Oxidation-Ugi reaction alginic acid derivative / modified kaolin compound synergistically stable drug-loaded Pickering emulsion and preparation method thereof
Through the synergistic stabilization of oxidation-Ugi reaction alginic acid derivatives and modified kaolin complexes, the problem of poor stability of Pickering emulsions is solved, and a hydrophobic pesticide emulsion with high stability and high loadability is achieved, which is suitable for environmentally friendly pesticide formulations. Reduced production costs.
Patent Information
- Application Number
- CN202410778982.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-18
AI Technical Summary
It is difficult to form a stable Pickering emulsion with the existing technology, especially due to the insufficient hydrophilicity or lipophilicity of natural surface-active particles, resulting in poor emulsion stability, and the cyclohexyl isonitrile used in the traditional Ugi four-component reaction is not environmentally friendly and limits the use of alginic acid. Application of salt-based polymers in industrial production.
Oxidation-Ugi reaction alginic acid derivatives and modified kaolin complexes are used to form a highly stable Pickering emulsion through the synergistic stabilization of Ugi-OSAOcT and MKL. Ultrasonic dispersion and shear emulsification technology are used to construct hydrophobic pesticide carriers.
A hydrophobic pesticide emulsion with high stability and high loadability is achieved, which has good sustained and controlled release properties, expands the application scope of environmentally friendly pesticide carriers, and reduces the amount of emulsifier and production cost.
Smart Images

Figure CN118786991A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of pesticide carrier materials, and particularly relates to a drug-loaded Pickering emulsion synergistically stabilized by an oxidation-Ugi reaction alginate derivative / modified kaolin composite and a preparation method thereof. Background Art
[0002] Pickering emulsion is a thermodynamically unstable dispersion system composed of two immiscible liquid phases using surfactant particles as emulsifiers. The main factors affecting the stability of Pickering emulsions include particle surface wettability, particle concentration, continuous phase ionic strength and pH value, among which particle surface wettability (particle surface activity) has the most significant effect on the stability of Pickering emulsions. Since there are few natural surfactant particles, it is difficult to form a stable Pickering emulsion, which limits the discovery and development of Pickering emulsions. Nanoparticles such as various nano-oxides, polymer colloids, calcium carbonate particles, clays, and nano-carbon black used as Pickering emulsifiers are either too hydrophilic or too lipophilic. Only nanoparticles with suitable surface wettability can gather at the liquid-liquid or liquid-gas interface to form a stable emulsion. Therefore, in order to change its surface wettability, it is usually necessary to modify its surface or synergistically mix it with surfactants.
[0003] In recent years, new Pickering emulsions stabilized by "soft particles" formed by amphiphilic polymers / solid particles have met people's special requirements in industry, medicine and emerging industries. The new soft particle emulsifier combines the dual advantages of amphiphilic polymers and solid particles, so it has obvious stability advantages in stabilizing Pickering emulsions, thus expanding the basic research and application of emulsions. The dominant factor in emulsion stability is the interfacial behavior and properties, and the fundamental reason is caused by the particle emulsifier itself, so the development of new polymers / solid particles has attracted the attention of researchers.
[0004] Sodium alginate (SA) is a polyanionic natural polymer material. It is widely used in biomedicine due to its wide source, renewable, non-toxic, degradable and good biocompatibility. By periodate oxidation modification of alginate, the C2-C3 bond on the polysaccharide monomer can be broken to form a highly active aldehyde group. The Ugi four-component (Ugi-4CR) reaction is a multi-component reaction involving ketone or aldehyde, amine, carboxylic acid and isocyanide. It has the advantages of powerful function, simple operation, low cost, simple and efficient, no catalyst, good atom economy, etc. However, the current literature reports basically use toxic, odorous and expensive flammable liquid cyclohexyl isonitrile to prepare alginate-based polymers through the Ugi four-component (Ugi-4CR) reaction, which is not conducive to environmental protection and health, nor to industrial production. In addition, the preparation of alginate-based polymers and solid particles for synergistic stabilization of Pickering emulsions cannot obtain Pickering emulsions with high stability.
[0005] Therefore, there is an urgent need for an alginate-based polymer / solid particle that can improve the Pickering emulsion to solve the above problems. Summary of the invention
[0006] In order to solve the above technical problems, the present invention proposes a drug-loaded Pickering emulsion synergistically stabilized by an oxidation-Ugi reaction alginate derivative / modified kaolin composite and a preparation method thereof.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a drug-loaded Pickering emulsion synergistically stabilized by an oxidation-Ugi reaction alginate derivative / modified kaolin composite, comprising the following steps:
[0009] (1) adding octylamine, glacial acetic acid, and p-toluenesulfonylmethyl isocyanide to a sodium periodate oxidized alginate derivative solution in sequence to carry out Ugi reaction, and obtaining an oxidized-Ugi reaction alginate derivative Ugi-OSAOcT through precipitation, centrifugation, dialysis, and freeze drying;
[0010] (2) mixing kaolin and dimethylpolysiloxane, ball milling, washing and freeze-drying to obtain modified kaolin MKL;
[0011] (3) mixing the oxidized-Ugi reaction alginic acid derivative Ugi-OSAOcT obtained in step (1) and the modified kaolin MKL obtained in step (2) to obtain a Ugi-OSAOcT / MKL complex; adding the Ugi-OSAOcT / MKL complex into water, dispersing by ultrasonication and allowing to stand by shaking to obtain a Ugi-OSAOcT / MKL complex suspension;
[0012] (4) using the oil containing the hydrophobic pesticide as the oil phase and the Ugi-OSAOcT / MKL complex suspension obtained in step (3) as the water phase, mixing the two and then shearing and emulsifying them to obtain an oxidation-Ugi reaction alginate derivative / modified kaolin complex synergistically stabilized drug-loaded Pickering emulsion;
[0013] There is no order of precedence for steps (1) and (2).
[0014] Preferably, in step (1), the molar ratio of the uronic acid monomer of the sodium periodate oxidized alginate derivative to octylamine, glacial acetic acid and p-toluenesulfonylmethyl isocyanide in the sodium periodate oxidized alginate derivative solution is (1:2:2:2.2)-(1:2.8:2.8:3.1).
[0015] Preferably, in step (2), the amount of dimethylpolysiloxane used is 0.5-2.0% of the mass of kaolin.
[0016] Preferably, in step (2), the medium of the ball mill is steel balls, the rotation speed is 516 r / min, and the time is 1 h; when the amount of kaolin used is 3.00-6.00 g, the balls used for the ball mill are: 2 steel balls with a diameter of 20 mm, 10 steel balls with a diameter of 10 mm, and 10 steel balls with a diameter of 6 mm.
