layer at wavelengths of 400nm to 780nm.
[0251] Rs(λ) and Rf2(λ) are reflectances at wavelength (λ) when non-polarized light of wavelength 400 nm to 780 nm is incident on the target layer, and the reflectance can be measured using, for example, an ultraviolet-visible spectrophotometer (UV-Vis 550, manufactured by JASCO Corporation). The measured value measured by the above device may include interface reflection, so in such a case, the reflectance Rs(λ) and Rf2(λ) are calculated by subtracting the interface reflection portion.
[0252] When Ssf2 / S2 is greater than 0.7, when the identification medium is observed from the second layer side, the information of the second layer can be observed with the naked eye, but when the identification medium is reversed and observed from the first layer side, the information of the second layer cannot be viewed. Therefore, when the Ssf2 / S2 value is large, it is effective in determining authenticity. The Ssf2 / S2 value is preferably greater than 0.75, and more preferably greater than 1.0. When the Ssf2 / S2 value is greater than 1.0, there is almost no difference between individuals in determining whether it is unviewable or viewable, and the determination can be made objectively. The upper limit of the Ssf2 / S2 value is not particularly limited, and may preferably be less than 5, and more preferably less than 3. By setting it in such a range, information such as text patterns on the second layer can be well viewed.
[0253] The reflectivity of the first layer to the incident non-polarized light is preferably 35% or more and 50% or less at all wavelengths in the wavelength range of 420nm to 650nm. The above reflectivity is more preferably 40% or more, and further preferably 45% or more. When the reflectivity of the first layer to the incident non-polarized light is in the above range, the first layer can be made into a broadband layer, thereby increasing the wavelength region where the reflection spectrum of the first layer overlaps with the reflection spectrum of the second layer, and the Ssf2 / S2 value can be increased. The reflectivity of the first layer to the incident non-polarized light can include the interface reflection part.
[0254] The wavelength of the reflected light of the first layer and the wavelength of the reflected light of the second layer are usually in the visible light region, and sometimes there is a difference ΔE between the hue produced by the reflected light of the first layer and the hue produced by the reflected light of the second layer. * , sometimes it does not have the above hue difference ΔE * . In the case of the difference ΔE with the above hue * In the case of , its value can be appropriately selected. The difference in hue ΔE * The measuring method is described in Implementation Example 2 described later.
[0255] The identification medium of the present embodiment is preferably transparent or translucent. When the identification medium 10 is transparent or translucent, it is preferred because it can make the copying and counterfeiting of the identification medium difficult. The transparency of the identification medium is sufficient as long as the identification medium is placed on an article printed with text, patterns, etc., and the text, etc. printed on the article can be viewed through the identification medium. When the identification medium is transparent or translucent, the transmittance of the non-polarized light incident on the identification medium can be preferably 20% or more, more preferably 40% or more. The upper limit of the transmittance is not particularly limited, and can be set to, for example, 90%. The above transmittance can be measured using, for example, the above-mentioned ultraviolet-visible spectrophotometer.
[0256] [2. Implementation Method 2]
[0257] Below, refer to Figure 7 to Figure 12 An identification medium according to a second embodiment of the present invention will be described.
[0258] Figure 7 This is an exploded perspective view schematically showing an identification medium according to Embodiment 2 of the present invention. Figure 8 For viewing from the second floor Figure 7 Schematic top view of the identification medium. Fig. 9 For viewing from the third floor Figure 7 Schematic top view of the identification medium. Fig.10 To schematically illustrate Figure 8 and Fig. 9 A cross-sectional view of the cross section taken along the X2-X2 direction. Fig.11An exploded cross-sectional view schematically showing the optical path when light is irradiated from the second layer side of the identification medium. Fig.12 The figure is an exploded cross-sectional view schematically showing the optical path when light is irradiated from the third layer side of the identification medium.
[0259] The identification medium 100 of the present embodiment is different from that of the first embodiment in that the surface of the first layer 111 opposite to the surface on which the second layer 112 is provided includes a third layer 113 provided to overlap with the first layer 111 .
[0260] The identification medium 100 of the present embodiment is a mode in which a third layer is provided on the surface of the first layer 11 of the identification medium 10 of the first embodiment which is opposite to the surface on which the second layer 12 is provided. That is, the first layer 111 (cholesteric resin layer 111a, norbornene resin layer 111b, and adhesive layer 111c), the second layer 112 including the sheet 112f, the adhesive layer (A) 114, the adhesive layer 115, and the protective layer 116 of the identification medium 100 of the present embodiment correspond to the first layer 11 (cholesteric resin layer 11a, norbornene resin layer 11b, and adhesive layer 11c), the second layer 12 including the sheet 12f, the adhesive layer (A) 14, the adhesive layer 15, and the protective layer 16 of the identification medium 10 of the first embodiment, respectively. In the following description, the description will be mainly based on the differences from the first embodiment.
