Method and system for efficiently and reliably welding zinc-aluminum-magnesium coating steel

By regulating the phase point power on the zinc-aluminum-magnesium steel plate through the global power modulation laser welding system, combined with cleaning and protective gas, the problem of welding instability and defects is solved, an efficient and reliable welding process is achieved, and the quality of zinc-aluminum-magnesium products is improved. Welding quality and application prospects.

CN118789097AInactive Publication Date: 2024-10-18LANZHOU UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411084187.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The welding process of zinc-aluminum-magnesium steel plates is complex. The difference in melting points leads to unstable welding and prone to spatter, white spots, pores and cracks. Uneven manual polishing increases costs and accuracy errors.

Method used

A global power modulation laser welding system is used to control the power of 36 phase points in a circular scanning cycle through the galvanometer laser. The coating is cleaned with low power in the first half and high-power welding in the second half, combined with protective gas to prevent oxidation.

Benefits of technology

It achieves efficient and reliable welding of galvanized aluminum-magnesium steel plates, reduces welding process requirements, improves welding efficiency and quality, reduces welding defects, and expands the application prospects of galvanized aluminum-magnesium products in the manufacturing industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118789097A_ABST
    Figure CN118789097A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of welding, discloses a method and a system for efficiently and reliably welding zinc-aluminum-magnesium coated steel, provides a method for regulating and controlling the power of a laser phase point of a zinc-aluminum-magnesium coated steel plate, develops a welding-following cleaning technology, reduces process requirements and improves welding efficiency. Regulating and controlling the structure form of the nickel-based alloy laser welding joint; the problems of splashing, white points, air holes, cracks and the like in zinc, aluminum and magnesium in the welding process are solved, and the narrow heat affected zone and low internal stress welding technology is achieved. A zinc-aluminum-magnesium coating plate product for welding the steel pipe is developed, and the application of the zinc-aluminum-magnesium coating plate product in the welding field is improved; according to the method, a solid technical theoretical basis is provided for welding of the zinc-aluminum-magnesium-plated steel, a new way is opened up for developing efficient and reliable welding products, and the prospect of zinc-aluminum-magnesium-plated steel materials in industrial application is greatly expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding, and in particular relates to a method and system for efficient and reliable welding of zinc-aluminum-magnesium coated steel. Background Art

[0002] The alloy coating of hot-dip galvanized aluminum-magnesium steel sheet is formed by high-temperature solidification of zinc (Zn), aluminum (Al), and magnesium (Mg). Its microstructure is composed of a dense ternary eutectic structure of Zn, Al, and MgZn2, so that a dense barrier is formed on the surface of the steel sheet that effectively prevents corrosion factors from penetrating. Hot-dip aluminum-zinc-magnesium steel sheet has good corrosion resistance and can be used in harsh environments to significantly improve the service life of the product. With the growing market demand for high-performance materials, the application of zinc-aluminum-magnesium steel sheet is also expanding. At present, a hot-rolled pickled plate (2.5-6.0mm) galvanized aluminum-magnesium combined unit with an annual output of 450,000 tons has been built. These units are mainly used in photovoltaic brackets, highway guardrails, underground pipe corridors, communication towers, steel plate warehouses, lamp poles, etc. However, in actual processing applications, zinc-aluminum-magnesium steel sheets are connected in various ways, including bolting, riveting, bonding, plugging and welding. Bolt connection is often used to connect different structural parts because of its simplicity and reliability; riveting and plug-in connection are often used to connect various alloy plates and load-bearing parts; although non-welding methods can achieve good connection effects, they also increase the processing and installation process and cost. At the same time, welding connection can achieve metallurgical bonding and provide better bonding effects. Therefore, in the actual processing process, welding technology is still an important means to reduce costs, improve production efficiency and connection reliability.