[0017] Preferably, in step (3), the mass ratio of the oxidized-Ugi reaction alginate derivative Ugi-OSAOcT and the modified kaolin MKL in the Ugi-OSAOcT / MKL complex is (1:2)-(1:10).
[0018] Preferably, in step (3), the mass fraction of the Ugi-OSAOcT / MKL complex in the Ugi-OSAOcT / MKL complex suspension is 0.5-2.5%.
[0019] Preferably, in step (4), the hydrophobic pesticide includes one of cyhalothrin, bifenthrin and emamectin benzoate; and the oil includes one of xylene, toluene and liquid paraffin.
[0020] Preferably, in step (4), the concentration of the hydrophobic pesticide in the oil containing the hydrophobic pesticide is 0.5-5.0 mg / mL.
[0021] Preferably, in step (4), the volume ratio of the oil containing the hydrophobic pesticide to the Ugi-OSAOcT / MKL complex suspension is (2:8)-(5:5).
[0022] The present invention also provides a drug-loaded Pickering emulsion prepared by the preparation method described in the above technical solution and synergistically stabilized by an oxidation-Ugi reaction alginate derivative / modified kaolin complex.
[0023] Compared with the prior art, the present invention has the following advantages and technical effects:
[0024] The present invention adopts green, mild conditions and high yield Ugi reaction to prepare amphiphilic Ugi-OSAOcT, and uses dry ball milling to prepare MKL with interfacial activity. By organically combining the two, the synergistic effect and hydrophobic association self-assembly behavior between the two are utilized to construct a Pickering emulsion with high stability that can load hydrophobic pesticides, and expand the application range of the Pickering emulsion formed by natural modified polymer surfactants and mineral soil particles as an environmentally friendly new hydrophobic pesticide drug carrier. In addition, the Pickering emulsion synergistically stabilized by the Ugi-OSAOcT / MKL complex has a high encapsulation rate for hydrophobic pesticides and exhibits good slow-release performance, and can be used as an environmentally friendly pesticide formulation for the field of agricultural pest control. This drug carrier developed with natural polysaccharide macromolecules and clay minerals as raw materials provides a scientific basis and corresponding technology for the development and utilization of renewable resources and the research and development of new functionalized pesticide carriers.
[0025] Compared with traditional emulsions, the synergistically stabilized drug-loaded Pickering emulsion prepared by the oxidation-Ugi reaction alginate derivative / modified kaolin complex of the present invention has the following advantages: (1) the amount of emulsifier used is small, the source is wide, the price is low, and it is conducive to industrial production; (2) the solid particles are inorganic mineral soil particles and biological macromolecules, which have the characteristics of small toxic side effects, no foam, easy degradation, and environmental protection; (3) good stability, strong adsorption of solid particles at the oil-water interface, which can effectively prevent the emulsion from destabilizing; (4) it has a high loading capacity and good slow-release performance for hydrophobic pesticides. Therefore, the synergistically stabilized drug-loaded Pickering emulsion prepared by the oxidation-Ugi reaction alginate derivative / modified kaolin complex of the present invention has extremely high application value and development prospects in the field of environmentally friendly pesticide formulation development. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0027] Figure 1 The synthetic route of Ugi-OSAOcT in Examples 1-3 of the present invention;
[0028] Figure 2FT-IR spectra of ammonium alginate SA, sodium periodate oxidized alginate derivative OSA, Ugi-OSA10OcT in Example 1, Ugi-OSA30OcT in Example 2, Ugi-OSA50OcT in Example 3, octylamine OCA, and a mixture of octylamine OCA and sodium periodate oxidized alginate derivative OSA;
[0029] Figure 3 is octylamine OCA (CDCl3) (a), p-toluenesulfonylmethyl isocyanide TOSMIC (D2O) (b), sodium alginate SA (D2O) (c), sodium periodate oxidized alginate derivative OSA (D2O) (d), Ugi-OSA10OcT in Example 1 (D2O) (e), Ugi-OSA30OcT in Example 2 (D2O) (f) and Ugi-OSA50OcT in Example 3 (D2O) (g) 1 H NMR spectrum;
[0030] Figure 4 The graph (A) shows the relationship between the concentration of Ugi-OSA10OcT in Example 1, the Ugi-OSA30OcT in Example 2, and the Ugi-OSA50OcT in Example 3 and the ratio I1 / I3 of the fluorescence intensity of pyrene, and the graph (B) shows the change of CMC value with the substitution degree of polymer Ugi-OSAOcT;
[0031] Figure 5 FT-IR spectra (a) and XRD spectra (b) of the raw kaolin and modified kaolin MKL in Example 1;
[0032] Figure 6 The scanning electron microscope images and transmission electron microscope images of the kaolin and modified kaolin MKL in Example 1;
[0033] Figure 7 The particle size distribution diagram (a) and zeta potential distribution diagram (b) of kaolin and modified kaolin MKL in Example 1;
[0034] Figure 8 Physical images of contact angles of kaolin (a) and modified kaolin MKL (b) in Example 1;
[0035] Fig. 9 A schematic diagram of the drug-loaded Pickering emulsion synergistically stabilized by the Ugi-OSAOcT / MKL complex prepared in the present invention and its stabilizing mechanism;
[0036] Fig.10 The actual picture of the Pickering emulsion synergistically stabilized by the Ugi-OSAOcT / MKL complex prepared in Comparative Example 1, Example 1, and Examples 4-7;
[0037] Fig.11 The droplet morphology of the Pickering emulsion synergistically stabilized by the Ugi-OSAOcT / MKL complex prepared in Comparative Example 1, Example 1, and Examples 4-7;
[0038] Fig.12 The droplet morphology (a) and schematic diagram (b) of the Pickering emulsion synergistically stabilized by the Ugi-OSAOcT / MKL complex in Example 1;
[0039] Fig.13 This is the in vitro cumulative release curve of the drug-loaded Pickering emulsion synergistically stabilized by chlorofluorocyanate LF and the Ugi-OSAOcT / MKL complex in Example 1-3 in PBS at pH = 7.4 at 37°C. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0042] The embodiment of the present invention provides a method for preparing a drug-loaded Pickering emulsion synergistically stabilized by an oxidation-Ugi reaction alginate derivative / modified kaolin composite, comprising the following steps:
[0043] (1) adding octylamine, glacial acetic acid, and p-toluenesulfonylmethyl isocyanide to a sodium periodate oxidized alginate derivative solution in sequence to carry out Ugi reaction, and obtaining an oxidized-Ugi reaction alginate derivative Ugi-OSAOcT through precipitation, centrifugation, dialysis, and freeze drying;
[0044] (2) mixing kaolin and dimethylpolysiloxane, ball milling, washing and freeze-drying to obtain modified kaolin MKL;
[0045] (3) mixing the oxidized-Ugi reaction alginic acid derivative Ugi-OSAOcT obtained in step (1) and the modified kaolin MKL obtained in step (2) to obtain a Ugi-OSAOcT / MKL complex; adding the Ugi-OSAOcT / MKL complex into water, dispersing by ultrasonication and allowing to stand by shaking to obtain a Ugi-OSAOcT / MKL complex suspension;
[0046] (4) using the oil containing the hydrophobic pesticide as the oil phase and the Ugi-OSAOcT / MKL complex suspension obtained in step (3) as the water phase, mixing the two and then shearing and emulsifying them to obtain an oxidation-Ugi reaction alginate derivative / modified kaolin complex synergistically stabilized drug-loaded Pickering emulsion;
[0047] There is no order of precedence for steps (1) and (2).