[0261] like Figure 7 to Figure 10 As shown, the identification medium 100 of the present embodiment includes: a first layer 111; a second layer 112, which is arranged overlapping with the first layer 111; and a third layer 113, which is arranged overlapping with the first layer 111 on the surface of the first layer 111 opposite to the surface on which the second layer 112 is arranged. The third layer 113 is a layer that can transmit circularly polarized light with a rotation direction opposite to that of the circularly polarized light reflected by the first layer 111, that is, a layer that does not reflect or hardly reflects the circularly polarized light. In addition, the third layer 113 is a layer including a thin sheet 113f of a resin having cholesteric regularity. In Figure 7 and Fig. 9 In the embodiment, the third layer 113 is directly formed on the substrate layer 114 ( Fig.10 and Fig.13 The part with the letter pattern EFG on the lower surface (refer to Fig.12 ). The third layer 113 is formed at a position where the entire area thereof completely overlaps with the first layer 111.
[0262] The identification medium 100 is similar to the identification medium 10 of embodiment 1. When the adhesive layer (A) 114 is adhered to an adherend (not shown), the adhesive force F1 between the layer 111b of the first layer 111 and the second layer 112, the adhesive force F2 between the second layer 112 and the adhesive layer (A) 114, and the adhesive force F3 between the adhesive layer (A) 114 and the adherend satisfy the relationship of the following equations (1) and (2). Furthermore, when the adhesive layer (A) 14 is provided on the layer 111b of the first layer 111, the adhesive force F3 between the adhesive layer (A) 14 and the adherend, and the adhesive force F4 between the layer 111b of the first layer 111 and the adhesive layer (A) 114 satisfy the relationship of the following equation (4).
[0263] F1<F2(1)
[0264] F1<F3(2)
[0265] F 4<F 3(4)
[0266] According to this embodiment, by making the adhesive forces F1 and F2 between the layers of the identification medium when the identification medium is attached to the adherend, and the adhesive force F3 between the adhesive layer and the adherend satisfy a prescribed relationship, when the identification medium attached to the adherend is peeled off, the identification medium can be separated between the first layer and the second layer. The identification medium of this embodiment exhibits an optical function by having a structure in which the first layer, the second layer, and the third layer are stacked, and the authenticity can be determined by using this function without using a special observer. Therefore, when the first layer and the second layer are separated, the optical function is lost, and the function as the identification medium disappears, so it is possible to prevent the reuse of the identification medium peeled off from the adherend.
[0267] The optical function of the identification medium according to the present embodiment will be described using the drawings.
[0268] Fig.11 1 is a schematic exploded cross-sectional view showing the optical path when light is irradiated from the second layer 112 side of the identification medium. Fig.12 FIG. 1 is an exploded cross-sectional view schematically showing the light path when light is irradiated from the third layer side 113 of the identification medium. Fig.11 and Fig.12 The following example is shown: the first layer 111 is a layer capable of reflecting right-handed circularly polarized light and allowing left-handed circularly polarized light to pass through, the second layer 112 and the third layer 113 are layers capable of reflecting at least a portion of right-handed circularly polarized light and allowing left-handed circularly polarized light to pass through, that is, layers that do not reflect, or hardly reflect, left-handed circularly polarized light.
[0269] like Fig.11As shown, when non-polarized light A1 such as natural light is irradiated from the second layer 112 side, at least a portion of right-handed circularly polarized light A1R in the non-polarized light A1 is reflected by the thin sheets of the second layer 112. The thin sheets included in the second layer 112 are usually scattered in different directions, so the circularly polarized light A1R is observed as backscattered light A2R. On the other hand, left-handed circularly polarized light A1L in the non-polarized light A1 passes through the second layer 112, and the left-handed circularly polarized light A1L that has passed through the second layer 112 passes through the first layer 111. Furthermore, in the area where the third layer 113 is provided in the first layer 111, the left-handed circularly polarized light A1L that has passed through the first layer 111 passes through the third layer 113.
[0270] Furthermore, when the non-polarized light A1 is irradiated from the second layer 112 side toward the first layer 111 where the second layer 112 is not provided, the right circularly polarized light A1R in the non-polarized light A1 is specularly reflected by the first layer 111 to become the reflected light A3R. On the other hand, the left circularly polarized light A1L in the non-polarized light A1 passes through the first layer 111. Furthermore, in the region where the third layer 113 is provided in the first layer 111, the left circularly polarized light A1L that has passed through the first layer 111 passes through the third layer 113.
[0271] like Fig.12 As shown, when non-polarized light A1 such as natural light is irradiated from the third layer 113 side, at least a portion of right-handed circularly polarized light A1R in the non-polarized light A1 is reflected by the thin sheets of the third layer 113. The thin sheets included in the third layer 113 are usually scattered in different directions, so the circularly polarized light A1R is observed as backscattered light A2R. On the other hand, left-handed circularly polarized light A1L in the non-polarized light A1 passes through the third layer 113, and the left-handed circularly polarized light A1L that has passed through the third layer 113 passes through the first layer 111. Furthermore, in the area where the second layer 112 is provided in the first layer 111, the left-handed circularly polarized light A1L that has passed through the first layer 111 passes through the second layer 112.
