Tissue adhesion electrode and preparation method and application thereof
By preparing tissue-adhesive polymers and conductive polymer slurries, combined with 3D printing and other technologies, the problem of poor integration stability of traditional bioelectrodes has been solved, and non-invasive, rapid adhesion and bidirectional electrical signal conduction with biological tissues have been achieved to meet the needs of pattern design. Chemical structural requirements, high toughness and good biocompatibility.
Patent Information
- Application Number
- CN202410751411.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-18
AI Technical Summary
The integration of traditional bioelectrodes with target tissues or organs has poor stability and high invasiveness. The reliability and accuracy of electrophysiological signal collection and regulation performance are low, and they cannot meet the needs of patterned structures.
Using the preparation method of tissue-adhesive polymer slurry and conductive polymer slurry, tissue-adherent electrodes are prepared through steps such as mechanical stirring, polymerization reaction and precipitation, and 3D printing and other technologies are used to form a patterned structure, combined with conductive materials such as graphite ene and carbon nanotubes, etc., to achieve non-invasive, rapid and stable adhesion and bidirectional electrical signal transmission between electrodes and biological tissues.
It achieves rapid, strong and stable adhesion to wet biological tissues, maintains high toughness and elasticity, has bidirectional electrical signal conduction properties, is suitable for physiological electrical signal monitoring and regulation, and shows good biocompatibility in in vitro and in vivo experiments. and electrical properties.
Smart Images

Figure CN118787359A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of medical materials, and in particular relates to a tissue adhesion electrode and a preparation method and application thereof. Background Art
[0002] Electrophysiological sensing and regulation require the establishment of an intimate bioelectronic interface between the electrode and the target biological tissue or organ. The traditional method is to fix the bioelectrode to the target tissue by suturing or inserting the electrode, or to attach the thin and flexible bioelectrode to the biological tissue. These methods will damage the reliability and accuracy of electrophysiological monitoring and regulation, and cause scarring and life-threatening complications. Especially in the moist and dynamic environment of the body (such as important organs such as the heart), traditional methods will bring huge risks and cause various adverse consequences, including device failure, heart cavity perforation (especially atrium), bleeding, pericardial effusion and cardiac tamponade. Therefore, this field urgently needs electrode materials that can fuse with target biological tissues non-invasively, quickly and stably.
[0003] In recent years, tissue adhesives have shown great potential as an alternative to traditional surgical suturing methods, playing an important role in reducing tissue damage and improving patient rehabilitation outcomes. At the same time, tissue adhesives have also shown potential in the seamless integration of electronic devices and tissues. However, current tissue adhesives are generally not conductive and cannot form bidirectional electrical signal conduction between tissues and electronic devices. In addition, tissue adhesives are usually processed into thin films or block structures through mold molding, which have low compatibility with the design and manufacturing of various electronic devices, lack processing flexibility, and cannot meet the needs of electrode arraying, patterning, and miniaturization. Summary of the invention
[0004] The purpose of the present invention is to provide a tissue adhesion electrode and its preparation method and application, aiming to solve the problems of poor integration stability and high trauma between existing biological electrodes and target tissues or organs, and low reliability and accuracy of electrophysiological signal acquisition and regulation performance, while meeting the needs of manufacturing tissue adhesion electrodes with patterned structures.
[0005] The method for preparing a tissue adhesion electrode provided by the present invention specifically comprises the steps of preparing a tissue adhesion polymer slurry, preparing a tissue adhesion conductive polymer slurry and preparing an electrode;
[0006] (I) Preparation of tissue adhesion polymer slurry:
[0007] Its synthetic route is:
[0008]
[0009] Where R is an alkyl chain, R 1 is hydroxyl or carboxyl, R3 is hydrogen or methyl
[0010] The specific steps of preparation are:
[0011] (1) dissolving the dried hydrophilic polyurethane and isocyanate in NN-dimethylformamide (DMF), wherein the mass ratio of isocyanate to hydrophilic polyurethane is 0.5%-10%, and mechanically stirring for 1-4 hours under nitrogen at 40-80° C. to obtain a uniform mixture;
[0012] (2) dissolving the bridging compound in DMF, adding the mixture to the mixture obtained in step (1), and stirring evenly;
[0013] (3) then slowly adding an initiator and acrylic acid and its derivatives, wherein the mass ratio of acrylic acid and its derivatives to hydrophilic polyurethane or isocyanate is 10%-50%, and continuing the polymerization reaction at 40-80° C. with stirring for 2-4 hours;
[0014] (4) After the reaction is completed, the product is precipitated in distilled water to terminate the polymerization reaction;
[0015] (5) cutting the product of step (3) into small pieces weighing about 0.5 g each, washing them thoroughly in distilled water to remove residual reactants, and then drying the product;
[0016] (6) dissolving the product in a solvent to prepare a tissue adhesion polymer slurry; the mass fraction of the tissue adhesion polymer is 5-30%;
[0017] in:
[0018] The polyurethane described in step (1) is a hydrophilic polyurethane, preferably, a HydroMed D series product of AdvanSource Biomaterials Corp.
