Method for purifying low-grade crystalline flake graphite ore through forward-reverse flotation ion activation
Through the forward-reverse flotation ion activation purification method, the problem of impurities entrained by large-sized flake graphite in forward flotation is solved, the fixed carbon content of the flake graphite concentrate is increased, the large-sized flake graphite is protected, and an efficient purification effect is achieved. .
Patent Information
- Application Number
- CN202410982726.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-22
AI Technical Summary
During the positive flotation process, large-sized flake graphite is difficult to adhere to the bubbles due to its large size, resulting in the entrainment of small particle impurities, reducing the fixed carbon content of the graphite concentrate, and multi-stage grinding will damage the large-sized flake graphite.
The forward-reverse flotation ion activation and purification method is used to process the flake graphite ore through crushing and grinding, so that the particle size reaches -150 mesh accounting for 90%. Different pH adjusters and inhibitors are used in forward flotation and reverse flotation. It uses ionic activators to react with the surface of impurities such as quartz to enhance the adsorption of collectors, remove impurities and protect large-scale flake graphite.
It effectively removes small particle impurities during the positive flotation process, increases the fixed carbon content of graphite concentrate, protects large-sized flake graphite, and significantly improves the quality of the concentrate.
Smart Images

Figure CN118788495A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral processing, and in particular relates to a method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation. Background Art
[0002] As a material with many unique physical and chemical properties, graphite plays an increasingly important role in today's society. It not only has good electrical and thermal conductivity, but also has excellent corrosion resistance, high temperature resistance and lubricity, making it an indispensable material in many fields such as battery manufacturing, chemical industry, metal smelting, electronic devices, aerospace and environmental protection.
[0003] Natural graphite ore is mainly divided into flake graphite and microcrystalline graphite. Flake graphite is mainly used as raw material for batteries and cutting-edge technologies such as atomic energy. However, with the acceleration of global industrialization, high-grade flake graphite ore has begun to show signs of shortage. At the same time, many countries with graphite resources have implemented graphite export restrictions in order to protect their own economic and strategic resources. Therefore, strengthening the research on low-grade flake graphite ore and exploring more economical and efficient purification methods are of great significance to the development of high-precision and advanced technologies related to graphite products and promoting the effective use of resources.
[0004] At present, flake graphite is mainly purified by flotation. In the positive flotation production process, some large-sized flake graphite is difficult to attach to the bubbles and be brought to the liquid surface due to its large size. Therefore, multi-stage grinding is usually performed to reduce the graphite size or increase the air intake to form larger bubbles. However, these large bubbles are prone to entrain small particles of impurities to the liquid surface during the rising process, resulting in a decrease in the fixed carbon content in the graphite concentrate. Therefore, it is particularly important to explore a process to solve the problem of entrainment of small particles of impurities during flotation while protecting large-sized flake graphite. Summary of the invention
[0005] In view of the serious entrainment of the large-sized flake graphite in the forward flotation process and the problem that the large-sized flake graphite is easily destroyed by multi-stage grinding, the present invention provides a method for purifying low-grade flake graphite ore by forward-reverse flotation ion activation, which aims to protect the large-sized flake graphite and remove the impurities entrained in the forward flotation process, thereby increasing its fixed carbon content. In order to achieve the above-mentioned purpose of the present invention, the following technical scheme is specially adopted:
[0006] The present invention discloses a method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation, comprising the following steps:
[0007] Step 1 Crushing and Grinding
[0008] Crushing and grinding the flake graphite ore until the grinding particle size of -150 mesh accounts for more than 90%, thereby obtaining flake graphite ore;
[0009] Step 2: Positive flotation
[0010] The obtained flake graphite ore is added to a flotation tank, and water is added for mixing to obtain a pulp, a pH adjuster is added to the pulp to adjust the pH of the pulp to 6-9, and then inhibitor A, collector A, and frother A are added in sequence, followed by flotation to obtain a graphite concentrate;
[0011] Step 3: Reverse flotation
[0012] The obtained graphite concentrate is mixed with water and added to a flotation tank to obtain a pulp; then a pH adjuster is added to adjust the pH of the pulp to 5-8, and then an ion activator is added, and then inhibitor B, collector B and frother B are added in sequence and stirred respectively, and then the aeration switch is turned on to perform reverse flotation, and the remaining pulp in the flotation tank is filtered and dried to obtain flake graphite concentrate;
[0013] The ion activator is selected from at least one of MgCl2, AlCl3 and CaCl2;
[0014] The depressant B used in the reverse flotation process is selected from at least one of carboxymethyl cellulose and MF (formaldehyde condensate of sodium methyl naphthalene sulfonate);
[0015] The collector B used in the reverse flotation process is selected from at least one of monoamine, alkyl polyamine ether, ether monoamine, N-alkyl amide, dodecylamine, octadecylamine, kerosene and sodium oleate;
[0016] The frother B used in the reverse flotation process is selected from at least one of terpineol and octanol;
[0017] During the reverse flotation process, ion activator is added in an amount of 80-320 g / t, inhibitor B is added in an amount of 700-1300 g / t, collector B is added in an amount of 260-420 g / t, and frother is added in an amount of 150-300 g / t.
[0018] The invention discloses a method for purifying low-grade flake graphite ore by positive-reverse flotation ion activation. The flake graphite ore is firstly coarsely crushed to obtain a coarsely crushed product, and then finely crushed by a crushing and screening machine to obtain a finely crushed product. The finely crushed product is ground by a crusher to make the mineral particle size of -150 mesh account for more than 90%, thereby obtaining flake graphite ore.
[0019] The flake graphite ore includes low-grade natural flake graphite ore. In the present invention, the low-grade natural flake graphite ore includes natural flake graphite ore with a fixed carbon content of less than or equal to 8.5%.
[0020] When used in industry, the natural flake graphite ore is coarsely crushed by a crusher to 8-35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then finely crushed by a crushing and screening machine to 0.1-3 mm, accounting for more than 70%, to obtain a fine crushed product; the obtained fine crushed product is ground by a sample preparation crusher for 2-5 minutes, and the grinding particle size is -150 mesh, accounting for more than 90%, to obtain flake graphite ore.
[0021] In order to further improve the application value, the present invention has certain requirements on the fixed carbon content in the natural flake graphite ore, that is, the fixed carbon content is greater than or equal to 2%, at which time the industrial application value is greater. Of course, low fixed carbon content can also be used in the present invention, but the cost is slightly higher.