[0272] Furthermore, when the non-polarized light A1 is irradiated from the third layer 113 side toward the first layer 111 where the second layer 113 is not provided, the right circularly polarized light A1R in the non-polarized light A1 is specularly reflected by the first layer 111 to become the reflected light A3R. On the other hand, the left circularly polarized light A1L in the non-polarized light A1 passes through the first layer 111. Furthermore, in the region where the second layer 112 is provided in the first layer 111, the left circularly polarized light that has passed through the first layer 111 passes through the second layer 112.
[0273] Therefore, when the identification medium is observed from the second layer 112 side, the backscattered light A2R is observed in the area of the identification medium where the second layer 112 is provided, and the reflected light A3R by specular reflection is observed in the area where the second layer 112 is not provided, by the non-polarized light A1 irradiated from the second layer 112 side, so the observer can see the information of the second layer 112 based on the difference between the backscattered light A2R and the reflected light A3R. In addition, when the non-polarized light A1 is irradiated from the third layer 113, the area where the third layer 113 is provided and the area where the third layer 113 is not provided in the identification medium are both transmitted to the same extent by the left-handed circularly polarized light A1L. Therefore, when the identification medium is observed from the second layer 112 side, the transmitted light A1L from the third layer 113 side can have no effect on the visibility of the information of the second layer 112, or even if there is an effect, it can be made very small. Specifically, the information of the third layer 113 can be prevented from being viewed.
[0274] On the other hand, when the identification medium is observed from the third layer 113 side, the backscattered light A2R is observed in the area of the identification medium where the third layer 113 is provided, and the reflected light A3R by specular reflection is observed in the area where the third layer 113 is not provided, by the non-polarized light A1 irradiated from the third layer 113 side. Therefore, the observer can observe the information of the third layer 113 based on the difference between the backscattered light A2R and the reflected light A3R. In addition, when the non-polarized light A1 is irradiated from the second layer 112 side, the left-handed circularly polarized light A1L is transmitted to the same extent in the area where the second layer 112 is provided and the area where the second layer 112 is not provided in the identification medium. Therefore, when the identification medium is observed from the third layer 113 side, the transmitted light A1L from the second layer 112 side can have no effect on the visibility of the information of the third layer 113, or even if there is an effect, it can be made very small. Specifically, the information of the second layer 112 can be prevented from being viewed.
[0275] As described above, when the structure in which the third layer, the first layer, and the second layer are stacked in sequence is observed from the front and back of the identification medium, the difference in visibility between the front and back of the identification medium of this embodiment can be recognized. Therefore, in the stacked body of the third layer and the first layer, and the single layer of the second layer, the expected difference in visibility cannot be recognized, and the identification function is lost, thereby preventing the reuse of the identification medium.
[0276] Furthermore, according to the present embodiment, different information can be given to the second layer 112 and the third layer 113 , respectively, so that authenticity can be determined more clearly, thereby improving the anti-counterfeiting effect.
[0277] Regarding the identification medium of this embodiment, the first layer, the second layer, and any structure may be the same as those described in the identification medium of the first embodiment.
[0278] [2.1. Third layer]
[0279] The third layer is a layer provided to overlap with the first layer. The third layer is a layer provided to overlap with the first layer directly (ie, in contact with the first layer) or indirectly (ie, separated via another layer or the like).
[0280] The third layer is a layer that can transmit circularly polarized light in a rotation direction opposite to that of the circularly polarized light reflected by the first layer. In other words, the second layer is a layer that does not reflect or hardly reflects circularly polarized light in a rotation direction opposite to that of the circularly polarized light reflected by the first layer. In addition, the third layer is preferably a layer that can reflect at least a portion of the circularly polarized light in the same rotation direction as that of the circularly polarized light reflected by the first layer.
[0281] Since the third layer is a layer disposed on the surface of the first layer opposite to the surface on which the second layer is disposed, the adhesive force between the first layer and the third layer is preferably greater than the adhesive force between the layers disposed on the surface of the first layer on which the second layer is disposed, and the adhesive force between the adhesive layer (A) and the adherend, i.e., the adhesive forces F1 to F4. In addition, when the third layer is disposed on the first layer via other layers, the adhesive force between the third layer and the other layers is preferably greater than the above-mentioned adhesive forces F1 to F4.
[0282] The materials included in the third layer, the manufacturing method, and the physical properties of the third layer may be the same as those described in the item of the second layer in the first embodiment.
[0283] [2.2. Physical properties of identification medium]
[0284] In the identification medium 100 of the present embodiment, the ratio (Ssf3 / S3) of Ssf3 defined by the following formula (11) to S3 defined by the formula (10) is larger than 0.7.
[0285] [Mathematical formula 3]
[0286]
[0287] In the formula (10), Rf3(λ) represents the reflectivity of the third layer at the wavelength (λ). The S3 value defined by the formula (10) is the integral value of the reflectivity Rf3 of the third layer.
[0288] [Formula 4]
[0289]
[0290] The Ssf3 value defined by the formula (11) is the integrated value of the square root of the product of the reflectivity Rs of the first layer and the reflectivity Rf3 of the third layer at a wavelength of 400 nm to 780 nm.