[0019] The isocyanate described in step (1) is at least one of toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), hexamethylene diisocyanate (HDI), and lysine diisocyanate (LDI).
[0020] The bridging compound in step (2) is at least one of the following structures:
[0021]
[0022] Preferably, at least one of hydroxyethyl methacrylate (HEMA), hydroxyethyl acrylate, mono[2-[(2-methyl-acryloyl)oxy]ethyl] succinate (MMES), 4-(2-(methacryloyloxy)ethoxy)-4-oxobut-2-enoic acid (HEMA maleate), and 2-[[(carboxymethyl)dithio]acetoxy]ethyl 2-methyl-2-acrylate is selected.
[0023] The initiator described in step (3) is at least one of azobisisobutyronitrile (AIBN), benzoyl peroxide (BPO), dicumyl peroxide (DCP), and tert-butyl perbenzoate (TBPB).
[0024] The acrylic acid and its derivatives described in step (3) are at least one of acrylic acid, methacrylic acid, N-succinimidyl acrylic acid ester, sodium salt of N-succinimidyl acrylic acid sulfonate, methyl methacrylate, ethyl methacrylate, and acrylamide.
[0025] The solvent in step (6) is ethanol, water, isopropanol, dimethyl sulfoxide, etc.;
[0026] (II) Preparation of tissue adhesion conductive polymer slurry:
[0027] The conductive material is mixed with the tissue adhesion polymer slurry obtained above to obtain tissue adhesion conductive polymer slurry; the solid content of the conductive material in the tissue adhesion conductive slurry is 1-10%.
[0028] The conductive material is at least one of polyaniline and its derivatives, polypyrrole and its derivatives, polythiophene and its derivatives, graphene, carbon nanotubes, carbon black, and metal nanoparticles. Preferably, poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT:PSS) particles are selected.
[0029] (iii) Preparation of tissue adhesion electrodes;
[0030] Tissue adhesion polymer slurry has good biocompatibility and mechanical properties, and is usually used in applications such as tissue repair and wound hemostasis. Tissue adhesion conductive polymer slurry has good electrical conductivity and is usually used to prepare flexible bioelectrodes and sensors. Whether to add conductive materials depends on the specific application needs and performance requirements.
[0031] The tissue adhesion electrode is prepared using the tissue adhesion polymer slurry obtained in step (1) or the tissue adhesion conductive polymer slurry obtained in step (2).
[0032] Specifically, methods such as 3D printing, screen printing, spin coating, spray coating or scraping coating may be used. Preferably, a 3D printing method is used to obtain a patterned tissue adhesion electrode after evaporating the solvent.
[0033] The tissue adhesion electrode prepared by the present invention has excellent performance, can form fast, strong, stable and non-invasive adhesion with wet tissue, can maintain high toughness and elasticity when deformed, and adapt to the dynamic deformation tissue environment; at the same time, it has the performance of bidirectional electrical signal conduction. It can be used as a monitoring and regulation device for physiological electrical signals.
[0034] The present invention has the following advantages:
[0035] (1) The tissue-adhesive polymer slurry and tissue-adhesive conductive slurry of the present invention have good rheological properties, are easy to flow and diffuse when a force is applied, and can maintain their shape after the force is removed ( Figure 1 ), tissue adhesion electrodes can be prepared by 3D printing, screen printing, spin coating, spray coating, scraping and other methods.