[0003] Table Comparison of physical and chemical properties of Zn, Al, Mg and Fe elements

[0004]

[0005] However, the welding process of zinc-aluminum-magnesium steel plate is more complicated than that of ordinary galvanized steel plate. In the welding process of zinc-aluminum-magnesium, it is mainly because the physical and chemical properties of the coating elements Zn, Al, Mg and the matrix element Fe are very different, as shown in the table above. In particular, the melting points of each element are very different. When the coating elements are all melted, the Fe element has not yet melted, and the liquid phase combination during the welding process cannot be guaranteed. The physical behavior of the multi-alloy welding process is complex, and the metallurgical reaction is complex, making it difficult to ensure the stability of the welding process. The weld width of arc welding is large and the heat input is large. The large amount of gasification of the coating zinc reduces the corrosion resistance of the galvanized steel weld. Secondly, there are great differences in the thermal expansion coefficient and thermal conductivity between magnesium / steel. There are large residual stresses and thermal stresses between magnesium / steel welded joints. At the same time, the low-melting-point substances in the zinc-aluminum-magnesium welding alloy will melt first, so solidification crack defects are prone to occur in the joints, affecting the performance of the joints. In addition, since welding is a process of rapid heating and cooling, when the molten pool solidifies, the zinc vapor and magnesium vapor have low boiling points and are mixed in the molten pool. If they are not removed in time, it will directly lead to pores, which can form small pores inside and on the surface of the weld. In the process of magnesium-aluminum welding, it is easy to produce brittle magnesium-aluminum intermetallic compounds, and such compounds have extremely high hardness and poor plasticity and toughness, which greatly reduces the performance of the joint and makes the joint easily oxidized. These shortcomings seriously affect the connection between zinc, magnesium and aluminum, such as Al3Mg2, Mg 17 Al 12 , Fe2Al5, FeAl3, etc. At the same time, these compounds will form intermetallic compounds different from the matrix during the solidification process, resulting in the formation of white spots on the weld surface.

[0006] Therefore, in order to ensure the quality of the weld and reduce welding defects, it is necessary to carry out careful pretreatment before welding the zinc-aluminum-magnesium steel plate, especially cleaning the surface of the steel plate, and grinding to remove the zinc-magnesium-aluminum coating to improve the welding quality. In the actual processing process, manual grinding will add a processing process, which will increase production costs and production time. On the other hand, manual grinding will lead to uneven and incomplete grinding, leaving the coating components in the area to be welded, affecting the welding quality; and manual grinding is prone to excessive cleaning, which will reduce the thickness of the substrate in the grinding area and affect the size and mechanical properties of the welded joint. In addition, it is necessary to consider the welding assembly grinding area, which will reserve a certain precision error, resulting in more zinc-magnesium-aluminum coating loss, which will undoubtedly increase the process requirements and costs.

[0007] In summary, how to achieve integrated forming with welding cleaning; how to regulate the microstructure of nickel-based alloy laser welding joints; how to solve the problems of spatter, white spots, pores, cracks, etc. in zinc, aluminum and magnesium during the welding process, and realize narrow heat-affected zone and low internal stress welding technology have become the contents to be discussed in this invention.

[0008] In view of the above problems of weld quality control in zinc-aluminum-magnesium welding manufacturing, the formation mechanism of the microstructure, the dynamic changes of the molten pool, and the metallurgical problems of zinc-aluminum-magnesium welding are analyzed during the welding process. The present invention attempts to design the mass transfer and heat transfer during the solidification of the molten pool, develop a method for laser molten pool shaping and control of galvanized aluminum-magnesium steel plates, and achieve one-time forming of the coating cleaning welding; regulate the organizational morphology of nickel-based alloy laser welded joints; solve the problems of spatter, white spots, pores, cracks, etc. in zinc-aluminum-magnesium during the welding process, and realize narrow heat-affected zone and low internal stress welding technology. Develop zinc-aluminum-magnesium coated plate products for welded steel pipes to improve the application of zinc-aluminum-magnesium products in the field of welding.

[0009] Through the above analysis, the problems and defects of the prior art are as follows:

[0010] (1) In the actual welding process, manual grinding of the plate before welding will lead to uneven and incomplete grinding, leaving the coating components in the area to be welded, affecting the welding quality;

[0011] (2) Manual grinding can easily lead to excessive cleaning, which reduces the thickness of the substrate in the grinding area and affects the mechanical properties of the welded joint.