[0048] In a preferred embodiment, in step (1), the preparation method of the sodium periodate oxidized alginate derivative comprises the following steps: dissolving 5 g of sodium alginate SA in 200 mL of distilled water, adding 50 mL of anhydrous ethanol and mixing evenly, then adding sodium periodate, stirring electrically in the dark for 24 h at room temperature, then adding 10 mL of ethylene glycol, stirring magnetically in the dark for 2 h to terminate the reaction; precipitating the reaction solution with 5 g of sodium chloride and 800 mL of anhydrous ethanol, then re-dissolving the obtained precipitate in 100 mL of distilled water, and then precipitating with 3 g of sodium chloride and 600 mL of anhydrous ethanol, repeating the precipitation 3 times, and placing the obtained solution into a dialysis bag with a molecular weight cutoff of 3500 for 5 days, and freeze-drying to obtain the sodium periodate oxidized alginate derivative OSA.
[0049] In a preferred embodiment, the mass average molecular weight Mw of the sodium alginate is ≤200000, and the molar ratio of guluronic acid (G) to mannuronic acid (M) in the sodium alginate is G / M ≤1.0.
[0050] In a preferred embodiment, the mass ratio of sodium alginate to sodium periodate is 5:(0.54-2.68).
[0051] In a preferred embodiment, the theoretical degree of oxidation of the alginate derivative OSA by sodium periodate is 10%, 30% or 50%.
[0052] In a preferred embodiment, in step (1), the mass fraction of the sodium periodate-oxidized alginate derivative solution is 1.0% (m / v).
[0053] In a preferred embodiment, in step (1), the molar ratio of the uronic acid monomer of the sodium periodate oxidized alginate derivative to octylamine, glacial acetic acid and p-toluenesulfonylmethyl isocyanide in the sodium periodate oxidized alginate derivative solution is (1:2:2:2.2)-(1:2.8:2.8:3.1). The p-toluenesulfonylmethyl isocyanide in the present invention is a stable solid with almost no special odor and can be stored at room temperature without decomposition, and has a low price.
[0054] In a preferred embodiment, in step (1), the degree of substitution of the oxidation-Ugi reaction alginate derivative Ugi-OSAOcT is 4.8-24.3%, more preferably 4.8-14.8%. The present invention controls the degree of substitution of the oxidation-Ugi reaction alginate derivative Ugi-OSAOcT within the above range, which has better hydrophilicity and lipophilicity.
[0055] In a preferred embodiment, the degree of substitution of the oxidation-Ugi reaction alginate derivative Ugi-OSAOcT is calculated as follows:
[0056]
[0057] Among them, α is the content ratio of N / C, M C and M N are the relative atomic masses of C and N respectively.
[0058] In a preferred embodiment, in step (1), the reagent used for precipitation is anhydrous ethanol; the molecular weight cutoff of the dialysis bag used for dialysis is 3500, the dialysis fluid is deionized water, and the dialysis time is 3 days; the temperature of the freeze-drying is -60 to -50°C, and the time is 48 hours.
[0059] In a preferred embodiment, in step (2), the kaolin is pre-treated by drying the kaolin raw material in an oven at 105° C. to a constant weight.
[0060] In a preferred embodiment, in step (2), the amount of dimethicone used is 0.5-2.0% of the mass of kaolin, more preferably 1.0-2.0%.
[0061] In a preferred embodiment, in step (2), the medium for ball milling is steel balls, the rotation speed is 516 r / min, and the time is 1 h; when the amount of kaolin used is 3.00-6.00 g, the balls for ball milling are: 2 steel balls with a diameter of 20 mm, 10 steel balls with a diameter of 10 mm, and 10 steel balls with a diameter of 6 mm; the equipment for ball milling is a PM type planetary ball mill.
[0062] In a preferred embodiment, in step (2), the washing reagents are petroleum ether and deionized water; the freeze-drying temperature is -60 to -50°C, and the time is 48 hours.
[0063] In a preferred embodiment, in step (3), the mass ratio of the oxidized-Ugi reaction alginate derivative Ugi-OSAOcT and the modified kaolin MKL in the Ugi-OSAOcT / MKL complex is (1:2)-(1:10), (1:5)-(1:10).
[0064] In a preferred embodiment, in step (3), the power of the ultrasonic dispersion is 100-200 W, and the method is probe ultrasound; and the oscillation and static time is more than 24 hours.
[0065] In a preferred embodiment, in step (3), the mass fraction of the Ugi-OSAOcT / MKL complex in the Ugi-OSAOcT / MKL complex suspension is 0.5-2.5%, more preferably 0.5-2.0%.
[0066] In a preferred embodiment, in step (4), the hydrophobic pesticide includes one of cyfluthrin, bifenthrin and avermectin benzoate, more preferably cyfluthrin; the oil includes one of xylene, toluene and liquid paraffin, more preferably xylene.
[0067] In a preferred embodiment, in step (4), the concentration of the hydrophobic pesticide in the oil containing the hydrophobic pesticide is 0.5-5.0 mg / mL, more preferably 2.0-5.0 mg / mL.
[0068] In a preferred embodiment, in step (4), the volume ratio of the oil containing the hydrophobic pesticide to the Ugi-OSAOcT / MKL complex suspension is (2:8)-(5:5), more preferably (3:7)-(5:5).
[0069] The present invention also provides a drug-loaded Pickering emulsion prepared by the preparation method described in the above technical solution and synergistically stabilized by an oxidation-Ugi reaction alginate derivative / modified kaolin complex.
[0070] The drug-loaded Pickering emulsion synergistically stabilized by the oxidation-Ugi reaction alginate derivative / modified kaolin composite provided by the present invention has the advantages of good stability, high loading capacity for hydrophobic pesticides and good sustained-release performance.
[0071] The room temperature in the embodiments of the present invention refers to "25±2°C".
[0072] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.