[0022] When used in industry, the flake graphite ore obtained by grinding is added to a flotation tank, deionized water is added for mixing, and the flake graphite ore slurry is obtained by stirring for 2 to 5 minutes, a pH adjuster is added thereto, the pH of the slurry is adjusted to 6 to 9, and the slurry is stirred for 2 to 5 minutes; then inhibitor A and collector A are added thereto in sequence and stirred for 2 to 5 minutes respectively, and then a frother A is added thereto, after stirring for 1 to 3 minutes, the aeration switch is turned on, and then the scraping foam is performed for 3 to 12 minutes, and the scraped foam is the graphite concentrate; the slurry concentration of the flake graphite ore slurry is 8wt.% to 25wt.%, preferably 15wt.% to 25wt.%. The dosage of inhibitor A is 700 to 1300g / t, preferably 880 to 1260g / t; the dosage of collector A is 260 to 420g / t, and the dosage of frother A is 150 to 300g / t.
[0023] The crusher used in the present invention comprises a jaw crusher, and the crushing and screening machine comprises a roller crushing and screening machine. Of course, other crushers and crushing and screening machines can also be used in the present invention.
[0024] The water used in the present invention includes deionized water.
[0025] The flotation machine used in the present invention is preferably an XFG5-35 hanging tank flotation machine, and of course other flotation machines can also be used in the present invention.
[0026] The stirring process of the present invention adopts the impeller of the flotation machine for stirring, and the rotating speed is 800-1500r / min.
[0027] The pH adjuster used in the present invention is one of HCl, NaOH and CaO.
[0028] The inhibitor A used in the positive flotation process of the present invention is one or more of water glass, CaO and sodium carboxymethyl cellulose.
[0029] The collector A used in the positive flotation process of the present invention is one or more of kerosene and diesel.
[0030] The frother A used in the positive flotation process of the present invention is one or more of terpineol, methyl isobutyl carbinol and sec-octanol.
[0031] The air intake volume of the positive flotation process of the present invention is 40-60 L / h.
[0032] The invention discloses a method for purifying low-grade flake graphite ore by ion activation through direct-reverse flotation. During reverse flotation, the obtained graphite concentrate is mixed with water at a ratio of 10wt% to 20wt% of pulp concentration and added to a flotation tank, and stirred for 2 to 5 minutes to obtain pulp; then a pH adjuster is added to adjust the pH of the pulp to 5 to 8, and stirred for 2 to 5 minutes; an ion activator is added to the pulp with adjusted pH, and stirred for 2 to 5 minutes; a depressant B, a collector B and a frother B are sequentially added to the pulp with the ion activator and stirred respectively, and then an aeration switch is turned on, and reverse flotation is performed. After the reverse flotation is completed, the remaining pulp in the flotation tank is the flake graphite concentrate.
[0033] After the frothing is finished, the remaining pulp in the flotation tank is filtered and dried to obtain flake graphite concentrate.
[0034] When used in industry, turn on the aeration switch and scrape the foam for 4 to 9 minutes to complete the reverse flotation. After the reverse flotation scraping is completed, the remaining pulp in the flotation tank is filtered and dried to obtain flake graphite concentrate.
[0035] In the reverse flotation process, the present invention adds an ion activator in an amount of 80 to 320 g / t because the ion activator used in the present invention can react with the surface of impurities such as quartz, or selectively adsorb, thereby activating the surface, thereby enhancing the adsorption effect with the collector. However, if too little activator is added, the activation effect is not ideal, and too much activator will also cause the activator to form too many activation points on the mineral surface, resulting in reduced selectivity of the collector, thereby inhibiting the effective flotation separation of the target mineral. Different activators have different chemical reactions and adsorption characteristics with the surface of the target mineral. Other activators may not be able to form effective chemical bonds and adsorption with specific functional groups and ions on their surfaces, thereby failing to activate their surfaces. Moreover, the hydration of ions strongly affects the arrangement of ions at the gas-liquid interface, and the enrichment or depletion of ions at the gas-liquid interface changes the liquid film strength of the bubbles, thereby inhibiting the combination of bubbles, making the average size of the bubbles smaller and more stable. The presence of small bubbles is more conducive to combining with small-sized minerals during the reverse flotation process, thereby being more conducive to the separation of impurities and minerals.
[0036] As a preferred embodiment, the present invention provides a method for purifying low-grade flake graphite ore by positive-reverse flotation ion activation, during reverse flotation,
[0037] The obtained graphite concentrate is mixed with water at a ratio of 10% to 20% of the pulp concentration and added to the flotation tank, and stirred for 2 to 5 minutes to obtain pulp;
[0038] A pH adjuster is added to the obtained slurry to adjust the pH of the slurry to 5 to 8, and the slurry is stirred for 2 to 5 minutes.
[0039] As a preferred embodiment, the present invention provides a method for purifying low-grade flake graphite ore by positive-reverse flotation ion activation, during reverse flotation,
[0040] Add ion activator in an amount of 170-220 g / t to the pH-adjusted slurry and stir for 2-5 minutes.
[0041] For natural flake graphite ores whose impurities are mainly mica, quartz, feldspar and silicate, the ion activator is preferably at least one of CaCl2 and MgCl2.
[0042] As a further preference, for natural flake graphite ore whose impurities are mainly mica, quartz, feldspar and silicate, the ion activator is composed of a mixture of CaCl2 and MgCl2.
[0043] As a further preference, for natural flake graphite ore whose impurities are mainly mica, quartz, feldspar and silicate, the ion activator is composed of a mixture of MgCl2 and CaCl2, and the amount of MgCl2 added to the ion activator is greater than or equal to the amount of CaCl2 added.
[0044] As a further preference, for natural flake graphite ore whose impurities are mainly mica, quartz, feldspar and silicate, the amount of MgCl2 added in the ion activator is 95-125g / t, and the amount of CaCl2 added is 75-90g / t.
[0045] As a preferred embodiment, the present invention provides a method for purifying low-grade flake graphite ore by positive-reverse flotation ion activation, during reverse flotation,
[0046] Add an inhibitor in an amount of 1000-1300 g / t to the slurry after adding the ion activator, and stir for 2-5 minutes; then add a collector in an amount of 150-300 g / t to the slurry with the inhibitor, and stir for 2-5 minutes; then add a frother in an amount of 180-240 g / t to the slurry with the collector, and after stirring for 1-3 minutes, turn on the inflation switch, and then scrape the foam for 4-9 minutes. After the scraping foam is completed, the remaining slurry in the flotation tank is filtered and dried to obtain flake graphite concentrate, that is, graphite concentrate in the reverse flotation process, and the scraped foam is the tailings.
[0047] The pH adjusting agent used in the reverse flotation process of the present invention is one of HCl and H2SO4.