[0036] (2) The tissue adhesion electrode prepared by the present invention has good adhesion and mechanical properties, and can form a strong adhesion to wet biological tissue within seconds. The dry tissue adhesion electrode can quickly absorb moisture from the tissue surface, form hydrogen bonds or electrostatic interactions with the tissue, and further form covalent crosslinks with amino groups, carboxyl groups, etc. on the tissue surface. The shear strength of the ionic conductive and ion conductive tissue adhesion electrodes for biological tissue adhesion reached 50 kPa and 35 kPa respectively, and the fracture toughness reached 300 J m -2 and 200 J m -2 ( Figure 2 ).
[0037] (3) The tissue adhesion electrode prepared by the present invention has good electrical properties, and the charge injection performance and interfacial electrochemical impedance remain stable for a long time in a physiological environment ( Figure 3 ).
[0038] (4) The tissue adhesion electrode prepared by the present invention has excellent mechanical strength. The dynamic hydrogen bond interaction in the material provides an energy dissipation mechanism, so that the material maintains high toughness and elasticity when deformed.
[0039] (5) The tissue adhesion electrode prepared by the present invention exhibits good biocompatibility in in vitro cell and in vivo animal experiments.
[0040] (6) The tissue adhesion electrode prepared by the present invention can form long-term stable electrical bidirectional conduction with the tissue, and stably monitor and regulate electrophysiological signals. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is the rheological properties of the tissue adhesion polymer slurry and the tissue adhesion conductive slurry in the present invention.
[0042] Figure 2The adhesion properties of the tissue adhesion electrode of the present invention are ionic conductivity and ion conductivity.
[0043] Figure 3 It is the electrical stability performance of the tissue adhesion electrode in the present invention under physiological conditions.
[0044] Figure 4 The tissue adhesion electrode is prepared by 3D printing in the present invention.
[0045] Figure 5 This is a photo of the tissue adhesion electrode used for monitoring and regulating ECG signals on the heart surface in the present invention.
[0046] Figure 6 The invention relates to the cardiac surface electrocardiographic signal monitoring and regulation performance of the tissue adhesion electrode. DETAILED DESCRIPTION
[0047] The present invention is further described below in conjunction with specific examples, but is not limited to the contents of the specification. All raw materials used are commercially available products in the art.
[0048] Example 1: Preparation of a tissue adhesion electrode, comprising the following steps:
[0049] (1) The hydrophilic polyurethane and MDI were dried under vacuum overnight.
[0050] (2) Hydrophilic polyurethane (10 g) and MDI (0.5 g) were dissolved in 30 mL of DMF and mechanically stirred at 50° C. for 2 hours under nitrogen atmosphere to obtain a homogeneous mixture.
[0051] (3) 0.6 g of HEMA was dissolved in 10 mL of DMF, added to the reaction mixture and stirred for 1 hour.
[0052] (4) Slowly add 0.3 g of AIBN and 30 g of acrylic acid, and continue the reaction at 70° C. for 3 hours.
[0053] (5) After the reaction was completed, the product was precipitated in distilled water to terminate the polymerization reaction, and the product was cut into small pieces and thoroughly washed in distilled water to remove residual reactants. The final product was dried in a fume hood for 3 days.
[0054] (6) Dissolve 15 g of the product in 85 g of 70% ethanol to obtain a tissue adhesion polymer slurry. The rheological properties of the slurry are as follows: Figure 1 shown.
[0055] (7) Screen printing the tissue adhesion polymer slurry on the surface of the gold electrode, and after drying, obtaining an ion-conductive tissue adhesion electrode.
[0056] (8) The adhesion properties of the obtained ion-conductive tissue adhesion electrode are as follows: Figure 2 shown.