[0012] (3) The welding assembly grinding area needs to be considered, and a certain precision error will be reserved, resulting in more zinc-magnesium-aluminum coating loss, which undoubtedly increases the welding process requirements and production costs. Summary of the invention

[0013] In view of the problems existing in the prior art, the present invention provides a method for efficient and reliable welding of zinc-aluminum-magnesium coated steel.

[0014] The present invention is achieved in that a method for efficient and reliable welding of zinc-aluminum-magnesium coated steel comprises:

[0015] Step 1, changing the laser power modulation mode, and regulating 36 phase points in the circular scanning track within a circular scanning cycle of the galvanometer laser;

[0016] Step 2: During laser welding, a low-power laser is used to clean the zinc-aluminum-magnesium steel plate coating in the first half of the circular scanning cycle along the welding forward direction;

[0017] Step 3: Use a larger power to weld the steel plate in the second half of the scanning cycle.

[0018] Further, specifically including:

[0019] Step 1: Assemble two zinc-aluminum-magnesium coated steel plates on a welding test platform in a butt-jointed manner, with a reserved gap of less than 0.5 mm between the two test plates, and fix them with a clamping device;

[0020] Step 2: Adjust the height of the laser welding head so that the upper surface of the test plate is at the position where the laser beam defocus is 0.

[0021] Step 3, set up the welding gas protection device on the welding platform, set the protective gas nozzle to align with the welding pool area and form an angle of 45° with the test plate plane;

[0022] Step 4, set the global power modulation laser control parameters: laser power 3.6kW, welding speed 30mm / s, oscillation amplitude 0.4mm, three sets of scanning frequencies 100Hz, 150Hz, 200Hz respectively, and set the laser beam scanning trajectory to a circle;

[0023] Step 5, changing the laser power modulation mode, and regulating 36 phase points of the global power laser within a circular scanning cycle of the galvanometer laser;

[0024] Step 6: During laser welding, along the welding forward direction, 18 phase points in the first half of the circular scanning cycle are set to a lower laser power to clean the surface coating of the zinc-aluminum-magnesium steel plate;

[0025] Step 7, 18 phase points in the second half of the circular scanning cycle are set to a higher laser power to weld the steel plate after the coating is cleaned;

[0026] Step 8, during welding, the laser welding head is fixed, and a welding test is performed using a mobile welding test platform, and the laser and the welding test platform are started and stopped synchronously;

[0027] Step 9: The shielding gas is turned on 5 seconds before the laser is started, and the shielding gas is stopped for 10 seconds after the laser is stopped to continue to protect the weld surface and prevent it from oxidation.

[0028] Furthermore, the zinc-aluminum-magnesium steel plate has a size of 160×70×1.5 mm, and the welding form is butt welding.

[0029] Furthermore, the welding equipment adopts a full-range power modulation laser welding system with dual functions of "laser galvanometer + power modulation".

[0030] Another object of the present invention is to provide a system for efficient and reliable welding of zinc-aluminum-magnesium coated steel, comprising:

[0031] The control module is used to change the laser power modulation mode and control the 36 phase points of the global power laser within a circular scanning cycle of the galvanometer laser;

[0032] The cleaning module is used to clean the zinc-aluminum-magnesium steel plate coating with a low-power laser in the first half of the circular scanning cycle along the welding forward direction during laser welding;

[0033] The welding module is used to weld the steel plates with a higher power in the second half of the scanning cycle.

[0034] Another object of the present invention is to provide a computer device, comprising a memory and a processor, wherein the memory stores a computer program, and when the computer program is executed by the processor, the processor executes the steps of the method for efficient and reliable welding of zinc-aluminum-magnesium coated steel.

[0035] Another object of the present invention is to provide a computer-readable storage medium storing a computer program, which, when executed by a processor, enables the processor to execute the steps of the method for efficient and reliable welding of zinc-aluminum-magnesium coated steel.

[0036] Another object of the present invention is to provide an information data processing terminal, which is used to implement a system for efficient and reliable welding of zinc-aluminum-magnesium coated steel.