[0048] The collector B used in the reverse flotation process of the present invention is first mixed with hydrochloric acid or acetic acid in a ratio of 1:0.8 to 1:1.6, and then diluted to a 0.5% to 2% aqueous solution by adding hot water at a temperature of 35 to 50° C. and fully stirred to prepare the collector, wherein the amount of the collector is relative to the amount before the collector is mixed with the acid and hot water.
[0049] The air intake volume of the reverse flotation process of the present invention is 20 to 50 L / h.
[0050] The fixed carbon content of the graphite concentrate obtained in the reverse flotation process of the present invention is greater than or equal to 80%, and after optimization, the fixed carbon content is greater than or equal to 85%, and can even be greater than or equal to 90%.
[0051] In the present invention, the obtained large-sized flake graphite, for a single piece of large-sized flake graphite, has an equivalent radius of the largest side greater than or equal to 10 microns, and after optimization can be greater than or equal to 15 microns or even greater than or equal to 20 microns.
[0052] Compared with the prior art, the present invention has the following beneficial effects:
[0053] The present invention firstly adopts appropriate process and appropriate parameters to remove most of the impurities in the flake graphite ore by only one forward flotation, then adopts one reverse flotation to the forward flotation concentrate, and adds an appropriate amount of special ion activator in the reverse flotation process, which can not only protect the large-sized flake graphite from being destroyed, but also remove the small particle impurities entrained in the forward flotation process, and in the reverse flotation process, under the synergistic effect of ion activation and flotation process and its parameters, the fixed carbon content of the concentrate can be greatly increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 The figure is a flow chart of a specific implementation mode of the present invention.
[0055] Figure 2 These are SEM-EDS images of the positive flotation concentrate in Example 1, where (a) is a 2000-fold backscattered image of the positive flotation concentrate and (b) is a local surface scan energy spectrum of the positive flotation concentrate.
[0056] Figure 3 This is the SEM-EDS image of the entrainment of the positive flotation concentrate in Example 1.
[0057] Figure 4 This is the overall SEM-EDS image of the reverse flotation concentrate in Example 1.
[0058] Figure 5 This is a local SEM-EDS image of the reverse flotation concentrate in Example 1.
[0059] from Figure 1A process of a specific implementation of the present invention can be seen in FIG.
[0060] exist Figure 2 In the backscattered image, elements with different atomic numbers will show different brightness. The higher the atomic number, the brighter the contrast. Figure 2 (a) It can be seen that the white matter is impurities, while the black matter is graphite. There are still a lot of impurities in the positive flotation concentrate, and it is obvious that most of the impurities are smaller than graphite. The measurement shows that the size of impurities is mostly 6-12μm, while the size of graphite is mostly 18-30μm. Figure 2 (a) Figure 2 (b) It can be seen that the main impurity is silicon, and it also contains a small amount of aluminum, indicating that it contains more quartz and a small amount of aluminosilicate.
[0061] from Figure 3 It can be seen that a large number of small-sized impurities are gathered and carried away from the liquid surface by bubbles, resulting in a decrease in the fixed carbon content in the concentrate.
[0062] from Figure 4 It can be seen that Figure 4 and Figure 2 (a) The backscattered images of the positive flotation and reverse flotation concentrates at 2000 times magnification. After reverse flotation, Figure 4 Most of the impurities in the solution were removed, indicating that the reverse flotation process can effectively remove small-sized impurities.
[0063] from Figure 5 It can be seen that most of the impurities are removed, only a very small part of the impurities remain, and the surface of the flake graphite is smooth, and the large-sized flake graphite is well protected. DETAILED DESCRIPTION
[0064] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, the conventional conditions or the conditions recommended by the manufacturer are followed. The reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained commercially.
[0065] A method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation comprises the following steps:
[0066] (1) crushing the natural flake graphite ore with a fixed carbon content of 2.68% to 7.98% by a crusher to 8 to 35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then crushing it by a crushing and screening machine to 0.1 to 3 mm, accounting for more than 70%, to obtain a fine crushed product;
[0067] (2) grinding the finely crushed product with a sample preparation mill for 2 to 5 minutes, wherein the grinding particle size of -150 mesh accounts for more than 90%, thereby obtaining flake graphite ore;
[0068] (3) mixing the flake graphite ore obtained in step (2) with water at a ratio of 8% to 25% of the slurry concentration, adding the mixture to a flotation tank, and stirring for 2 to 5 minutes to obtain a slurry;
[0069] (4) adding a pH adjuster to the above slurry to adjust the pH of the slurry to 6 to 9, and stirring for 2 to 5 minutes;
[0070] (5) adding an inhibitor in an amount of 700 to 1300 g / t to the slurry after adjusting the pH, and stirring for 2 to 5 minutes;
[0071] (6) adding a collector at a dosage of 260 to 420 g / t to the slurry to which the inhibitor has been added, and stirring for 2 to 5 minutes;
[0072] (7) adding a frother in an amount of 150 to 300 g / t to the slurry to which the collector has been added, stirring for 1 to 3 minutes, turning on the aeration switch, and then scraping the foam for 3 to 12 minutes, filtering the scraped foam and drying to obtain a flake graphite roughing concentrate, i.e., a graphite concentrate in the positive flotation process, and the rest is tailings;
[0073] (8) mixing the graphite concentrate obtained in step (7) with water at a ratio of 10% to 20% of the slurry concentration, adding the mixture to a flotation tank, and stirring for 2 to 5 minutes to obtain a slurry;
[0074] (9) adding a pH adjuster to the slurry obtained in step (8) to adjust the pH of the slurry to 5 to 8, and stirring for 2 to 5 minutes;
[0075] (10) adding an ion activator in an amount of 80 to 320 g / t to the pH-adjusted slurry and stirring for 2 to 5 minutes;
[0076] (11) adding an inhibitor in an amount of 500 to 1300 g / t to the slurry after adding the ion activator, and stirring for 2 to 5 minutes;
[0077] (12) adding a collector in an amount of 120 to 380 g / t to the slurry to which the inhibitor has been added, and stirring for 2 to 5 minutes;
[0078] (13) Add a frother in an amount of 100 to 240 g / t to the slurry to which the collector has been added. After stirring for 1 to 3 minutes, turn on the aeration switch and then scrape the slurry for 4 to 9 minutes. After the scraping, filter the remaining slurry in the flotation tank and dry it to obtain flake graphite concentrate, i.e., graphite concentrate in the reverse flotation process, and the scraped foam is the tailings.
[0079] In a specific embodiment, the crusher in step (1) is a jaw crusher, and the crushing and screening machine is a roller crushing and screening machine.