[0291] Rs(λ) and Rf3(λ) are reflectances at wavelength (λ) when non-polarized light of wavelength 400 nm to 780 nm is incident on the target layer, and the reflectance can be measured using, for example, an ultraviolet-visible spectrophotometer (UV-Vis 550, manufactured by JASCO Corporation). The measured value measured by the above device may include interface reflection, so in such a case, the reflectance Rs(λ) and Rf3(λ) are calculated by subtracting the interface reflection portion.
[0292] When Ssf3 / S3 is greater than 0.7, when the identification medium is observed from the third layer side, the information of the third layer can be observed with the naked eye, but when the identification medium is reversed and observed from the second layer side, the information of the third layer cannot be observed, so it is effective in determining the authenticity. The Ssf3 / S3 value is preferably greater than 0.75, and more preferably greater than 1.0. When the Ssf3 / S3 value is greater than 1.0, there is almost no difference between people in determining whether it is unviewable or viewable, and the determination can be made objectively. The upper limit of the Ssf3 / S3 value is not particularly limited, and can be preferably less than 5, and more preferably less than 3. By setting it in such a range, the information of the third layer can be well viewed.
[0293] The wavelength of the reflected light from the first layer and the wavelength of the reflected light from the third layer are usually in the visible light region, and sometimes there is a difference ΔE* between the hue produced by the reflected light from the first layer and the hue produced by the reflected light from the third layer, or sometimes there is no such difference ΔE*. * In the case of , its value can be selected appropriately.
[0294] The wavelength of the reflected light from the second layer and the wavelength of the reflected light from the third layer are both in the visible light region. Sometimes, there is a difference ΔE between the hue produced by the reflected light from the first layer and the hue produced by the reflected light from the third layer. * , sometimes it does not have the above hue difference ΔE * , but the former is preferred. As the difference in hue ΔE * , preferably 10 or more, more preferably 30 or more, and particularly preferably 50 or more. * When the value is equal to or greater than the lower limit, it is possible to easily visually confirm that the reflection colors of the second layer and the third layer are different, making it more difficult to copy or forge the identification medium, and also providing design characteristics due to a clear color difference, which is preferred. * The upper limit of can be 140, for example.
[0295] Hue difference ΔE * A colorimeter can be used for quantitative evaluation. Any colorimetric system can be used for quantitative evaluation, and for example, an XYZ colorimetric system, an L * a *b * Color system, etc.
[0296] The identification medium of this embodiment is preferably transparent or translucent. The transparency of the identification medium may be the same as that of the identification medium of the first embodiment.
[0297] [3. Other embodiments]
[0298] In the above embodiment, as a method for forming the second layer and the third layer, a method of printing ink containing a cholesteric resin flake into a predetermined pattern (e.g., a pattern of characters) is shown, but the method for forming the second layer and the third layer is not limited thereto. The second layer and the third layer may also be formed by a method of printing ink containing flakes into a patterned shape, or by forming a dispersion containing flakes into a layered shape by a molding method such as an extrusion molding method and a solvent casting method.
[0299] [thing]
[0300] An article according to one embodiment of the present invention includes the above-mentioned identification medium and an adherend to which the identification medium is adhered.
[0301] According to this embodiment, by making the article contain the above-mentioned identification medium, the authenticity of the article can be identified without using a special viewer. In addition, since the identification medium that can prevent reuse is included, it is possible to suppress the improper behavior of peeling off the identification medium of the real adherend and sticking the identification medium on the forged adherend, thereby improving the reliability of the article itself.
[0302] The adherend is preferably made of transparent material, and more preferably transparent glass, because the front and back surfaces of the identification medium can be observed through the object, and thus it is suitable for determining the authenticity of the identification medium using the present embodiment.
[0303] The visible light transmittance of the transparent glass is, for example, 70% or more, preferably 80% or more, and more preferably 85% or more. The haze value of the transparent glass is, for example, 1.0% or less, preferably 0.5% or less, and ideally 0%.
[0304] The form of the adherend is not particularly limited, and typical examples thereof include perfume bottles, wine bottles, and tableware.
[0305] Example
[0306] Hereinafter, the present invention will be described in detail with reference to the examples. However, the present invention is not limited to the examples shown below, and can be arbitrarily modified and implemented without departing from the scope of the claims of the present invention and the scope of their equivalents.
[0307] In the following description, "%" and "parts" indicating amounts are by weight unless otherwise specified. In addition, the following operations were performed at normal temperature and pressure (23°C ± 2°C, 1 atm) unless otherwise specified.
[0308] [Evaluation method]
[0309] [Measurement of volume average particle size of flakes]
[0310] The volume average particle size (D50) of the flakes is the particle size at the position where the cumulative frequency accumulated from the small diameter side is 50% in the particle size distribution (volume basis) calculated by measuring the coating material containing the flakes based on the laser diffraction method using the laser diffraction / scattering particle size distribution measuring apparatus "LA-960V Series" manufactured by Horiba, Ltd.
[0311] [Calculation of the area ratio of the bottom area on one side of the sheet to the side area]
[0312] Assuming that the flakes are disk-shaped, assuming that the volume average particle size (D50) of the flakes is the diameter r of the bottom area of the disk, calculate the bottom area of one side (π(r / 2) 2 ). In addition, the thickness of the cholesteric resin layer (5.2 μm) was used as the thickness (height) L of the disk, and the side area (πrL) was calculated. Based on the obtained value, the area ratio of the bottom area of one side of the sheet to the side area was calculated.