[0037] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:

[0038] First, in view of the technical problems existing in the above-mentioned prior art and the difficulty of solving the problems, the technical solutions to be protected by the present invention and the results and data during the research and development process are closely combined to analyze in detail and deeply how the technical solutions of the present invention solve the technical problems, and some creative technical effects brought about after solving the problems. The specific description is as follows:

[0039] The present invention provides a method for controlling the power of laser phase points of galvanized aluminum-magnesium steel plates, develops a welding cleaning technology, combines the pre-welding coating cleaning process in the welding process of galvanized aluminum-magnesium steel plates with the welding process, reduces the welding process requirements, reduces the welding production process, and improves the welding efficiency; on the other hand, power-modulated galvanometer laser welding can control the organizational morphology of the welded joint; reduces the spatter, white spots, pores, cracks and other problems that occur in the welding process of galvanized aluminum-magnesium steel plates, and realizes a narrow heat-affected zone and low internal stress welding technology. The welding quality of galvanized aluminum-magnesium steel plates is improved, and efficient and reliable welding manufacturing of galvanized aluminum-magnesium steel plates is realized, which expands the application prospects of galvanized aluminum-magnesium products in the manufacturing industry.

[0040] The present invention successfully achieves efficient welding of galvanized aluminum-magnesium steel through innovative welding cleaning technology. The technology adopts a full-range power modulation laser welding system to accurately control the power size and speed of 36 phase points. First, in a circular scanning cycle of galvanometer laser welding, the weld area to be welded is pre-cleaned with lower power in the first half of the scanning cycle to effectively remove surface pollutants and oxide layers. Then, in the second half of the scanning cycle, the power is increased to weld the galvanized aluminum-magnesium steel. This power modulation laser welding strategy significantly reduces the process requirements for surface treatment before welding, making the welding of complex components more feasible, and greatly improving the welding efficiency. Compared with traditional arc welding, the full-range power modulation laser welding technology significantly improves the comprehensive mechanical properties of the welded joint while achieving good metallurgical bonding, and effectively overcomes the common defects of pores, cracks, and coarse welded joints in traditional welding methods. In addition, since the full-range power laser welding has a smaller heat-affected zone, it reduces the degree of damage to the base metal coating during welding, thereby reducing the coating spray width after welding, reducing the post-welding treatment process of zinc-aluminum-magnesium coated steel plates, and improving production efficiency. The present invention not only provides a solid technical theoretical basis for the welding of galvanized aluminum-magnesium steel, but also opens up a new path for the development of efficient and reliable welding products, greatly expanding the prospects of galvanized aluminum-magnesium steel materials in industrial applications.

[0041] Second, as auxiliary evidence of the inventiveness of the claims of the present invention, it is also reflected in the following important aspects:

[0042] (1) The expected benefits and commercial value of the technical solution of the present invention after transformation are:

[0043] The power-modulated laser welding cleaning technology for galvanized aluminum-magnesium steel plates of the present invention reduces the pre-weld coating cleaning and polishing steps in the welding manufacturing process, saves time costs, reduces welding process requirements, and improves welding production efficiency; on the other hand, compared with other welding methods, the laser welding cleaning technology of the present invention can effectively reduce the generation of welding defects such as spatter, pores, and cracks in the welding process of galvanized aluminum-magnesium steel plates, effectively improves the welding quality of galvanized aluminum-magnesium steel plates, and provides a solid technical foundation for the development of efficient and reliable welding products.

[0044] (2) The technical solution of the present invention solves a technical problem that people have been eager to solve but have never been able to solve successfully:

[0045] The technical solution of the present invention solves the welding process problems such as pores, spatter, cracks, etc. existing in the welding production and manufacturing process of galvanized aluminum-magnesium steel plates for new energy storage cabinets, and solves the technical difficulties of unqualified weld surface quality and substandard mechanical properties in the welding production of galvanized aluminum-magnesium steel plates.

[0046] Third, compared with the prior art, the method for efficient and reliable welding of zinc-aluminum-magnesium coated steel provided by the present invention has brought significant technological progress through sophisticated process parameter settings and innovative welding strategies.

[0047] 1) Improved welding quality: Through the precise setting of global power modulation laser control parameters, including laser power, welding speed, oscillation amplitude and scanning frequency, as well as the optimized design of the laser beam scanning trajectory (circular trajectory), the heat input during the welding process is made more uniform, thereby significantly improving the quality and strength of the welded joint.