[0080] In one specific embodiment, the aqueous solution used in step (3) is deionized water.
[0081] In a specific embodiment, the flotation machine used in step (3) is a XFG5-35 hanging tank flotation machine.
[0082] In a specific embodiment, the stirring process in steps (3) to (7) is carried out by stirring with a flotation machine impeller at a rotation speed of 800 to 1500 r / min.
[0083] In one specific embodiment, the pH adjuster used in step (4) is one of HCl, NaOH and CaO.
[0084] In a specific embodiment, the inhibitor used in step (5) is one or more of water glass, CaO, and sodium carboxymethyl cellulose.
[0085] In a specific embodiment, the collector used in step (6) is one of kerosene and diesel.
[0086] In a specific embodiment, the foaming agent used in step (7) is one of terpineol, methyl isobutyl carbinol and octanol.
[0087] In a specific embodiment, the air intake volume in step (7) is 40 to 60 L / h.
[0088] In one specific embodiment, the pH adjuster used in step (9) is one of HCl and H2SO4.
[0089] In a specific embodiment, the ionic activator used in step (10) is one or more of MgCl2, AlCl3 and CaCl2.
[0090] In a specific embodiment, the inhibitor used in step (11) is one or more of carboxymethyl cellulose and MF.
[0091] In a specific embodiment, the collector used in step (12) is one or more of monoamine, alkyl polyamine ether, ether monoamine, N-alkyl amide, dodecylamine, octadecylamine, kerosene and sodium oleate.
[0092] In a specific embodiment, the monoamine, alkyl polyamine ether, ether monoamine, N-alkylamide, dodecylamine and octadecylamine in the collector used in step (12) are first mixed with hydrochloric acid or acetic acid in a ratio of 1:0.8 to 1:1.6, and then diluted to a 0.5% to 2% aqueous solution by adding hot water at a temperature of 35 to 50° C. and fully stirred to prepare the collector, wherein the amount of the collector is relative to the amount of the collector before mixing with the acid and hot water.
[0093] In a specific embodiment, the foaming agent used in step (13) is one of terpineol and octanol.
[0094] In one specific embodiment, the air intake volume in step (13) is 20 to 50 L / h.
[0095] In one specific embodiment, the fixed carbon content of the graphite concentrate obtained in step (13) can reach 91.37%.
[0096] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.
[0097] Example 1-1
[0098] The XRD test results of natural flake graphite produced in a mining area in Hunan Province show that the impurities are mainly mica, quartz, feldspar and silicate. The composition is shown in Table 1.
[0099] Table 1 Composition of natural flake graphite from a mining area in Hunan (wt%)
[0100]
[0101] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 70%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 4 minutes, and the grinding particle size is -150 mesh, accounting for more than 90%, to obtain flake graphite ore;
[0102] The obtained flake graphite ore was mixed with water at a ratio of 25% of the pulp concentration and added to the flotation tank, stirred for 3 minutes to obtain a pulp, HCl was added to the pulp, the pH of the pulp was adjusted to 8, and stirred for 3 minutes;
[0103] Add 500 g / t water glass and 400 g / t sodium carboxymethyl cellulose as inhibitors to the slurry after adjusting the pH, and stir for 3 minutes; then add 320 g / t kerosene to the slurry, and stir for 3 minutes; then add 220 g / t pineneol to the slurry, and after stirring for 1 minute, turn on the aeration switch, adjust the air intake to 50 L / h, and then scrape the foam for 9 minutes, filter the scraped foam, and dry to obtain flake graphite positive flotation concentrate;
[0104] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 15% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain a pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 7, and stirred for 3 minutes;
[0105] Add ion activator in the amount of 120 g / t MgCl2 and 80 g / t CaCl2 to the slurry after adjusting pH, and stir for 4 minutes;
[0106] Add 700 g / t of inhibitor MF (formaldehyde condensate of sodium methylnaphthalene sulfonate) and 600 g / t of carboxymethyl cellulose to the slurry after adding the ion activator, and stir for 3 minutes;
[0107] Next, 160 g / t of dodecylamine and hydrochloric acid were mixed in a ratio of 1:1.2, and then diluted to a 1% aqueous solution by adding 40°C hot water and stirred thoroughly and added to the flotation tank, and 100 g / t of kerosene was added at the same time and stirred for 4 min;
[0108] To the slurry with the collector added, 190 g / t of 2-octanol as a foaming agent was added. After stirring for 1 minute, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 minutes. After the scraping was completed, the remaining slurry in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0109] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation product obtained through continuous expansion tests were: fixed carbon content of 91.37% and recovery rate of 74.55%.
[0110] Calculation of recovery rate: Assuming that the graphite content in the original ore is A, and the graphite content in the concentrate obtained after one flotation is B1, the recovery rate of one flotation is R1.
[0111]
[0112] If multiple flotation is performed, the recovery rate of each flotation is R1, R2, R3, ..., R n , then the total recovery rate R of multiple concentrations is
[0113] R=R1×R2×R3×…×R n
[0114] The graphite concentrate obtained by reverse flotation was concentrated in the presence of 300 g / t of water glass as an inhibitor, 160 g / t of kerosene as a collector and 110 g / t of pine alcohol as a frother. After one concentration, the fixed carbon content in the graphite concentrate increased to 95.31%.
[0115] Example 1-2
[0116] Other conditions are the same as those in Example 1-1, except that:
[0117] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 15% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain a pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 7, and stirred for 3 minutes;
[0118] Add ion activator at a dosage of 200 g / t MgCl2 to the pH-adjusted slurry and stir for 4 min;
[0119] Add 700 g / t of inhibitor MF and 600 g / t of carboxymethyl cellulose to the slurry after adding the ion activator, and stir for 3 minutes;
[0120] Next, 160 g / t of dodecylamine and hydrochloric acid were mixed in a ratio of 1:1.2, and then diluted to a 1% aqueous solution by adding 40°C hot water and stirred thoroughly and added to the flotation tank, and 100 g / t of kerosene was added at the same time and stirred for 4 min;
[0121] To the slurry with the collector added, 190 g / t of 2-octanol as a foaming agent was added. After stirring for 1 minute, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 minutes. After the scraping was completed, the remaining slurry in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0122] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 88.61% and recovery rate of 69.38%.