[0073] Example 1
[0074] A method for preparing a drug-loaded Pickering emulsion synergistically stabilized by an oxidation-Ugi reaction alginate derivative / modified kaolin complex:
[0075] (1) 5 g of sodium alginate SA was dissolved in 200 mL of distilled water, and then 50 mL of anhydrous ethanol was added to mix well, and then 0.54 g of sodium periodate was added, and the mixture was stirred electrically in the dark for 24 h at room temperature, and then 10 mL of ethylene glycol was added, and the mixture was stirred magnetically in the dark for 2 h to terminate the reaction; the solution after the reaction was precipitated with 5 g of sodium chloride and 800 mL of anhydrous ethanol, and then the precipitate was redissolved in 100 mL of distilled water, and then precipitated with 3 g of sodium chloride and 600 mL of anhydrous ethanol, and the precipitation was repeated 3 times. The resulting solution was placed in a dialysis bag with a molecular weight cutoff of 3500, dialyzed for 5 days, and freeze-dried to obtain a sodium periodate oxidized alginate derivative with a theoretical oxidation degree of 10%, which was recorded as OSA10;
[0076] (2) 2.0 g (containing 10.1 mmol uronic acid monomer) of OSA10 obtained in step (1) was placed in a 250 mL three-necked flask, 200 mL of deionized water was added, and mechanical stirring was performed to obtain an OSA10 solution with a mass fraction of 1.0% (m / v), and then 4.01 mL (24.0 mmol) of octylamine was added, and the mixture was stirred at room temperature for 30 min, and then 1.72 mL (30.0 mmol) of glacial acetic acid was added, and 5.58 g (33.0 mmol) of p-toluenesulfonylmethyl isonitrile TOSMIC was added at the same time, and the mixture was stirred at room temperature for 12 h, and then 1 L of anhydrous methanol was added to the reaction solution for precipitation. After centrifugation, the precipitate was placed in a dialysis bag with a molecular weight cutoff of 3500, and dialyzed with deionized water for 3 days to remove residual small molecular impurities, and then freeze-dried at -60°C for 48 h to obtain Ugi-OSA10OcT with a degree of substitution DS of 4.8%;
[0077] (3) 3.00 g of kaolin raw material was first dried in an oven at 105°C to constant weight, then mixed with 0.03 g of dimethylpolysiloxane, and ball milled using a PM planetary ball mill with steel balls as the ball milling medium. The balls were: 2 steel balls with a diameter of 20 mm, 10 steel balls with a diameter of 10 mm, and 10 steel balls with a diameter of 6 mm. The main disk rotated at 516 r / min and ball milled for 1 h. The ball milled product was then washed with petroleum ether and deionized water, respectively, and freeze-dried at -60°C for 48 h to obtain MKL.
[0078] (4) mixing the Ugi-OSAOcT obtained in step (2) and the MKL obtained in step (3) at a mass ratio of 1:10 to obtain a Ugi-OSAOcT / MKL complex; then adding the Ugi-OSAOcT / MKL complex into deionized water and performing ultrasonic dispersion at 100 W, and then shaking and standing for more than 24 hours to obtain a Ugi-OSAOcT / MKL complex suspension with a mass fraction of 1.0%;
[0079] (5) Dissolving chlorofluorocyanate (LF) in xylene to obtain chlorofluorocyanate-containing xylene at a concentration of 4.0 mg / mL, using the chlorofluorocyanate-containing xylene as the oil phase and the Ugi-OSAOcT / MKL complex suspension obtained in step (4) as the aqueous phase, mixing the two in a volume ratio of 3:7, and then subjecting the mixture to high-speed shearing at 12000 r / min for 5 min at room temperature using an emulsifier to obtain a Ugi-OSAOcT / MKL complex synergistically stabilized drug-loaded Pickering emulsion.
[0080] Example 2
[0081] A method for preparing a drug-loaded Pickering emulsion stabilized by an oxidation-Ugi reaction alginate derivative / modified kaolin complex:
[0082] (1) 5 g of sodium alginate SA was dissolved in 200 mL of distilled water, and then 50 mL of anhydrous ethanol was added to mix well, and then 1.60 g of sodium periodate was added, and the mixture was stirred electrically in the dark for 24 h at room temperature, and then 10 mL of ethylene glycol was added, and the mixture was stirred magnetically in the dark for 2 h to terminate the reaction; the solution after the reaction was precipitated with 5 g of sodium chloride and 800 mL of anhydrous ethanol, and then the precipitate was redissolved in 100 mL of distilled water, and then precipitated with 3 g of sodium chloride and 600 mL of anhydrous ethanol, and the precipitation was repeated 3 times. The resulting solution was placed in a dialysis bag with a molecular weight cutoff of 3500, dialyzed for 5 days, and freeze-dried to obtain a sodium periodate oxidized alginate derivative with a theoretical oxidation degree of 30%, which was recorded as OSA30;
[0083] (2) 2.0 g (containing 10.1 mmol uronic acid monomer) of OSA30 obtained in step (1) was placed in a 250 mL three-necked flask, 200 mL of deionized water was added, and mechanical stirring was performed to obtain an OSA30 solution with a mass fraction of 1.0% (m / v), and then 4.01 mL (24.0 mmol) of octylamine was added, and the mixture was stirred at room temperature for 30 min, and then 1.72 mL (30.0 mmol) of glacial acetic acid was added, and 5.58 g (33.0 mmol) of p-toluenesulfonylmethyl isonitrile TOSMIC was added at the same time, and the mixture was stirred at room temperature for 12 h, and then 1 L of anhydrous methanol was added to the reaction solution for precipitation. After centrifugation, the precipitate was placed in a dialysis bag with a molecular weight cutoff of 3500, and dialyzed with deionized water for 3 days to remove residual small molecular impurities, and then freeze-dried at -60°C for 48 h to obtain Ugi-OSA30OcT with a degree of substitution DS of 14.8%;
[0084] (3) 3.00 g of kaolin raw material was first dried in an oven at 105°C to constant weight, then mixed with 0.06 g of dimethylpolysiloxane, and ball milled using a PM planetary ball mill with steel balls as the ball milling medium. The balls were: 2 steel balls with a diameter of 20 mm, 10 steel balls with a diameter of 10 mm, and 10 steel balls with a diameter of 6 mm. The main disk rotated at 516 r / min and ball milled for 1 h. The ball milled product was then washed with petroleum ether and deionized water, respectively, and freeze-dried at -60°C for 48 h to obtain MKL.