[0313] [Area ratio of sheet group per unit area of the second layer]
[0314] The second layer (printing layer) of the identification medium was observed using a digital microscope ("VHX-7000" manufactured by KEYENCE Corporation), and image analysis was performed on the digital microscope to measure the volume per unit volume (1 mm 2 ) are measured, the total value is obtained, and the area ratio of the sheet group per unit area of the second layer is calculated based on the total value.
[0315] [Measurement of Adhesion Strength and Tension]
[0316] The sample film for evaluation was prepared using the first layer of norbornene resin layer (ZNR film), the second layer (printed layer containing thin sheets), the easy-adhesive PET film, and the adhesive layer (A) in the example. A film was prepared from the sample film for evaluation, and after the film was bonded to the soda glass, a 90-degree peel test was performed to measure the adhesion between the layers. When the film was bonded to the soda glass, a 2kg roller was pressed back and forth from the film side at a speed of 300mm / min to apply pressure, and then left to stand for 20 minutes. In addition, the adhesion and tension were measured in an environment with a temperature of 22°C and a humidity of 50%.
[0317] Fig.13 It is a cross-sectional view schematically showing a method of measuring the adhesive force F1 between the first layer and the second layer in the example. Fig.14 It is a cross-sectional view schematically showing a method for measuring the adhesive force F2 between the second layer and the adhesive layer in the example. Fig.15 It is a cross-sectional view schematically showing a method for measuring the adhesive force F3 between the adhesive layer and the adherend in the example. Fig.16 It is a cross-sectional view schematically showing a method for measuring the adhesive force F4 between the first layer and the adhesive layer in the example.
[0318] (1. Measurement of Adhesion Force F1 between First Layer and Second Layer)
[0319] On one side of the ZNR film, a coating containing a sheet of the embodiment is used to manufacture a printed layer by screen printing. As a screen printing plate, an 80-mesh plate for full-surface printing is used. When manufacturing the printed layer, a space of about 10 mm is set from one end of the ZNR film, and the printed layer is manufactured outside the gap. Next, an adhesive layer (A) having a peeling layer on both sides is prepared, the peeling layer on one side is peeled off, and the adhesive layer (A) and the printed layer are laminated to make a sample film.
[0320] The obtained sample film was cut into a width of 10 mm. Fig.13 As shown, a film having a ZNR film (norbornene resin layer) 311b and a printed layer (second layer) 312 is obtained. At this time, the sample film is cut in a direction parallel to the width direction of the gap so that one end of the film has a gap. The peeling layer (not shown) of the film is peeled off, and the adhesive layer 314 of the film is bonded to the soda glass 220.
[0321] Next, the gap of the ZNR film 311b of the film sheet was sandwiched at the front end of the dynamometer 210, and the ZNR film 311b was pulled at a speed of 300 mm / min along the line direction of the surface of the soda glass 220, and the strength of the pulling force when the ZNR film 311b was peeled off from the printed layer 312 was measured as the adhesive force F1. The adhesive force F1 was 1.5 N / 10 mm.
[0322] (2. Measurement of Adhesion Force F2 between Second Layer and Adhesive Layer (A))
[0323] On one side of an easily adhesive PET film ("PET film A4100" manufactured by Toyobo Co., Ltd., hereinafter referred to as "PET film"), a coating containing the flakes of the embodiment was used to manufacture a printed layer by screen printing. As a screen printing plate, an 80-mesh plate for full-surface printing was used. When manufacturing the printed layer, the printed layer was manufactured on the entire surface of one side of the PET film. Next, an adhesive layer (A) with a peeling layer was prepared, and a gap of about 10 mm was set from one end of the printed layer, and the adhesive layer (A) and the printed layer were laminated to manufacture a sample film.
[0324] The obtained sample film was cut into a width of 10 mm. Fig.14 As shown in the figure, a film sheet having a PET film 320, a printing layer 312, and an adhesive layer (A) 314 is obtained. At this time, the sample film is cut in a direction parallel to the width direction of the gap so that one end of the film sheet has a gap. The peeling layer (not shown) of the film sheet is peeled off, so that the adhesive layer 314 of the film sheet is attached to the soda glass 220.
[0325] Next, the gap between the laminated portion of the PET film 320 and the printed layer 312 of the film sheet was sandwiched at the front end of the force gauge 210, and the laminated portion was pulled at a speed of 300 mm / min along the line direction of the surface of the soda glass 220, and the strength of the pulling force when the printed layer 312 was peeled off from the adhesive layer 314 was measured as the adhesive force F2. The adhesive force F2 was 5.8 N / 10 mm.
[0326] (3. Measurement of Adhesion Force F3 between Adhesive Layer (A) and Adherend)
[0327] A sample film was prepared by laminating the adhesive layer (A) on one side of a highly adhesive PET film.