[0123] Examples 1-3
[0124] Other conditions are the same as those in Example 1-1, except that:
[0125] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 15% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain a pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 7, and stirred for 3 minutes;
[0126] Add ion activator at a dosage of 200 g / t CaCl2 to the pH-adjusted slurry and stir for 4 min;
[0127] Add 700 g / t of inhibitor MF and 600 g / t of carboxymethyl cellulose to the slurry after adding the ion activator, and stir for 3 minutes;
[0128] Next, 160 g / t of dodecylamine and hydrochloric acid were mixed in a ratio of 1:1.2, and then diluted to a 1% aqueous solution by adding 40°C hot water and stirred thoroughly and added to the flotation tank, and 100 g / t of kerosene was added at the same time and stirred for 4 min;
[0129] To the slurry with the collector added, 190 g / t of 2-octanol as a foaming agent was added. After stirring for 1 minute, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 minutes. After the scraping was completed, the remaining slurry in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0130] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 87.92% and recovery rate of 68.41%.
[0131] Examples 1-4
[0132] Other conditions are the same as those in Example 1-1, except that:
[0133] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 15% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain a pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 7, and stirred for 3 minutes;
[0134] Add ion activator in the amount of 100g / t CaCl2+100g / t MgCl2 to the pH-adjusted slurry and stir for 4 minutes;
[0135] Add 700 g / t of inhibitor MF and 600 g / t of carboxymethyl cellulose to the slurry after adding the ion activator, and stir for 3 minutes;
[0136] Next, 160 g / t of dodecylamine and hydrochloric acid were mixed in a ratio of 1:1.2, and then diluted to a 1% aqueous solution by adding 40°C hot water and stirred thoroughly and added to the flotation tank, and 100 g / t of kerosene was added at the same time and stirred for 4 min;
[0137] To the slurry with the collector added, 190 g / t of 2-octanol as a foaming agent was added. After stirring for 1 minute, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 minutes. After the scraping was completed, the remaining slurry in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0138] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 90.17% and recovery rate of 73.32%.
[0139] Examples 1-5
[0140] Other conditions are the same as those in Example 1-1, except that:
[0141] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 15% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain a pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 7, and stirred for 3 minutes;
[0142] Add ion activator in the amount of 120g / t CaCl2+80g / t MgCl2 to the pH-adjusted slurry and stir for 4 minutes;
[0143] Add 700 g / t of inhibitor MF and 600 g / t of carboxymethyl cellulose to the slurry after adding the ion activator, and stir for 3 minutes;
[0144] Next, 160 g / t of dodecylamine and hydrochloric acid were mixed in a ratio of 1:1.2, and then diluted to a 1% aqueous solution by adding 40°C hot water and stirred thoroughly and added to the flotation tank, and 100 g / t of kerosene was added at the same time and stirred for 4 min;
[0145] To the slurry with the collector added, 190 g / t of 2-octanol as a foaming agent was added. After stirring for 1 minute, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 minutes. After the scraping was completed, the remaining slurry in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0146] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 89.56% and recovery rate of 71.35%.
[0147] Example 2
[0148] The XRD test results of natural flake graphite produced in a mining area in Yunnan show that the impurities are mainly mica, quartz, feldspar and pyrite. Its composition is shown in Table 2.
[0149] Table 2 Composition of natural flake graphite in a mining area in Yunnan (wt%)
[0150]
[0151] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 70%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 4 minutes, and the grinding particle size is -150 mesh, accounting for more than 90%, to obtain flake graphite ore;
[0152] The obtained flake graphite ore was mixed with water at a pulp concentration ratio of 15% and added to a flotation tank, stirred for 3 minutes to obtain a pulp, NaOH was added to the pulp, the pH of the pulp was adjusted to 9, and stirred for 3 minutes;
[0153] Add 1100 g / t water glass as an inhibitor to the slurry after adjusting the pH, and stir for 3 minutes; then add 260 g / t diesel to it, and stir for 3 minutes; then add 210 g / t methyl isobutyl carbinol to it, and after stirring for 1 minute, turn on the inflation switch, adjust the air intake to 50 L / h, and then scrape the foam for 8 minutes, filter the scraped foam and dry it to obtain flake graphite positive flotation concentrate;
[0154] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 10% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 6, and stirred for 3 minutes;
[0155] Add 180 g / t MgCl2, an ion activator, to the pH-adjusted slurry and stir for 4 min;
[0156] Add 1300 g / t of inhibitor MF to the slurry after adding the ion activator, and stir for 3 minutes;
[0157] Next, 190 g / t N-alkylamide was mixed with hydrochloric acid in a ratio of 1:1, and then diluted to a 1% aqueous solution by adding 40°C hot water and stirred thoroughly and added to the flotation tank, while 80 g / t sodium oleate was added and stirred for 4 min;
[0158] To the ore pulp with the collector added, 200 g / t of terpineol as a foaming agent was added. After stirring for 1 minute, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 minutes. After the scraping was completed, the remaining ore pulp in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0159] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 89.16% and recovery rate of 72.91%.
[0160] Example 3
[0161] The XRD test results of natural flake graphite produced in a mining area in Henan Province show that the impurities are mainly mica, quartz and feldspar. The composition is shown in Table 3.
[0162] Table 3 Composition of natural flake graphite in a mining area in Henan
[0163]
[0164] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 70%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 4 minutes, and the grinding particle size is -150 mesh, accounting for more than 90%, to obtain flake graphite ore;
[0165] The obtained flake graphite ore was mixed with water at a ratio of 20% of the pulp concentration and added to the flotation tank, stirred for 3 minutes to obtain a pulp, HCl was added to the pulp, the pH of the pulp was adjusted to 8, and stirred for 3 minutes;
[0166] Add 1250 g / t water glass as an inhibitor to the slurry after adjusting the pH, and stir for 3 minutes; then add 250 g / t kerosene to it, and stir for 3 minutes; then add 240 g / t pineneol to it, and after stirring for 1 minute, turn on the aeration switch, adjust the air intake to 50 L / h, and then scrape the foam for 9 minutes, filter the scraped foam and dry it to obtain flake graphite positive flotation concentrate;
[0167] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 15% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain a pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 7, and stirred for 3 minutes;
[0168] Add 180 g / t AlCl3, an ion activator, to the pH-adjusted slurry and stir for 3 min;
[0169] Add 1200 g / t of inhibitor carboxymethyl cellulose to the slurry after adding the ion activator, and stir for 3 minutes;
[0170] Next, 280 g / t of alkyl polyamine ether and acetic acid were mixed in a ratio of 1:1.3, and then diluted to a 1.5% aqueous solution by adding 45°C hot water and stirred thoroughly and added to the flotation tank and stirred for 3 min;
[0171] To the slurry with the collector added, 240 g / t of octanol as a foaming agent was added. After stirring for 1 minute, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 minutes. After the scraping was completed, the remaining slurry in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0172] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 88.64% and recovery rate of 71.03%.