[0085] (4) The Ugi-OSAOcT obtained in step (2) and the MKL obtained in step (3) were mixed at a mass ratio of 1:10 to obtain a Ugi-OSAOcT / MKL complex; the Ugi-OSAOcT / MKL complex was then added to deionized water and ultrasonically dispersed at 100 W, and then shaken and allowed to stand for more than 24 hours to obtain a Ugi-OSAOcT / MKL complex suspension with a mass fraction of 2.0%;
[0086] (5) Dissolving chlorofluorocyanate (LF) in xylene to obtain chlorofluorocyanate-containing xylene at a concentration of 5.0 mg / mL, using the chlorofluorocyanate-containing xylene as the oil phase and the Ugi-OSAOcT / MKL complex suspension obtained in step (4) as the aqueous phase, mixing the two in a volume ratio of 3:7, and then subjecting the mixture to high-speed shearing at 12000 r / min for 5 min at room temperature using an emulsifier to obtain a Ugi-OSAOcT / MKL complex synergistically stabilized drug-loaded Pickering emulsion.
[0087] Example 3
[0088] A method for preparing a drug-loaded Pickering emulsion stabilized by an oxidation-Ugi reaction alginate derivative / modified kaolin complex:
[0089] (1) Dissolve 5 g of sodium alginate SA in 200 mL of distilled water, add 50 mL of anhydrous ethanol and mix well, then add 2.68 g of sodium periodate, stir electrically in the dark for 24 h at room temperature, then add 10 mL of ethylene glycol, stir magnetically in the dark for 2 h to terminate the reaction; precipitate the solution after the reaction with 5 g of sodium chloride and 800 mL of anhydrous ethanol, then redissolve the precipitate in 100 mL of distilled water, and precipitate with 3 g of sodium chloride and 600 mL of anhydrous ethanol, repeat the precipitation 3 times, put the resulting solution into a dialysis bag with a molecular weight cutoff of 3500, dialyze for 5 days, and freeze-dry to obtain a sodium periodate oxidized alginate derivative with a theoretical oxidation degree of 50%, recorded as OSA50;
[0090] (2) 2.0 g (containing 10.1 mmol uronic acid monomer) of OSA50 obtained in step (1) was placed in a 250 mL three-necked flask, 200 mL of deionized water was added, and mechanical stirring was performed to obtain an OSA50 solution with a mass fraction of 1.0% (m / v), and then 4.01 mL (24.0 mmol) of octylamine was added, and the mixture was stirred at room temperature for 30 min, and then 1.72 mL (30.0 mmol) of glacial acetic acid was added, and 5.58 g (33.0 mmol) of p-toluenesulfonylmethyl isonitrile TOSMIC was added at the same time, and the mixture was stirred at room temperature for 12 h, and then 1 L of anhydrous methanol was added to the reaction solution for precipitation. After centrifugation, the precipitate was placed in a dialysis bag with a molecular weight cutoff of 3500, and dialyzed with deionized water for 3 days to remove residual small molecular impurities, and then freeze-dried at -60°C for 48 h to obtain Ugi-OSA50OcT with a degree of substitution DS of 24.3%;
[0091] (3) 3.00 g of kaolin raw material was first dried in an oven at 105°C to constant weight, then mixed with 0.03 g of dimethylpolysiloxane, and ball milled using a PM planetary ball mill with steel balls as the ball milling medium. The balls were: 2 steel balls with a diameter of 20 mm, 10 steel balls with a diameter of 10 mm, and 10 steel balls with a diameter of 6 mm. The main disk rotated at 516 r / min and ball milled for 1 h. The ball milled product was then washed with petroleum ether and deionized water, respectively, and freeze-dried at -60°C for 48 h to obtain MKL.
[0092] (4) mixing the Ugi-OSAOcT obtained in step (2) and the MKL obtained in step (3) at a mass ratio of 1:10 to obtain a Ugi-OSAOcT / MKL complex; then adding the Ugi-OSAOcT / MKL complex into deionized water and performing ultrasonic dispersion at 100 W, and then shaking and standing for more than 24 hours to obtain a Ugi-OSAOcT / MKL complex suspension with a mass fraction of 0.5 wt%;
[0093] (5) Dissolving chlorofluorocyanate (LF) in xylene to obtain chlorofluorocyanate in xylene at a concentration of 2.0 mg / mL, using the chlorofluorocyanate in xylene as the oil phase and the Ugi-OSAOcT / MKL complex suspension obtained in step (4) as the aqueous phase, mixing the two in a volume ratio of 3:7, and then subjecting the mixture to high-speed shearing at 12000 r / min for 5 min at room temperature using an emulsifier to obtain a drug-loaded Pickering emulsion synergistically stabilized by the Ugi-OSAOcT / MKL complex.
[0094] The solvent extraction method was used to measure the content of hydrophobic pesticides in the Pickering emulsion samples. 2.0 mL of the Ugi-OSAOcT / MKL complex synergistically stabilized drug-loaded Pickering emulsion prepared in Examples 1-3 was taken out and added to 8.0 mL of toluene. After being placed in an oscillator for thorough mixing and shaking, the oil phase was collected and the step was repeated three times. Finally, the toluene phases were combined and the pesticide content was measured using an Agilent HP6890N gas chromatograph. The encapsulation efficiency (EE) of the pesticides in different emulsion samples was calculated based on the measured pesticide content. The formula for calculating the encapsulation efficiency of the pesticide is shown in formula (2),
[0095]
[0096] Wherein, m1 is the measured content of pesticide in the emulsion, and m2 is the content of added pesticide.
[0097] Distilled water containing 0.5% Tween 80 was used as the drug release medium to conduct a simulated drug release test to test the cumulative release of pesticides in 48 hours by the Ugi-OSAOcT / MKL complex prepared in Examples 1-3 to stabilize the drug-loaded Pickering emulsion.
[0098] The test results are as follows: the synergistically stabilized drug-loaded Pickering emulsion of the Ugi-OSAOcT / MKL complex prepared in Example 1 has an encapsulation efficiency (EE) of up to 75.3% for hydrophobic pesticides, and the cumulative release of pesticides within 48 hours is 73.2%; the synergistically stabilized drug-loaded Pickering emulsion of the Ugi-OSAOcT / MKL complex prepared in Example 2 has an encapsulation efficiency (EE) of up to 93.7% for hydrophobic pesticides, and the cumulative release of pesticides within 48 hours is 67.2%; the synergistically stabilized drug-loaded Pickering emulsion of the Ugi-OSAOcT / MKL complex prepared in Example 3 has an encapsulation efficiency (EE) of up to 81.0% for hydrophobic pesticides, and the cumulative release of pesticides within 48 hours is 63.1%.
[0099] Moreover, the drug-loaded Pickering emulsions synergistically stabilized by the Ugi-OSAOcT / MKL complexes prepared in Examples 1-3 exhibited regular and uniform droplet morphology, and the synergistic effect and hydrophobic self-assembly behavior of the Ugi-OSAOcT / MKL complexes enabled the solid particles to be tightly adsorbed at the oil-water interface, effectively preventing the emulsion from destabilizing and greatly enhancing the emulsion stability.