[0328] The obtained sample film was cut into a width of 10 mm. Fig.15 As shown, a film having a PET film 320 and an adhesive layer (A) 314 is obtained. The peeling layer (not shown) of the film is peeled off, and the adhesive layer 314 of the film is bonded to the soda glass 220. At this time, a gap of about 10 mm is provided from one end of the short side of the film so as not to bond to the soda glass.
[0329] The gap between the laminated portion of the PET film 320 and the adhesive layer 314 of the film sheet was sandwiched at the front end of the dynamometer 210, and the laminated portion was pulled at a speed of 300 mm / min along the linear direction of the surface of the soda glass 220, and the strength of the pulling force when the adhesive layer (A) 314 was peeled off from the soda glass 220 was measured as the adhesive force F3. The adhesive force F3 was 7.8 N / 10 mm.
[0330] (4. Measurement of Adhesion Force F4 between First Layer and Adhesive Layer (A))
[0331] The adhesive layer (A) was attached to one side of the ZNR film to prepare a sample film, and a gap of about 10 mm was provided from one end of the ZNR film where the adhesive layer (A) was not attached.
[0332] The obtained sample film was cut into a width of 10 mm. At this time, the sample film was cut in a direction parallel to the width direction of the gap so that one end of the film had a gap. Fig.16 As shown, a film having a ZNR film 311b and an adhesive layer 314 is obtained. The release layer (not shown) of the film is peeled off, and the adhesive layer 314 of the film is bonded to the soda glass 220.
[0333] Next, the ZNR film 311b of the diaphragm was clamped in the gap at the front end of the dynamometer 210, and the ZNR film 311b was pulled at a speed of 300 mm / min along the line direction of the surface of the soda glass 220, and the strength of the pulling force when the ZNR film 311b was peeled off from the adhesive layer 314 was measured as the adhesive force F4. The adhesive force F4 was 2.3 N / 10 mm.
[0334] (5. Measurement of Tension T1 Due to Deformation of Adhesive Layer (A))
[0335] Fig.17 This is a cross-sectional view schematically showing a method of measuring the tension T1 for deforming the adhesive layer of the example.
[0336] The adhesive layer (A) having release layers on both sides was cut into a width of 10 mm. Fig.17 As shown, the peeling layers (not shown) on both sides of the adhesive layer sheet 314 are peeled off and bonded to the soda glass. At this time, a gap of about 10 mm is provided from one end of the short side of the adhesive layer sheet 314 so as not to bond to the soda glass 220.
[0337] Next, the gap of the adhesive layer 314 was sandwiched at the front end of the dynamometer 210, and the adhesive layer was pulled at a speed of 300 mm / min along the line direction of the surface of the soda glass 220, and the strength of the pulling force when the gap of the adhesive layer 314 began to stretch was measured as the tension T1. The tension T1 was 3.3 N / 10 mm.
[0338] The evaluation results are shown in Table 1.
[0339] [Table 1]
[0340] Table 1
[0341] 90 degree peel test results (N / 10mm) Adhesion F1 1.5 Adhesion force F 2 5.8 Adhesion F3 7.8 Adhesion force F 4 2.3 Tension T1 3.3
[0342] [Description of materials for the structural layers of the reagent and the recognition medium]
[0343] The reagents used in the following examples and the materials of the structural layer of the recognition medium are as follows.
[0344] As the photopolymerizable liquid crystal compound, a compound (X1) having the following structure was used.
[0345] [Chemical formula 5]
[0346]
[0347] As the photopolymerizable non-liquid crystal compound, a compound (X2) having the following structure was used.
[0348] [Chemical formula 6]
[0349]
[0350] As a chiral reagent, "LC756" manufactured by BASF was used.
[0351] As a photopolymerization initiator, "IRGACURE OXEO2" manufactured by Ciba Specialty Chemicals Japan Ltd. was used.
[0352] As a surfactant, "FTERGENT 209F" manufactured by Neos Corporation was used.
[0353] [Example]
[0354] [1. Production of cholesteric resin layer]
[0355] The cholesteric resin layer used in the manufacture of the identification medium of the examples and comparative examples was manufactured using a photocurable liquid crystal composition prepared by the method shown below. The cholesteric resin layer was used as the first layer in some cases, and was crushed into flakes in other cases and used as a pigment for the coating material forming the second layer.
[0356] (Preparation of Photocurable Liquid Crystal Composition)
[0357] A photocurable liquid crystal composition was prepared by mixing 21.9 parts of a photopolymerizable liquid crystal compound, 5.47 parts of a photopolymerizable non-liquid crystal compound, 1.69 parts of a chiral agent, 0.9 parts of a photopolymerization initiator, 0.03 parts of a surfactant, and 70 parts of cyclopentanone.
[0358] (Manufacture of a multilayer film having a cholesteric resin layer)
[0359] As a support, a polyethylene terephthalate film ("PET film A4100" manufactured by Toyobo Co., Ltd.; thickness 100 μm, hereinafter referred to as "PET film") having an isotropic refractive index in the plane was prepared. The PET film was mounted on the delivery portion of the film conveying device, and the following operations were performed while the PET film was conveyed in the length direction. First, a friction treatment was applied in the length direction parallel to the conveying direction. Next, a die coater was used to apply the prepared liquid crystal composition to the surface subjected to the friction treatment. Thus, a film of the liquid crystal composition in an uncured state was formed on one side of the PET film. The film of the liquid crystal composition in an uncured state was subjected to an orientation treatment at 120°C for 4 minutes.