[0048] 2) Enhanced coating protection effect: This method uses a phased laser power modulation mode during the welding process. In the first half, a lower power is used to clean the surface coating of the zinc-aluminum-magnesium steel plate, effectively removing the surface oxides and impurities, creating better conditions for the subsequent welding process; in the second half, a higher power is used for welding to ensure the depth and strength of the welding. This phased treatment method not only protects the coating, but also improves welding efficiency and quality.

[0049] 3) Improved welding efficiency: By carrying out welding tests on a mobile welding test platform, the laser and the welding test platform can be started and stopped synchronously, which simplifies the operation process, shortens the welding cycle, and thus improves production efficiency.

[0050] 4) Optimization of weld protection: The timing and duration of the use of shielding gas are precisely controlled, effectively preventing the weld from oxidation during the welding process, further improving the quality and durability of the weld. The shielding gas is turned on in advance before the laser is started, and continues to protect for a period of time after the laser stops, ensuring the safety of the weld throughout the welding process.

[0051] In summary, this method of efficient and reliable welding of zinc-aluminum-magnesium coated steel significantly improves the welding quality, efficiency and weld protection effect through innovative process parameter settings and welding strategies, making important contributions to technological progress in related fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 This is a flow chart of a method for efficient and reliable welding of zinc-aluminum-magnesium coated steel provided by an embodiment of the present invention;

[0053] Figure 2 This is a system structure diagram for efficient and reliable welding of zinc-aluminum-magnesium coated steel provided by an embodiment of the present invention;

[0054] Figure 3 Schematic diagram of global power modulation laser welding provided by an embodiment of the present invention; (a) galvanometer laser system, (b) gradient power setting, (c) scanning path;

[0055] Figure 41 is a heat source distribution diagram under different laser modes provided by an embodiment of the present invention; (a) is a plane diagram of arc heat source distribution, (b) is a stereogram of (a), (c) is a plane diagram of global power modulated laser heat source distribution, and (d) is a stereogram of (c);

[0056] Figure 5 The present invention provides a schematic diagram of a tensile specimen and a tensile load-displacement curve diagram of full-range power modulated laser and arc welding;

[0057] Figure 6 The following are microscopic morphology diagrams of different welding methods provided by the embodiments of the present invention; (a) optical microstructure of arc weld (b) arc electron microscope microstructure (c) optical microstructure of full-domain power modulated laser weld (d) full-domain power modulated laser electron microscope microstructure;

[0058] Figure 7 The following are the element distribution diagrams of the galvanized aluminum-magnesium steel weld surface under different welding methods provided in the embodiments of the present invention; (a), (c), and (e) are the element distributions of Al, Mg, and Zn on the arc weld surface; (b), (d), and (f) are the element distributions of Al, Mg, and Zn on the full-domain power modulated laser weld surface. DETAILED DESCRIPTION

[0059] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0060] Industrial application: Welding of zinc-aluminum-magnesium coated steel in automobile manufacturing

[0061] In the automobile manufacturing process, zinc-aluminum-magnesium coated steel is widely used in the welding of body and chassis structures. This material has excellent corrosion resistance, but its coating is easily damaged during traditional welding, resulting in unstable welding quality. To solve this problem, an efficient welding method based on global power modulation laser technology is adopted.

[0062] 1) Assembly and fixing:

[0063] Assemble two zinc-aluminum-magnesium coated steel plates in a butt-jointed manner on a welding test platform, leaving a gap of less than 0.5 mm, and fix them with a clamping device to ensure that the plates are stable and do not move.

[0064] 2) Laser head adjustment:

[0065] Adjust the height of the laser welding head so that the upper surface of the test plate is located at a position where the laser beam defocus is 0, to ensure that the laser beam is accurately focused on the welding area.

[0066] 3) Protective gas device:

[0067] Set up the welding gas protection device, set the shielding gas nozzle to aim at the welding pool area and form a 45° angle with the test plate plane to provide effective gas protection and prevent oxidation.

[0068] 4) Laser parameter setting:

[0069] The global power modulation laser control parameters were set as follows: the laser power was 3.6 kW, the welding speed was 30 mm / s, the oscillation amplitude was 0.4 mm, the three scanning frequencies were 100 Hz, 150 Hz, and 200 Hz, and the laser beam scanning trajectory was circular.