[0100] Example 4
[0101] The only difference from Example 1 is that the mass fraction of the Ugi-OSAOcT / MKL complex suspension in step (4) is 0.5 wt %.
[0102] Example 5
[0103] The only difference from Example 1 is that the mass fraction of the Ugi-OSAOcT / MKL complex suspension in step (4) is 1.5 wt %.
[0104] Example 6
[0105] The only difference from Example 1 is that the mass fraction of the Ugi-OSAOcT / MKL complex suspension in step (4) is 2.0 wt %.
[0106] Example 7
[0107] The only difference from Example 1 is that the mass fraction of the Ugi-OSAOcT / MKL complex suspension in step (4) is 2.5 wt %.
[0108] Comparative Example 1
[0109] The only difference from Example 1 is that dimethylpolysiloxane is not added in step (3).
[0110] The contents of C, H, and N elements in Ugi-OSAOcT in Examples 1-3 were determined by elemental analysis, and the results are shown in Table 1. The DS values of polymers Ugi-OSA10OcT, Ugi-OSA30OcT, and Ugi-OSA50OcT were calculated to be 4.8%, 14.8%, and 24.3%, respectively, indicating that the degree of substitution of octylamine in the polymer increases with the increase in the degree of oxidation of OSA, which is attributed to the fact that OSA with a high degree of oxidation contains more aldehyde groups, which increases the active sites of the reaction.
[0111] Table 1 Content of elements in Ugi-OSAOcT
[0112] C(%m / m) H(%m / m) N(%m / m) DS(%) Ugi-OSA10OcT 5150 745 089 48 Ugi-OSA30OcT 4169 717 196 148 Ugi-OSA50OcT 30.36 6.77 2.10 24.3
[0113] Figure 1 The synthetic route of Ugi-OSAOcT in Examples 1-3 of the present invention is shown in FIG. Figure 1 It can be seen that the present invention first uses sodium periodate to oxidize alginate to obtain sodium periodate oxidized alginate derivative OSA, and then adds octylamine, glacial acetic acid, and tosylmethyl isocyanide in sequence to carry out Ugi reaction, thereby obtaining amphiphilic Ugi-OSAOcT.
[0114] Figure 2FT-IR spectra of ammonium alginate SA, sodium periodate oxidized alginate derivative OSA, Ugi-OSA10OcT in Example 1, Ugi-OSA30OcT in Example 2, Ugi-OSA50OcT in Example 3, octylamine OCA, and a mixture of octylamine OCA and sodium periodate oxidized alginate derivative OSA, wherein a is SA, b is OSA, c is Ugi-OSA10OcT, d is Ugi-OSA30OcT, e is Ugi-OSA50OcT, f is OCA, and g is a mixture of OCA and OSA. Figure 2 It can be seen that SA, OSA and Ugi-OSAOcT are in the range of 4000-3000cm -1 There is a broad and strong peak at 1621 and 1419 cm, which is attributed to the stretching vibration of hydroxyl OH. -1 The two bands appearing at 1734 cm-1 belong to the asymmetric and symmetric stretching vibrations of carboxylate CO, respectively. -1 The characteristic bands of the aldehyde group in the OSA structure are not observed. This is because the free aldehyde group in the OSA structure forms a hemiacetal or acetal structure. Compared with the infrared spectrum of OSA, Ugi-OSAOcT has characteristic absorption peaks similar to OSA at 2925 and 2842 cm -1 Very strong and sharp absorption peaks appeared at the octylamine structure, which were attributed to the antisymmetric and symmetric stretching vibration absorption peaks of the methylene (-CH2-) in the octylamine structure. These changes indicated that Ugi-OSAOcT was successfully synthesized.
[0115] Figure 3 is octylamine OCA (CDCl3) (a), p-toluenesulfonylmethyl isocyanide TOSMIC (D2O) (b), sodium alginate SA (D2O) (c), sodium periodate oxidized alginate derivative OSA (D2O) (d), Ugi-OSA10OcT in Example 1 (D2O) (e), Ugi-OSA30OcT in Example 2 (D2O) (f) and Ugi-OSA50OcT in Example 3 (D2O) (g) 1 H NMR spectrum. Figure 3 It can be seen that the proton signal peaks at δ3.5-5.1ppm are typical proton signal peaks of uronic acid residues in the SA structure. OSA has new proton signal peaks at δ5.35, 5.02 and 4.30ppm, which are attributed to the chemical shift of the hemiacetal proton obtained by the condensation of the aldehyde group on OSA and the hydroxyl group on the adjacent uronic acid, confirming that SA was successfully oxidized by sodium periodate. 1Compared with the H NMR spectrum, new proton signal peaks appeared at δ7.0-8.0, 2.3, 2.0-3.0, 1.1-1.5 and 0.8 ppm for the polymer Ugi-OSAOcT. Among them, the proton signal peaks at δ0.8, 1.1-1.5 and 2.0-3.0 ppm were attributed to the chemical shifts of the protons on the methyl group, the methylene group connected to the carbon and the methylene group connected to the nitrogen in the octylamine structure. δ2.3 and δ7.0-8.0 ppm were attributed to the chemical shifts of the protons on the methyl group and the benzene ring in the TOSMIC structure. This result further verified that the Ugi-4CR reaction of glacial acetic acid, octylamine OCA and TOSMIC with OSA occurred, and the polymer Ugi-OSAOcT was successfully synthesized.
[0116] Figure 4 The graph (A) shows the relationship between the concentration of Ugi-OSA10OcT in Example 1, Ugi-OSA30OcT in Example 2, and Ugi-OSA50OcT in Example 3 and the ratio of pyrene fluorescence intensity I1 / I3, and the graph (B) shows the change of CMC value with the substitution degree of polymer Ugi-OSAOcT. Figure 4 (A) It can be seen that when the concentration of polymer Ugi-OSAOcT is low, the I1 / I3 value is large and basically does not change with the increase of concentration, indicating that the polymer exists in the form of molecular chains in the aqueous solution at this time, and pyrene is in a polar environment. When the concentration increases to a certain value, the I1 / I3 value will drop sharply with the continuous increase of concentration, indicating that the polymer begins to form micelles under the hydrophobic force at this time, encapsulating pyrene in the hydrophobic core formed by the hydrophobic side chain octylamine group. The concentration corresponding to the inflection point at this time is the CMC value of the amphiphilic polymer. The CMC values of polymers Ugi-OSA10OcT, Ugi-OSA30OcT and Ugi-OSA50OcT are 0.30, 0.20 and 0.085 mg / mL respectively. Figure 4 (B) is a trend chart of the CMC value as the degree of substitution of hydrophobic groups in the polymer changes after OSA with different oxidation degrees is grafted with hydrophobic octylamine groups. As can be seen from the figure, the CMC value (0.30 mg / mL) of the polymer Ugi-OSA10OcT with the lowest degree of substitution of octylamine groups (about 4.8%) is higher than the CMC value (0.085 mg / mL) of the polymer Ugi-OSA50OcT with the highest degree of substitution (about 24.3%), indicating that the CMC value of the polymer shows a downward trend with the increase of the degree of substitution of hydrophobic octylamine groups. This is attributed to the increase in the grafting rate of hydrophobic octylamine groups, which increases the hydrophobic interaction force between polymer chains, is conducive to the formation of a denser hydrophobic core, and promotes the formation of molecular self-assembled micelles.