[0173] Comparative Example 1
[0174] The other conditions are the same as those in the forward flotation process in Example 1, except that reverse flotation is not performed; that is:
[0175] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 70%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 4 minutes, and the grinding particle size is -150 mesh, accounting for more than 90%, to obtain flake graphite ore;
[0176] The obtained flake graphite ore was mixed with water at a ratio of 25% of the pulp concentration and added to the flotation tank, stirred for 3 minutes to obtain a pulp, HCl was added to the pulp, the pH of the pulp was adjusted to 8, and stirred for 3 minutes;
[0177] To the slurry after adjusting the pH, 500 g / t water glass and 400 g / t sodium carboxymethyl cellulose as inhibitors were added and stirred for 3 minutes; then 320 g / t kerosene was added and stirred for 3 minutes; then 220 g / t pineneol was added, and after stirring for 1 minute, the aeration switch was turned on, the air intake was adjusted to 50 L / h, and then the foam was scraped for 9 minutes, and the scraped foam was filtered and dried to obtain flake graphite positive flotation concentrate.
[0178] During the flotation process, natural flake graphite ore was flotated at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 53.27% and recovery rate of 82.30%.
[0179] Comparative Example 2
[0180] The other conditions are the same as those in the forward-reverse flotation process in Example 1, except that no ion activator is added in the reverse flotation process; that is:
[0181] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 70%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 4 minutes, and the grinding particle size is -150 mesh, accounting for more than 90%, to obtain flake graphite ore;
[0182] The obtained flake graphite ore was mixed with water at a ratio of 25% of the pulp concentration and added to the flotation tank, stirred for 3 minutes to obtain a pulp, HCl was added to the pulp, the pH of the pulp was adjusted to 8, and stirred for 3 minutes;
[0183] Add 500 g / t water glass and 400 g / t sodium carboxymethyl cellulose as inhibitors to the slurry after adjusting the pH, and stir for 3 minutes; then add 320 g / t kerosene to the slurry, and stir for 3 minutes; then add 220 g / t pineneol to the slurry, and after stirring for 1 minute, turn on the aeration switch, adjust the air intake to 50 L / h, and then scrape the foam for 9 minutes, filter the scraped foam, and dry to obtain flake graphite positive flotation concentrate;
[0184] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 15% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain a pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 7, and stirred for 3 minutes;
[0185] Add 700 g / t of inhibitor MF and 600 g / t of carboxymethyl cellulose to the slurry after adjusting pH, and stir for 3 min;
[0186] Next, 160 g / t of dodecylamine and hydrochloric acid were mixed in a ratio of 1:1.2, and then diluted to a 1% aqueous solution by adding 40°C hot water and stirred thoroughly and added to the flotation tank, and 100 g / t of kerosene was added at the same time and stirred for 4 min;
[0187] To the slurry with the collector added, 190 g / t of 2-octanol as a foaming agent was added. After stirring for 1 minute, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 minutes. After the scraping was completed, the remaining slurry in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0188] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 83.91% and recovery rate of 72.13%.
[0189] Comparative Example 3
[0190] The other conditions are the same as those in the forward-reverse flotation process in Example 1, except that the amount of the ion activator used in the reverse flotation process is not within the protection range of the present invention of 80 to 320 g / t, that is:
[0191] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 70%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 4 minutes, and the grinding particle size is -150 mesh, accounting for more than 90%, to obtain flake graphite ore;
[0192] The obtained flake graphite ore was mixed with water at a ratio of 25% of the pulp concentration and added to the flotation tank, stirred for 3 minutes to obtain a pulp, HCl was added to the pulp, the pH of the pulp was adjusted to 8, and stirred for 3 minutes;
[0193] Add 500 g / t water glass and 400 g / t sodium carboxymethyl cellulose as inhibitors to the slurry after adjusting the pH, and stir for 3 minutes; then add 320 g / t kerosene to the slurry, and stir for 3 minutes; then add 220 g / t pineneol to the slurry, and after stirring for 1 minute, turn on the aeration switch, adjust the air intake to 50 L / h, and then scrape the foam for 9 minutes, filter the scraped foam, and dry to obtain flake graphite positive flotation concentrate;
[0194] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 15% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain a pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 7, and stirred for 3 minutes;
[0195] Add ion activator in the amount of 240 g / t MgCl2 and 160 g / t CaCl2 to the pH-adjusted slurry and stir for 4 minutes;
[0196] Add 700 g / t of inhibitor MF and 600 g / t of carboxymethyl cellulose to the slurry after adding the ion activator, and stir for 3 minutes;
[0197] Next, 160 g / t of dodecylamine and hydrochloric acid were mixed in a ratio of 1:1.2, and then diluted to a 1% aqueous solution by adding 40°C hot water and stirred thoroughly and added to the flotation tank, and 100 g / t of kerosene was added at the same time and stirred for 4 min;
[0198] To the slurry with the collector added, 190 g / t of 2-octanol as a foaming agent was added. After stirring for 1 minute, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 minutes. After the scraping was completed, the remaining slurry in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0199] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 79.33% and recovery rate of 67.60%.
[0200] Comparative Example 4
[0201] The other conditions are the same as those in the forward-reverse flotation process in Example 1, except that the dosage range of the inhibitor in the reverse flotation process is not within the protection range of the present invention of 500-1300 g / t, that is:
[0202] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 70%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 4 minutes, and the grinding particle size is -150 mesh, accounting for more than 90%, to obtain flake graphite ore;
[0203] The obtained flake graphite ore was mixed with water at a ratio of 25% of the pulp concentration and added to the flotation tank, stirred for 3 minutes to obtain a pulp, HCl was added to the pulp, the pH of the pulp was adjusted to 8, and stirred for 3 minutes;
[0204] Add 500 g / t water glass and 400 g / t sodium carboxymethyl cellulose as inhibitors to the slurry after adjusting the pH, and stir for 3 minutes; then add 320 g / t kerosene to the slurry, and stir for 3 minutes; then add 220 g / t pineneol to the slurry, and after stirring for 1 minute, turn on the aeration switch, adjust the air intake to 50 L / h, and then scrape the foam for 9 minutes, filter the scraped foam, and dry to obtain flake graphite positive flotation concentrate;
[0205] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 15% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain a pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 7, and stirred for 3 minutes;
[0206] Add ion activator in the amount of 120 g / t MgCl2 and 80 g / t CaCl2 to the slurry after adjusting pH, and stir for 4 minutes;
[0207] Add 800 g / t of inhibitor MF and 800 g / t of carboxymethyl cellulose to the slurry after adding the ion activator, and stir for 3 minutes;
[0208] Next, 160 g / t of dodecylamine and hydrochloric acid were mixed in a ratio of 1:1.2, and then diluted to a 1% aqueous solution by adding 40°C hot water and stirred thoroughly and added to the flotation tank, and 100 g / t of kerosene was added at the same time and stirred for 4 min;
[0209] To the slurry with the collector added, 190 g / t of 2-octanol as a foaming agent was added. After stirring for 1 minute, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 minutes. After the scraping was completed, the remaining slurry in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0210] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 78.63% and recovery rate of 62.80%.