[0070] 5) Phase point control:

[0071] In one circular scanning cycle of the galvanometer laser, 36 phase points are precisely controlled. The first 18 phase points use low-power laser to clean the surface coating of the zinc-aluminum-magnesium steel plate, and the last 18 phase points use high-power laser to weld the cleaned steel plate.

[0072] 6) Mobile welding platform:

[0073] During laser welding, the laser welding head is fixed and the welding test is carried out using a mobile welding test platform. The laser and the welding test platform are started and stopped synchronously to ensure the accuracy of the welding trajectory.

[0074] 7) Protective gas operation:

[0075] The shielding gas is turned on 5 seconds before the laser starts, and the shielding gas is stopped 10 seconds after the laser stops, so as to continue to protect the weld surface and prevent it from oxidation.

[0076] Effect:

[0077] Improve welding quality: Through precise phase point laser power control, the coating can be effectively cleaned and high-quality welding can be achieved, with uniform welds and no pores.

[0078] Enhanced welding efficiency: Global power modulation laser technology significantly improves welding speed and efficiency to meet the needs of large-scale production in automotive manufacturing.

[0079] Prevent oxidation: The optimized setting and delayed closing operation of the shielding gas device effectively prevents weld oxidation and ensures welding quality.

[0080] This welding method based on global power modulation laser technology has broad application prospects in the automotive manufacturing industry and can significantly improve the welding quality and production efficiency of zinc-aluminum-magnesium coated steel.

[0081] like Figure 1 As shown, a method for efficient and reliable welding of zinc-aluminum-magnesium coated steel provided by an embodiment of the present invention comprises the following steps:

[0082] S101, changing the laser power modulation mode, and regulating 36 phase points of the global power laser within a circular scanning cycle of the galvanometer laser;

[0083] S102, during laser welding, the zinc-aluminum-magnesium steel plate coating is cleaned by using a low-power laser in the first half of the circular scanning cycle along the welding forward direction;

[0084] S103, in the second half of the scanning cycle, a larger power is used to weld the steel plate.

[0085] The zinc-aluminum-magnesium steel plate provided in the embodiment of the present invention has a size of 160×70×1.5 mm, and the welding form is butt welding.

[0086] The welding equipment provided in the embodiment of the present invention adopts a full-range power modulation laser welding system with the dual functions of "laser galvanometer + power modulation".

[0087] like Figure 2 As shown, a system for efficient and reliable welding of zinc-aluminum-magnesium coated steel provided by an embodiment of the present invention comprises:

[0088] The control module is used to change the laser power modulation mode and control the 36 phase points of the global power laser within a circular scanning cycle of the galvanometer laser;

[0089] The cleaning module is used to clean the zinc-aluminum-magnesium steel plate coating with a low-power laser in the first half of the circular scanning cycle along the welding forward direction during laser welding;

[0090] The welding module is used to weld the steel plates with a higher power in the second half of the scanning cycle.

[0091] Another object of the present invention is to provide a computer device, comprising a memory and a processor, wherein the memory stores a computer program, and when the computer program is executed by the processor, the processor executes the steps of the method for efficient and reliable welding of zinc-aluminum-magnesium coated steel.

[0092] Another object of the present invention is to provide a computer-readable storage medium storing a computer program, which, when executed by a processor, enables the processor to execute the steps of the method for efficient and reliable welding of zinc-aluminum-magnesium coated steel.

[0093] Another object of the present invention is to provide an information data processing terminal, which is used to implement a system for efficient and reliable welding of zinc-aluminum-magnesium coated steel.

[0094] The present invention is specifically implemented:

[0095] The present invention provides a method for controlling the laser phase point power of galvanized aluminum-magnesium steel plates, develops a welding cleaning technology, reduces process requirements, and improves welding efficiency; controls the organizational morphology of nickel-based alloy laser welded joints; solves the problems of spatter, white spots, pores, cracks, etc. in the zinc, aluminum, and magnesium during the welding process, and realizes a narrow heat-affected zone and low internal stress welding technology. Develop zinc, aluminum, and magnesium coated plate products for welded steel pipes to improve the application of zinc, aluminum, and magnesium products in the field of welding.