[0117] Figure 5The FT-IR spectra (a) and XRD spectra (b) of the raw kaolin and modified kaolin MKL in Example 1 are shown in FIG. Figure 5 (a) It can be seen that the basic framework of the infrared absorption spectrum of kaolin before and after modification has not changed, but the main change is at 800cm -1 The bending vibration absorption peaks of the Si-O bond and Al-O bond below are significantly enhanced, at 885cm -1 The hydroxyl (-OH) bending vibration absorption peak around 3600cm -1 The stretching vibration peaks of hydroxyl (-OH) are significantly enhanced. Due to the overlap of the vibration absorption peaks of the R-Si-O-Si bond on the surface of dimethylpolysiloxane and kaolin and the Si-O-Si bond on the surface of kaolin, the 1020cm -1 The vibration absorption peaks of Si-O and Si-O-Si bonds are significantly enhanced, 1500cm -1 The absorption peak enhancement around 2165cm is caused by the stretching vibration of carbon-carbon double bonds. -1 There is an absorption peak around the kaolinite particles. This absorption peak is caused by the stretching vibration of the Si-H bond, indicating that dimethylpolysiloxane is chemically or physically adsorbed on the surface of the kaolinite particles. Figure 5 (b) It can be seen that the characteristic peaks of kaolinite are obvious in the XRD spectrum of the raw material kaolinite, and there are also characteristic peaks of lauric zeolite, pyroxene and muscovite. The specific attributes of each peak are as follows: 2θ=9.45 is the characteristic diffraction peak of lauric zeolite; 2θ=12.28 is attributed to the characteristic diffraction peak of the 001 plane of kaolinite; 2θ=28.64 is attributed to the characteristic diffraction peak of pyroxene; 2θ=30.98 and 32.71 are attributed to the characteristic diffraction peaks of dolomite. After ball milling, there is no characteristic peak of kaolinite in the XRD spectrum of MKL. A large number of hydroxyl groups in its structure are removed, and the crystal structure is destroyed. The intensity of the diffraction peak characteristic of the crystalline structure of kaolinite gradually decreases or disappears with the increase of the modifier, showing the diffraction characteristics of an amorphous substance. This shows that during the ball milling process of kaolinite, the hydrogen bonds between the kaolinite layers are destroyed, which leads to the destruction of the crystal structure of kaolinite, the decrease of crystallinity, and the decrease of diffraction rate.
[0118] Figure 6The scanning electron microscope images and transmission electron microscope images of kaolin and modified kaolin MKL in Example 1, wherein (a) is a scanning electron microscope image of kaolin, (b) is a scanning electron microscope image of modified kaolin MKL, (c) is a transmission electron microscope image of kaolin, and (d) is a transmission electron microscope image of modified kaolin MKL. It can be clearly observed from the scanning electron microscope image that there are a large number of block structures in the original kaolin sample, and the size of the kaolin particles is relatively large. After ball milling modification, MKL obviously changes from block to fine particles, and the size is obviously smaller than before ball milling, indicating that the dry ball milling process has a certain crushing effect on the original kaolin sample. In addition, it can be clearly seen from its transmission electron microscope image that the raw kaolin has a flaky structure. After ball milling modification, the crystal structure of MKL is destroyed, the flaky structure disappears, and the modified MKL appears in a messy amorphous state.
[0119] Figure 7 The particle size distribution diagram (a) and zeta potential distribution diagram (b) of the kaolin and modified kaolin MKL in Example 1 are shown in FIG. Figure 7 (a) It can be seen that the particle sizes of the raw materials kaolin and MKL are concentrated, indicating that their particle sizes are relatively uniform. The pulverization effect of the ball milling process significantly reduces the particle size of MKL. Figure 7 (b) It can be seen that ball milling modification significantly reduces the Zeta potential of MKL. The reason for this phenomenon is that the modifier dimethylpolysiloxane is not electrically conductive. The modifier is coated on the surface of kaolin particles, which hinders the electrical properties of MKL and reduces its zeta potential.
[0120] Figure 8 Contact angles of kaolin (a) and modified kaolin MKL (b) in Example 1. It can be seen from the figure that water droplets cannot form water beads on the original kaolin, and the water is instantly absorbed by the kaolin, with a contact angle of about 21°, showing strong hydrophilicity. Water droplets can form water beads on the MKL sample, with a contact angle of about 90°, showing excellent hydrophilic and lipophilic properties. This result shows that the modifier is coated on the surface of kaolin, making it more hydrophobic.
[0121] Fig. 9 Schematic diagram of the drug-loaded Pickering emulsion synergistically stabilized by the Ugi-OSAOcT / MKL complex prepared in the present invention and its stabilizing mechanism.
[0122] Fig.10These are physical pictures of the Pickering emulsions synergistically stabilized by Ugi-OSAOcT / MKL complexes prepared in Comparative Example 1, Example 1, and Examples 4-7, wherein (a) is Comparative Example 1 (1.0 wt% Ugi-OSAOcT / kaolin complex); (b) is Example 4 (0.5 wt% Ugi-OSAOcT / MKL complex); (c) is Example 1 (1.0 wt% Ugi-OSAOcT / MKL complex); (d) is Example 5 (1.5 wt% Ugi-OSAOcT / MKL complex); (e) is Example 6 (2.0 wt% Ugi-OSAOcT / MKL complex); and (f) is Example 7 (2.5 wt% Ugi-OSAOcT / MKL complex). As can be seen from the figure, the thickness of the emulsion layer of the Pickering emulsion stabilized by the Ugi-OSAOcT / MKL complex is significantly higher than that of the Pickering emulsion stabilized by the Ugi-OSAOcT / kaolin complex, and with the increase of the mass fraction of the Ugi-OSAOcT / MKL complex, the thickness of the emulsion layer gradually increases, the stratification phenomenon of the emulsion weakens, and the emulsion stability is enhanced. This result shows that the Ugi-OSAOcT / MKL complex is more conducive to improving the stability of the Pickering emulsion.