[0211] Comparative Example 5
[0212] The other conditions are the same as those in the forward-reverse flotation process in Example 1, except that the amount of collector used in the reverse flotation process is not within the protection range of the present invention of 120 to 380 g / t, that is:
[0213] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 70%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 4 minutes, and the grinding particle size is -150 mesh, accounting for more than 90%, to obtain flake graphite ore;
[0214] The obtained flake graphite ore was mixed with water at a ratio of 25% of the pulp concentration and added to the flotation tank, stirred for 3 minutes to obtain a pulp, HCl was added to the pulp, the pH of the pulp was adjusted to 8, and stirred for 3 minutes;
[0215] Add 500 g / t water glass and 400 g / t sodium carboxymethyl cellulose as inhibitors to the slurry after adjusting the pH, and stir for 3 minutes; then add 320 g / t kerosene to the slurry, and stir for 3 minutes; then add 220 g / t pineneol to the slurry, and after stirring for 1 minute, turn on the aeration switch, adjust the air intake to 50 L / h, and then scrape the foam for 9 minutes, filter the scraped foam, and dry to obtain flake graphite positive flotation concentrate;
[0216] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 15% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain a pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 7, and stirred for 3 minutes;
[0217] Add ion activator in the amount of 120 g / t MgCl2 and 80 g / t CaCl2 to the slurry after adjusting pH, and stir for 4 minutes;
[0218] Add 700 g / t of inhibitor MF and 600 g / t of carboxymethyl cellulose to the slurry after adding the ion activator, and stir for 3 minutes;
[0219] Next, 240 g / t of dodecylamine and hydrochloric acid were mixed in a ratio of 1:1.2, and then diluted to a 1% aqueous solution by adding 40°C hot water and stirred thoroughly and added to the flotation tank, while 180 g / t of kerosene was added and stirred for 4 min;
[0220] To the slurry with the collector added, 190 g / t of 2-octanol as a foaming agent was added. After stirring for 1 minute, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 minutes. After the scraping was completed, the remaining slurry in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0221] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation products obtained through continuous expansion tests were: fixed carbon content of 81.29% and recovery rate of 68.35%.
[0222] Comparative Example 6
[0223] The other conditions are the same as those in the forward-reverse flotation process in Example 1, except that the amount of frother used in the reverse flotation process is not within the protection range of the present invention of 100-240 g / t, that is:
[0224] The natural flake graphite ore is first crushed by an XPC-100X60 jaw crusher to 8-35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then finely crushed by an XPS-Ф250×150 roller crusher and screener to 0.1-3 mm, accounting for more than 70%, to obtain a finely crushed product, and the obtained finely crushed product is ground by a sample preparation mill for 4 minutes, and the grinding particle size is -150 mesh, accounting for more than 90%, to obtain flake graphite ore;
[0225] The obtained flake graphite ore was mixed with water at a ratio of 25% of the pulp concentration and added to the flotation tank, stirred for 3 minutes to obtain a pulp, HCl was added to the pulp, the pH of the pulp was adjusted to 8, and stirred for 3 minutes;
[0226] Add 500 g / t water glass and 400 g / t sodium carboxymethyl cellulose as inhibitors to the slurry after adjusting the pH, and stir for 3 minutes; then add 320 g / t kerosene to the slurry, and stir for 3 minutes; then add 220 g / t pineneol to the slurry, and after stirring for 1 minute, turn on the aeration switch, adjust the air intake to 50 L / h, and then scrape the foam for 9 minutes, filter the scraped foam, and dry to obtain flake graphite positive flotation concentrate;
[0227] The graphite concentrate obtained by direct flotation was mixed with water at a ratio of 15% of the pulp concentration and added to the flotation tank, and stirred for 3 minutes to obtain a pulp; H2SO4 was added to the obtained pulp, the pH of the pulp was adjusted to 7, and stirred for 3 minutes;
[0228] Add ion activator in the amount of 120 g / t MgCl2 and 80 g / t CaCl2 to the slurry after adjusting pH, and stir for 4 minutes;
[0229] Add 700 g / t of inhibitor MF and 600 g / t of carboxymethyl cellulose to the slurry after adding the ion activator, and stir for 3 minutes;
[0230] Next, 160 g / t of dodecylamine and hydrochloric acid were mixed in a ratio of 1:1.2, and then diluted to a 1% aqueous solution by adding 40°C hot water and stirred thoroughly and added to the flotation tank, and 100 g / t of kerosene was added at the same time and stirred for 4 min;
[0231] To the slurry with the collector added, 300 g / t of octanol as a foaming agent was added. After stirring for 1 min, the aeration switch was turned on, the air intake was set to 30 L / h, and then the frothing was scraped for 7 min. After the scraping was completed, the remaining slurry in the flotation tank was filtered and dried to obtain flake graphite reverse flotation concentrate.
[0232] In the flotation process, the natural flake graphite ore was subjected to forward-reverse flotation at room temperature. The indicators of the flotation product obtained through continuous expansion tests were: fixed carbon content of 86.11% and recovery rate of 72.68%.
Claims
1. A method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation, characterized in that: The following steps are involved: Step 1 Crushing and Grinding Crushing and grinding the flake graphite ore until the grinding particle size of -150 mesh accounts for more than 90%, thereby obtaining flake graphite ore; Step 2: Positive flotation The obtained flake graphite ore is added to a flotation tank, and water is added for mixing to obtain a pulp, a pH adjuster is added to the pulp to adjust the pH of the pulp to 6-9, and then inhibitor A, collector A, and frother A are added in sequence, followed by flotation to obtain a graphite concentrate; Step 3: Reverse flotation The obtained graphite concentrate is mixed with water and added to a flotation tank to obtain a pulp; then a pH adjuster is added to adjust the pH of the pulp to 5-8, and then an ion activator is added, and then inhibitor B, collector B and frother B are added in sequence and stirred respectively, and then the aeration switch is turned on to perform reverse flotation, and the remaining pulp in the flotation tank is filtered and dried to obtain flake graphite concentrate; The ion activator is selected from at least one of MgCl2, AlCl3 and CaCl2; The inhibitor B used in the reverse flotation process is selected from at least one of carboxymethyl cellulose and formaldehyde condensate of sodium methyl naphthalene sulfonate; The collector B used in the reverse flotation process is selected from at least one of monoamine, alkyl polyamine ether, ether monoamine, N-alkyl amide, dodecylamine, octadecylamine, kerosene and sodium oleate; The frother B used in the reverse flotation process is selected from at least one of terpineol and octanol; During the reverse flotation process, ion activator is added at a dosage of 80-320 g / t, and inhibitor B is added at a dosage of 700-1300 g / t; Collector B is added in an amount of 260-420 g / t, and foaming agent is added in an amount of 150-300 g / t.