[0096] The example material of the present invention is a zinc-aluminum-magnesium coated steel plate provided by Jiuquan Iron and Steel (Group) Co., Ltd. for welding test. The size of the welding test plate is 160×70×1.5mm, and the welding form is butt welding.

[0097] The welding equipment adopts a full-range power modulation laser welding system with dual functions of "laser galvanometer + power modulation". The structure of the system is as follows: Figure 3 As shown in a. The global power modulation laser welding system is based on the original laser scanning galvanometer welding system, and the power control function is added through research and development. In a closed motion cycle (360°), the power size of up to 36 phase points can be controlled, and each phase point can be adjusted dynamically. By setting the welding parameters of each of the 36 phase points of the global power modulation laser, precise control of the welding process can be achieved.

[0098] The combined use of the two functions can realize the autonomous setting of the laser power waveform and phase within the scanning cycle. Compared with the traditional laser scanning galvanometer welding system, the global power modulation laser welding system has a larger control space and more precise control ability for the heat and mass transfer process of the molten pool. For comparison, the welding test uses a traditional laser characterized by a Gaussian heat source and a global power modulation laser for welding. The welding parameters are shown in Table 1. Figure 3 b is a schematic diagram of the power setting of phase points in a single scanning domain when the global power modulated laser realizes gradient power input. The size of the red dots corresponds to the power level, and the power difference between adjacent phase points is 5%. Figure 3 c is the scanning path of full-range power modulated laser welding. As a comparison, the welding test uses the traditional arc welding characterized by Gaussian heat source and the full-range power modulated laser welding comparison experiment. Each test plate is polished with sandpaper to remove the surface oxide film, and the surface oil is cleaned with acetone to reduce the experimental differences caused by different welding test plates.

[0099] Before the welding experiment, the welding shielding gas was argon with a purity of 99.99% and a gas flow rate of 15 L min -1 .

[0100] For conventional arc welding: current 110A, welding speed 135mm·min -1, there is no controllable phase point, no oscillation frequency and oscillation amplitude, forming a traditional Gaussian heat source distribution.

[0101] For global power modulation laser control: laser power 3.6kW, welding speed 30mm / s. The global power modulation laser scanning frequencies are 100Hz, 150Hz, and 200Hz respectively. The oscillation amplitude is 0.4mm. In order to avoid the accumulation of heat at the edge of the molten pool due to the superposition of scanning paths and cause overheating of the heat-affected zone, the energy input at the edge of the scanning domain is reduced.

[0102] Figure 3 Schematic diagram of global power modulation laser welding

[0103] (a) Galvanometer laser system, (b) gradient power setting, (c) scanning path

[0104] Table 1 Welding parameters of two welding methods

[0105]

[0106] The present invention changes the laser power modulation mode (such as Figure 3 c) In one circular scanning cycle of the galvanometer laser, the 36 phase points of the global power laser are regulated ( Figure 3 b) During laser welding, the zinc-aluminum-magnesium steel plate coating is cleaned with low-power laser in the first half of the circular scanning cycle along the welding forward direction, and the steel plate is welded with higher power in the second half of the scanning cycle, which avoids the problem of grinding and cleaning the workpiece before welding of zinc-aluminum-magnesium steel products, realizes the welding cleaning technology, reduces the process requirements during welding, and improves the welding efficiency. At the same time, it avoids the problems of slag inclusion and spatter of coating elements, and improves the welding quality.

[0107] 3. Processing results

[0108] Figure 4 Heat source distribution diagram under different laser modes

[0109] (a) Plane diagram of arc heat source distribution, (b) is a stereogram of (a) (c) is a plane diagram of laser heat source distribution with full power modulation, (d) is a stereogram of (c)

[0110] Figure 4The heat source and molten pool model under different laser heat sources can be observed. It can be observed that the traditional laser spot diameter is small, while the global power modulation laser is spiral-shaped and has a certain amplitude, so that the nickel-based alloy is heated evenly. Secondly, by controlling the power size of 36 phase points, the heat of the molten pool can be precisely controlled. At the same time, the laser beam oscillation can disperse the laser power in the welding joint area, increase the molten pool width of the weld metal, thereby reducing gas concentration, and allowing the gas to overflow the molten pool in a larger area, reducing the generation of pores. In addition, the flow behavior of the molten pool from bottom to top will further promote gas flow and facilitate overflow. At the same time, the global power modulation laser will have a certain oscillation frequency and amplitude during the welding process, increase the fluidity of the molten pool, and avoid the phenomenon that the gas does not overflow and fuse when the weld solidifies. Furthermore, the global power modulation laser can control the power size of each phase point, control the heat input of the weld, reduce thermal stress, and reduce the possibility of joint solidification crack defects. Therefore, the global power modulation laser welding joint significantly reduces the influence range of the heat affected zone and improves the welding quality.