[0360] The film after the orientation treatment was subjected to the first ultraviolet irradiation treatment (illuminance: 5 mJ / cm 2 , 1 minute), first heat treatment (100°C, 1 minute), second ultraviolet irradiation treatment (illuminance: 30 mJ / cm 2 After the second heat treatment (100°C, 1 minute), the film of the liquid crystal composition was irradiated with 800 mJ / cm 2 The film of the liquid crystal composition was completely cured by ultraviolet rays. Thus, a multilayer film having a cholesteric resin layer with a thickness of 5.2 μm on one side of the long PET film was obtained.
[0361] [2. Manufacture of coating material using flakes]
[0362] A release sheet having a cholesteric resin layer is prepared by using the multilayer film having a cholesteric resin layer produced by the above-mentioned steps. As an apparatus for producing a release sheet, a Fig.18 The device shown. Fig.18 The figure is a side view schematically showing an apparatus for manufacturing a release sheet of a cholesteric resin layer.
[0363] like Fig.18 As shown in FIG. 1 , a manufacturing device 400 having a film delivery unit 420, a stripping unit 430, and a film recovery unit 440 is prepared. The stripping unit 430 has a long block 434 having an acute angled corner 435, and a nozzle 436, which is disposed immediately downstream of the corner 435 and can eject air. At this time, the angle of the corner 435 of the long block 434 is set so that the multilayer film 410 is folded back at an angle θ (45°). The corner is a chamfered structure with R = 0.2 mm to 0.3 mm.
[0364] The multilayer film 410 is installed in the film delivery section 420 in such a direction that the cholesteric resin layer 411 is positioned outside the PET film 412 at the corner portion 435 of the long strip 434 and the multilayer film 410 is folded back. Then, the multilayer film 410 is delivered from the film delivery section 420 while tension is applied to the multilayer film 410 in the conveying direction by the film recovery section 440. At this time, the magnitude of the tension applied to the multilayer film 410 is set to 80 N / m. In addition, air is sprayed from the nozzle 436 at a pressure of 0.5 MPa.
[0365] The multilayer film 410 is folded back at the corner portion 435 of the long strip 434 to form a plurality of cracks. Then, the cholesteric resin layer 411 with the cracks is peeled off and blown off by air ejected from the nozzle 436 to obtain a peeling sheet 411A. The obtained peeling sheet 411A is recovered by a recovery device.
[0366] (Manufacturing of thin sheets)
[0367] The recovered peeled pieces of the cholesteric resin layer were pulverized using a mortar mill ("micro·powder-MPW-G008" manufactured by WEST Co., Ltd.) to obtain flakes. The volume average particle size (D50) of the obtained flakes was 78 μm, and the area ratio of the bottom area to the side area on one side of the flakes was 1.78.
[0368] (Manufacture of paint)
[0369] The obtained flakes were used as a cholesteric resin layer pigment. A coating was obtained by mixing 10 parts of screen ink ("S240-800" manufactured by Seiko Ink Co., Ltd.: refractive index 1.49) as a binder solution (medium), 0.5 parts of a diluent solvent ("T472" manufactured by Seiko Ink Co., Ltd.), and 1 part of the above-mentioned flakes.
[0370] [3. Manufacture of identification medium]
[0371] The above-mentioned multilayer film having a cholesteric resin layer and a PET film, and a resin film as a layer containing a norbornene-based polymer (("ZF16-100" manufactured by Zeon Co., Ltd.; thickness 100 μm, ZNR film) were prepared. A UV curing adhesive ("UVX-6298" manufactured by Toagosei Co., Ltd.) was applied on the cholesteric resin layer of the multilayer film, and the ZNR film was attached, and irradiated with 350 mJ / cm from the above-mentioned ZNR film side. 2 The UV curing adhesive was cured by applying ultraviolet light. Next, the PET film was peeled off from the multilayer film. Through the above steps, a laminate of a cholesteric resin layer, a UV curing adhesive layer (thickness 2 μm), and a ZNR film was obtained.
[0372] On both sides of the above-mentioned laminate, screen printing is performed using the above-mentioned coating containing thin sheets. As a plate for screen printing, a 80-mesh screen with a text pattern is prepared. Then, the laminate of the cholesteric resin layer and the printed layer is heated on a hot plate at 80°C for 10 minutes to dry the coating, thereby obtaining an identification medium. The printed layers (second and third layers) arranged on the surface and back of the above-mentioned laminate have patterns of different texts, respectively. In addition, the area of the thin sheet group of each printed layer (second and third layers) accounts for 59.2% of the unit area of the layer.