2. The method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation according to claim 1, characterized in that: The flake graphite ore is first coarsely crushed to obtain a coarse crushed product, and then finely crushed with a crushing and screening machine to obtain a fine crushed product. The fine crushed product is ground with a crusher to make the mineral particle size of -150 mesh account for more than 90%, thereby obtaining flake graphite ore.
3. The method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation according to claim 1, characterized in that: The natural flake graphite ore is coarsely crushed by a crusher to 8-35 mm, accounting for more than 70%, to obtain a coarse crushed product, and then finely crushed by a crushing and screening machine to 0.1-3 mm, accounting for more than 70%, to obtain a fine crushed product; the obtained fine crushed product is ground by a sample preparation crusher for 2-5 minutes, and the grinding particle size is -150 mesh, accounting for more than 90%, to obtain flake graphite ore.
4. The method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation according to claim 1, characterized in that: The flake graphite ore obtained by grinding treatment is added to a flotation tank, deionized water is added for mixing, and the flake graphite ore pulp is obtained by stirring for 2 to 5 minutes, a pH adjuster is added thereto, the pH of the pulp is adjusted to 6 to 9, and the pulp is stirred for 2 to 5 minutes; then inhibitor A and collector A are added thereto in sequence and stirred for 2 to 5 minutes respectively, and then a frother A is added thereto, after stirring for 1 to 3 minutes, the aeration switch is turned on, and then the foam is scraped for 3 to 12 minutes, and the scraped foam is the graphite concentrate; the pulp concentration of the flake graphite ore pulp is 8wt.% to 25wt.%, preferably 15wt.% to 25wt.%. The dosage of inhibitor A is 700 to 1300g / t, preferably 880 to 1260g / t; the dosage of collector A is 260 to 420g / t, and the dosage of frother A is 150 to 300g / t.
5. The method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation according to claim 1, characterized in that: The inhibitor A used in the positive flotation process is one or more of water glass, CaO, and sodium carboxymethyl cellulose; The collector A used in the positive flotation process is one or more of kerosene and diesel; The frother A used in the positive flotation process is one or more of terpineol, methyl isobutyl carbinol, and sec-octanol; The air intake volume during the positive flotation process is 40-60L / h.
6. The method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation according to claim 1, characterized in that: During reverse flotation, the obtained graphite concentrate is mixed with water at a ratio of 10wt% to 20wt% of pulp concentration and added to a flotation tank, and stirred for 2 to 5 minutes to obtain pulp; then a pH adjuster is added to adjust the pH of the pulp to 5 to 8, and stirred for 2 to 5 minutes; an ion activator is added to the pulp with adjusted pH, and stirred for 2 to 5 minutes; a depressant B, a collector B and a frother B are sequentially added to the pulp with the ion activator and stirred respectively, and then an aeration switch is turned on, and reverse flotation is performed. After the reverse flotation is completed, the remaining pulp in the flotation tank is the flake graphite concentrate.
7. The method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation according to claim 1, characterized in that: During reverse flotation, The obtained graphite concentrate is mixed with water at a ratio of 10% to 20% of the pulp concentration and added to the flotation tank, and stirred for 2 to 5 minutes to obtain pulp; Adding a pH adjuster to the obtained slurry to adjust the pH of the slurry to 5 to 8, and stirring for 2 to 5 minutes; During reverse flotation, add ion activator at a dosage of 170-220 g / t to the pH-adjusted pulp and stir for 2-5 minutes.
8. The method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation according to claim 1, characterized in that: For natural flake graphite ores whose impurities are mainly mica, quartz, feldspar and silicate, the ion activator is preferably at least one of CaCl2 and MgCl2. Preferably, for natural flake graphite ore whose impurities are mainly mica, quartz, feldspar and silicate, the ion activator is composed of a mixture of CaCl2 and MgCl2. As a further preference, for natural flake graphite ore whose impurities are mainly mica, quartz, feldspar and silicate, the ion activator is composed of a mixture of MgCl2 and CaCl2, and the amount of MgCl2 added to the ion activator is greater than or equal to the amount of CaCl2 added. As a further preference, for natural flake graphite ore whose impurities are mainly mica, quartz, feldspar and silicate, the amount of MgCl2 added in the ion activator is 95-125g / t, and the amount of CaCl2 added is 75-90g / t.
9. The method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation according to claim 1, characterized in that: During reverse flotation, Add an inhibitor in an amount of 1000-1300 g / t to the slurry after adding the ion activator, and stir for 2-5 minutes; then add a collector in an amount of 150-300 g / t to the slurry with the inhibitor, and stir for 2-5 minutes; then add a frother in an amount of 180-240 g / t to the slurry with the collector, and after stirring for 1-3 minutes, turn on the inflation switch, and then scrape the foam for 4-9 minutes. After the scraping foam is completed, the remaining slurry in the flotation tank is filtered and dried to obtain flake graphite concentrate, that is, graphite concentrate in the reverse flotation process, and the scraped foam is the tailings.
10. The method for purifying low-grade flake graphite ore by direct-reverse flotation ion activation according to claim 1, characterized in that: The pH adjuster used in the reverse flotation process is one of HCl and H2SO4; The collector B used in the reverse flotation process is first mixed with hydrochloric acid or acetic acid in a ratio of 1:0.8 to 1:1.6, and then diluted to a 0.5% to 2% aqueous solution by adding hot water at a temperature of 35 to 50°C and fully stirred to prepare the collector, wherein the amount of the collector is relative to the amount before the collector is mixed with the acid and hot water; The air intake volume during the reverse flotation process is 20-50L / h.
Citation Information
Patent Citations
Fine-flake graphite direct-reverse flotation purification technology
CN107537696A
Mixture of octene hydroformylation by-product and diesel, kereosene or c8-c20 olefines as collectors
CN113518667A