[0057] Embodiment 2: A method for preparing a tissue adhesion electrode, comprising the following steps:
[0058] (1) drying the hydrophilic polyurethane and MDI under vacuum overnight;
[0059] (2) dissolving 10 g of hydrophilic polyurethane and 0.5 g of MDI in 30 mL of DMF and mechanically stirring for 2 hours at 50 °C in a nitrogen environment to obtain a uniform mixture;
[0060] (3) Add 3 g of 2-[[(carboxymethyl)dithio]acetoxy]ethyl 2-methyl-2-acrylate and 0.3 g of AIBN, and stir for 1 hour;
[0061] (4) adding 29.5 g of acrylic acid and 0.5 g of sodium succinimidyl sulfonate of acrylic acid, and continuing the reaction at 70° C. for 3 hours;
[0062] (5) After the reaction was completed, the product was precipitated in distilled water to terminate the polymerization reaction, and the product was cut into small pieces and thoroughly washed in distilled water to remove residual reactants; the final product was dried in a fume hood for 3 days;
[0063] (6) 5 g of the product was dissolved in 95 g of isopropanol to obtain a tissue adhesion slurry. The rheological properties of the slurry were as follows: Figure 1 As shown;
[0064] (7) applying the tissue adhesion slurry to the surface of the platinum electrode, and obtaining an ion-conductive tissue adhesion electrode after drying;
[0065] (8) The adhesion properties of the obtained ion-conductive tissue adhesion electrode are as follows: Figure 2 shown.
[0066] Embodiment 3: A method for preparing a tissue adhesion electrode, comprising the following steps:
[0067] (1) The hydrophilic polyurethane and MDI were dried under vacuum overnight.
[0068] (2) 10 g of hydrophilic polyurethane and 0.5 g of MDI were dissolved in 30 mL of DMF and mechanically stirred at 50° C. for 2 hours under a nitrogen atmosphere to obtain a uniform mixture.
[0069] (3) 0.6 g of HEMA was dissolved in 10 mL of DMF, added to the reaction mixture and stirred for 1 hour.
[0070] (4) Slowly add 0.3 g of AIBN and 30 g of acrylic acid, and continue the reaction at 70° C. for 3 hours.
[0071] (5) After the reaction was completed, the product was precipitated in distilled water to terminate the polymerization reaction, and the product was cut into small pieces and thoroughly washed in distilled water to remove residual reactants. The final product was dried in a fume hood for 3 days.
[0072] (6) 15 g of the product was dissolved in 85 g of 70% ethanol to obtain a tissue adhesion polymer slurry.
[0073] (7) 5 g of PEDOT:PSS particles (Orgacon series products purchased from Agfa Materials, Belgium) were dispersed in 95 g of deionized water-DMSO mixed solvent (water:DMSO=85:15 v / v). The solution was mixed with the polymer slurry in a volume ratio of 1:2 to obtain a tissue adhesion conductive slurry. The rheological properties of the slurry are as follows: Figure 1 shown.
[0074] (8) The tissue adhesion conductive paste is used to prepare a patterned electrode by 3D printing, which is further integrated with a stainless steel fiber electrode to obtain an ionically conductive tissue adhesion electrode after drying.
[0075] (9) The adhesion properties of the obtained ion-conductive tissue adhesion electrode are as follows: Figure 2 As shown, the electrical stability performance is Figure 3 As shown, the preparation steps are as follows Figure 4 shown.
[0076] Example 4: Monitoring and regulating ECG signals using tissue-adhesive electrodes of the present invention.
[0077] (1) Methods
[0078] The electrophysiological signal monitoring and regulation effect of the tissue adhesion electrode of Example 3 was evaluated using a pig heart model (3 in each group). After the pig was anesthetized, the skin was prepared, the chest cavity was opened using a left thoracotomy, and the pericardium was cut to expose the epicardium for device implantation. Two tissue adhesion electrodes were adhered to the atrium and ventricle respectively, and the other end of the stainless steel fiber electrode in the tissue adhesion electrode of Example 3 was modified by an Oscor C / IS adapter and connected to an implantable pacemaker (Dextronix, PetPacer-DR) ( Figure 5 The pacemaker was implanted subcutaneously, the chest was surgically closed, and the RENAMIC portable remote controller was used to obtain the ECG signals and pacing thresholds monitored by tissue-adherent electrodes in vitro.
[0079] (2) Results
[0080] Ten days after implantation, the tissue-adhesive electrodes can still collect ECG signals from the heart surface with a high signal-to-noise ratio, and the induced amplitude of the ECG signals is stable. The tissue-adhesive electrodes can stably stimulate the heart with tachycardia, increasing the heart rate of the pig heart from 60 beats / minute to 110 beats / minute. The threshold of electrical stimulation pacing remains stable within 10 days. Figure 6 .