[0123] Fig.11 These are droplet morphologies of the Pickering emulsions synergistically stabilized by Ugi-OSAOcT / MKL complexes prepared in Comparative Example 1, Example 1, and Examples 4-7, wherein (a) is Comparative Example 1 (1.0 wt% Ugi-OSAOcT / kaolin complex); (b) is Example 4 (0.5 wt% Ugi-OSAOcT / MKL complex); (c) is Example 1 (1.0 wt% Ugi-OSAOcT / MKL complex); (d) is Example 5 (1.5 wt% Ugi-OSAOcT / MKL complex); (e) is Example 6 (2.0 wt% Ugi-OSAOcT / MKL complex); and (f) is Example 7 (2.5 wt% Ugi-OSAOcT / MKL complex). It can be seen from the figure that the emulsion particle size of the Pickering emulsion stabilized by the Ugi-OSAOcT / MKL complex is also significantly smaller than that of the Pickering emulsion stabilized by the Ugi-OSAOcT / kaolin complex at the same mass fraction. Moreover, with the increase of the mass fraction of the Ugi-OSAOcT / MKL complex, the emulsion droplet size gradually decreases and the dispersibility of the droplets is enhanced. The smaller the droplet size, the more conducive to the stability of the emulsion.
[0124] Fig.12The droplet morphology (a) and schematic diagram (b) of the Pickering emulsion synergistically stabilized by the Ugi-OSAOcT / MKL complex in Example 1, and the laser confocal electron microscope image of the Pickering emulsion synergistically stabilized by the Ugi-OSAOcT / MKL complex stained with 1 mg / mL of Rhodamine B. It can be seen from the figure that the Ugi-OSAOcT / MKL complex stained with Rhodamine B is in an aggregated form at the oil-water interface. It is the good alternating interfacial activity of the Ugi-OSAOcT / MKL complex that allows it to be stably adsorbed at the oil-water interface, thereby constructing a stable pesticide Pickering emulsion.
[0125] Fig.13 The in vitro cumulative release curve of the drug-loaded Pickering emulsion stabilized by chlorofluorocyanoester LF and the Ugi-OSAOcT / MKL complex in Example 1-3 in PBS at pH = 7.4 at 37°C. Fig.13 It can be seen that the free pesticide chlorofluorocyanate (LF) was released up to 93.0% in PBS at pH = 7.4 within 7 hours. Compared with free LF, the release of LF from the drug-loaded Pickering emulsions stabilized by the Ugi-OSAOcT / MKL complex in Examples 1-3 was sustained-release, confirming that the LF molecules were well encapsulated in the oil phase of the Pickering emulsion. The cumulative release of LF from the drug-loaded Pickering emulsions stabilized by Ugi-OSA10OcT, Ugi-OSA30OcT and Ugi-OSA50OcT with different degrees of substitution and MKL within 48 hours was 73.2%, 67.2% and 63.1%, respectively, indicating that the increase in the degree of substitution of the hydrophobic group will reduce the cumulative release of the drug-loaded Pickering emulsions stabilized by the Ugi-OSAOcT / MKL complex, which may be attributed to the fact that Ugi-OSAOcT with a higher degree of hydrophobic substitution will enhance the affinity with the oil phase and form a tighter interfacial film. Therefore, the release of drugs can be better controlled by fine-tuning the degree of substitution of hydrophobic groups in Ugi-OSA10OcT, achieving better sustained-release effects of pesticides.
[0126] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a drug-loaded Pickering emulsion synergistically stabilized by an oxidation-Ugi reaction alginate derivative / modified kaolin composite, characterized in that: The following steps are involved: (1) adding octylamine, glacial acetic acid, and p-toluenesulfonylmethyl isocyanide to a sodium periodate oxidized alginate derivative solution in sequence to carry out Ugi reaction, and obtaining an oxidized-Ugi reaction alginate derivative Ugi-OSAOcT through precipitation, centrifugation, dialysis, and freeze drying; (2) mixing kaolin and dimethylpolysiloxane, ball milling, washing and freeze-drying to obtain modified kaolin MKL; (3) mixing the oxidized-Ugi reaction alginic acid derivative Ugi-OSAOcT obtained in step (1) and the modified kaolin MKL obtained in step (2) to obtain a Ugi-OSAOcT / MKL complex; adding the Ugi-OSAOcT / MKL complex into water, dispersing by ultrasonication and allowing to stand by shaking to obtain a Ugi-OSAOcT / MKL complex suspension; (4) using the oil containing the hydrophobic pesticide as the oil phase and the Ugi-OSAOcT / MKL complex suspension obtained in step (3) as the water phase, mixing the two and then shearing and emulsifying them to obtain an oxidation-Ugi reaction alginate derivative / modified kaolin complex synergistically stabilized drug-loaded Pickering emulsion; There is no order of precedence for steps (1) and (2).
2. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of the uronic acid monomer of the sodium periodate oxidized alginate derivative to octylamine, glacial acetic acid and p-toluenesulfonylmethyl isocyanide in the sodium periodate oxidized alginate derivative solution is (1:2:2:2.2)-(1:2.8:3.1:3.3).
3. The preparation method according to claim 1, characterized in that: In step (2), the amount of dimethylpolysiloxane used is 0.5-2.0% of the mass of kaolin.
4. The preparation method according to claim 1, characterized in that: In step (2), the medium of the ball mill is steel balls, the rotation speed is 516r / min, and the time is 1h; when the amount of kaolin used is 3.00-6.00g, the balls used for the ball mill are: 2 steel balls with a diameter of 20mm, 10 steel balls with a diameter of 10mm, and 10 steel balls with a diameter of 6mm.
5. The preparation method according to claim 1, characterized in that: In step (3), the mass ratio of the oxidized-Ugi reaction alginate derivative Ugi-OSAOcT and the modified kaolin MKL in the Ugi-OSAOcT / MKL complex is (1:2)-(1:10).
6. The preparation method according to claim 1, characterized in that: In step (3), the mass fraction of the Ugi-OSAOcT / MKL complex in the Ugi-OSAOcT / MKL complex suspension is 0.5-2.5%.
7. The preparation method according to claim 1, characterized in that: In step (4), the hydrophobic pesticide includes one of cyhalothrin, bifenthrin and avermectin benzoate; and the oil includes one of xylene, toluene and liquid paraffin.
8. The preparation method according to claim 1, characterized in that: In step (4), the concentration of the hydrophobic pesticide in the oil containing the hydrophobic pesticide is 0.5-5.0 mg / mL.
9. The preparation method according to claim 1, characterized in that: In step (4), the volume ratio of the oil containing the hydrophobic pesticide to the Ugi-OSAOcT / MKL complex suspension is (2:8)-(5:5).
10. The drug-loaded Pickering emulsion synergistically stabilized by the oxidation-Ugi reaction alginate derivative / modified kaolin complex prepared by the preparation method according to any one of claims 1 to 9.