[0373] On the surface of the cholesteric resin layer side of the laminate with a printed layer, a protective film with an adhesive layer ("TACKTITLE protective film" manufactured by Kokuyo Co., Ltd.) is laminated. In addition, an adhesive layer (A) with a release layer is prepared ("double-sided adhesive film OCA100" manufactured by IDcreate Co., Ltd.). The above-mentioned adhesive layer (A) with a release layer is an acrylic adhesive without a substrate, and has a structure in which a release layer, an adhesive layer (A) and a release layer are sequentially laminated. One of the release layers of the adhesive layer (A) with a release layer is peeled off, and the adhesive layer (A) is laminated on the surface of the ZNR film side of the laminate with a printed layer. Through the above steps, an identification medium with a release layer is obtained.
[0374] [4. Attachment and removal of identification medium to adherend]
[0375] The peeling layer of the obtained identification medium was peeled off, and the adhesive layer (A) was pasted on the soda glass. The attached identification medium was observed, and the pattern of the text on the front and back sides was different. In addition, it was not confirmed that the printing layer set on the other side was penetrated from one side.
[0376] Then, the identification medium was peeled off from the soda glass, and it was confirmed that the identification medium was separated at the interface between the first layer and the second layer, and the second layer and the adhesive layer (A) remained on the soda glass. Next, the remaining adhesive layer was peeled off, and it was confirmed that the adhesive layer (A) stretched during the peeling process, and the shape of the text pattern of the second layer was destroyed.
[0377] Description of Reference Numerals
[0378] 10, 100: Identification medium
[0379] 11, 111: First floor
[0380] 12, 112: Second floor
[0381] 12f, 112f, 113f: Thin sheets
[0382] 14, 114, 314: Adhesive layer (A)
[0383] 15, 115: Adhesive layer
[0384] 16, 116: Protective layer
[0385] 20, 220: Adhesive
[0386] 111a: Cholesteric resin layer
[0387] 111b: norbornene-based resin layer
[0388] 111c: Adhesive layer
[0389] 113: Third floor
[0390] 210: Dynamometer
[0391] 311b: Norbornene-based resin layer (ZNR film)
[0392] 312: Second layer (printing layer)
[0393] 320: PET film
[0394] 400: Apparatus for manufacturing a release sheet of a cholesteric resin layer
[0395] 410: Multilayer film
[0396] 411: Cholesteric resin layer
[0397] 412: Support (PET film)
[0398] 411A: Peel-off
[0399] 420: Film delivery department
[0400] 430: Stripping section
[0401] 434: Long strip
[0402] 435: Corner of the long strip
[0403] 436: Nozzle
[0404] 440: Membrane recovery department
Claims
1. An identification medium, comprising: First floor; a second layer disposed overlapping the first layer; and a bonding layer disposed on the second layer; The first layer is a layer capable of reflecting one of right-handed circularly polarized light or left-handed circularly polarized light and transmitting the other circularly polarized light, and the first layer includes a layer of a resin having cholesteric regularity. The second layer is a layer capable of reflecting at least a portion of circularly polarized light having the same rotation direction as the circularly polarized light reflected by the first layer and transmitting circularly polarized light having a rotation direction opposite to the circularly polarized light reflected by the first layer, and the second layer is a layer comprising a flake of a resin having cholesteric regularity, When the adhesive layer is attached to an adherend, the adhesive force F1 between the first layer and the second layer, the adhesive force F2 between the second layer and the adhesive layer, and the adhesive force F3 between the adhesive layer and the adherend satisfy the relationship between the following equations (1) and (2): F1<F2 (1) F1<F3 (2).
2. The identification medium according to claim 1, wherein: The tension T1 that causes the adhesive layer to deform and the adhesive force F3 between the adhesive layer and the adherend satisfy the relationship of the following formula (3): T1<F3 (3).
3. The identification medium according to claim 1, wherein: The second layer is a layer provided on a portion of the surface of the first layer, The bonding layer is a layer disposed on the first layer and the second layer, When the adhesive layer is attached to an adherend, the adhesive force F3 between the adhesive layer and the adherend, and the adhesive force F4 between the first layer and the adhesive layer satisfy the relationship of the following formula (4): F4<F3 (4).
4. The identification medium according to claim 1, wherein: The identification medium includes a third layer, the third layer being provided on a surface of the first layer opposite to a surface on which the second layer is provided so as to overlap with the first layer. The third layer is a layer capable of transmitting circularly polarized light having a rotation direction opposite to that of the circularly polarized light reflected by the first layer, and is a layer including a flake of a resin having cholesteric regularity.
5. The identification medium according to claim 1, wherein The volume average particle size D50 of the flakes of the resin having cholesteric regularity is 70 μm or more.
6. The identification medium according to claim 1, wherein The first layer is a laminate of a layer of the resin having cholesteric regularity and a layer containing a norbornene-based resin.
7. The identification medium according to claim 1, wherein: The adherend is transparent glass.
8. The identification medium according to claim 1, wherein When the identification medium is peeled off after being attached to the adherend, the laminated portion of the second layer and the adhesive layer is separated from the first layer.
9. The identification medium according to claim 8, wherein: When the adhesive layer of the laminated portion separated from the identification medium is peeled off from the adherend, the adhesive layer is deformed and the second layer is destroyed. 10 . An article comprising the identification medium according to claim 1 and an adherend to which the identification medium is adhered.