Claims
1. A method for preparing a tissue adhesion electrode, characterized in that: The specific steps are: (I) Preparation of tissue adhesion polymer slurry: Its synthetic route is: Wherein, R is an alkyl chain, R1 is a hydroxyl group or a carboxyl group, and R2 is a hydrogen or a methyl group; The specific steps of preparation are: (1) dissolving the dried hydrophilic polyurethane and isocyanate in NN-dimethylformamide (DMF), wherein the mass ratio of isocyanate to hydrophilic polyurethane is 0.5%-10%, and mechanically stirring for 1-4 hours under nitrogen at 40-80° C. to obtain a uniform mixture; (2) dissolving the bridging compound in DMF, adding the mixture to the mixture obtained in step (1), and stirring evenly; (3) then adding an initiator and acrylic acid and its derivatives, the mass ratio of acrylic acid and its derivatives to hydrophilic polyurethane or isocyanate being 10%-50%, and continuing the polymerization reaction at 40-80° C. with stirring for 2-4 hours; (4) After the reaction is completed, the product is precipitated in distilled water to terminate the polymerization reaction; (5) cutting the product of step (3) into small pieces, washing them thoroughly in distilled water to remove residual reactants, and then drying the product; (6) dissolving the product in a solvent to prepare a tissue adhesion polymer slurry; the mass fraction of the tissue adhesion polymer is 5-30%; (II) Preparation of tissue adhesion conductive polymer slurry: Mixing the conductive material with the tissue adhesion polymer slurry obtained above to obtain a tissue adhesion conductive polymer slurry; the solid content of the conductive material in the tissue adhesion conductive slurry is 1-10%; (iii) Preparation of tissue adhesion electrodes; The tissue adhesion electrode is prepared using the tissue adhesion polymer slurry obtained in step (1) or the tissue adhesion conductive polymer slurry obtained in step (2).
2. The method for preparing a tissue adhesion electrode according to claim 1, characterized in that: In step (1) of step (a), the hydrophilic polyurethane is a HydroMed D series product of AdvanSource Biomaterials Corp.; the isocyanate is selected from toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate.
3. The method for preparing a tissue adhesion electrode according to claim 1, characterized in that: The bridging compound in step (2) of step (1) is at least one of the following structures:
4. The method for preparing a tissue adhesion electrode according to claim 1, characterized in that: The bridging compound described in step (2) of step (a) is selected from hydroxyethyl methacrylate, hydroxyethyl acrylate, mono[2-[(2-methyl-acryloyl)oxy]ethyl]succinate, 4-(2-(methacryloyloxy)ethoxy)-4-oxobut-2-enoic acid (HEMA maleate), and 2-[[(carboxymethyl)dithio]acetoxy]ethyl 2-methyl-2-acrylate.
5. The method for preparing a tissue adhesion electrode according to claim 1, characterized in that: In step (3) of step (a), the initiator is selected from azobisisobutyronitrile, benzoyl peroxide, diisopropylbenzene peroxide, and tert-butyl perbenzoate; the acrylic acid and its derivatives are selected from acrylic acid, methacrylic acid, N-succinimidyl acrylate, sodium salt of N-succinimidyl sulfonic acid ester, methyl methacrylate, ethyl methacrylate, and acrylamide.
6. The method for preparing a tissue adhesion electrode according to claim 1, characterized in that: In step (6) of step (a), the solvent is selected from ethanol, water, isopropanol, and dimethyl sulfoxide.
7. The method for preparing a tissue adhesion electrode according to claim 1, characterized in that: The conductive material described in step (ii) is selected from polyaniline and its derivatives, polypyrrole and its derivatives, polythiophene and its derivatives, graphene, carbon nanotubes, carbon black, and metal nanoparticles.
8. The method for preparing a tissue adhesion electrode according to claim 1, characterized in that: The tissue adhesion electrode described in step (iii) is prepared by 3D printing, screen printing, spin coating, spray coating or scraping coating.
9. A tissue adhesion electrode obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the tissue adhesion electrode as claimed in claim 9 as a monitoring and regulating device for physiological electrical signals.
Citation Information
Patent Citations
Polyurethane binder, electrodes containing the same and lithium battery employing the electrodes
CN101007933A
Electrode, method for preparing the same, bindercomposition and lithium battery containing thematerials
KR1020060108792A
Bio-electrode composition, bio-electrode, method for manufacturing bio-electrode, and reaction composite
US20220135763A1
Hydrophilic, swellable coatings for biosensors