[0111] Figure 5 Schematic diagram of the tensile specimen and the tensile load-displacement curve of full-range power modulated laser and arc welding

[0112] The tensile test of zinc-magnesium-aluminum steel plates welded by arc welding and full-range power modulation laser welding was carried out using a sample tensile machine. The tensile sample fracture effect diagram and the sample tensile-load strain curve are shown in Figure 5 . It can be observed from the figure that the arc welding tensile specimen broke in the heat affected zone of the black joint, while the full-range power modulation galvanometer laser welding tensile specimen broke in the base material part, and the tensile strength of the joint tensile specimen under full-range power modulation was higher than that of the arc welding joint tensile specimen, and with the increase of load, the welding load displacement of the zinc-magnesium-aluminum steel plate under full-range power modulation laser welding was about 12mm, while that of arc welding was about 8.5mm, indicating that the plasticity and toughness of the heat affected zone of the arc welding joint were poor. The quality of the full-range power modulation laser welding joint is significantly higher than that of the arc welding. At the same time, the galvanometer scanning function of the full-range power modulation laser has a stirring effect on the molten pool, avoiding defects such as pores during welding. At the same time, during full-domain power modulation laser welding, a low-power laser is used in the first half of the scanning cycle to clean the zinc-magnesium-aluminum steel plate coating first, and then a high-power laser is used in the second half of the scanning cycle to weld the steel plate, which can obtain better welding joint quality and reduce the melting of zinc-magnesium-aluminum steel plate coating elements into the weld metal. In particular, the Al element in the coating will enter the weld and react metallurgically with the Fe element in the matrix, which is very easy to generate brittle intermetallic compounds such as Fe2Al5 and FeAl3, which have a certain impact on the microstructure, element distribution, and mechanical properties of the welded joint. Full-domain power modulation laser realizes the function of welding cleaning during welding, avoiding the problem of complex zinc-aluminum-magnesium coated workpieces being unable to be polished during welding, ensuring the quality of the welded joint and reducing the process requirements.

[0113] Figure 5 The following are the fracture effect diagrams of the tensile specimens of the welded joints prepared by TIG welding and power modulation laser welding processes and the load displacement curves of the tensile specimens. The tensile test found that the fracture position of the TIG welding tensile specimen was in the heat affected zone, with small necking. It can be clearly seen from the load displacement curve of the tensile specimen that the tensile displacement of the TIG welding tensile specimen was significantly smaller than that of the power modulation laser welding tensile specimen, indicating that the heat affected zone of the TIG welding joint is a weak area of ​​mechanical properties and has poor plasticity. The fracture position of the power modulation laser welding tensile specimens was the base material area, and the base material on both sides of the fracture had obvious necking and fractured at the base material with the most serious necking, indicating that the strength of the power modulation laser welding joint is not lower than that of the base material. In summary, the plasticity of the power modulation laser welding joint is significantly higher than that of the TIG self-melting welding joint.

[0114] Figure 6 Microstructures under different welding methods

[0115] (a) Light microstructure of arc weld (b) Microscopic morphology of arc electron microscope (c) Light microstructure of full-range power modulated laser weld (d) Microscopic morphology of full-range power modulated laser electron microscope

[0116] The microstructure of the welded joint was characterized and observed in depth by optical microscopy and scanning electron microscopy. Figure 6 The microstructure comparison under different welding methods is shown. Figure 6 a) and electron microscopy images ( Figure 6 b), obvious microstructure coarsening was observed, among which a large amount of coarse Widmanstätten structures were clearly visible. This strip-like distribution of ferrite and carbide not only reduces the toughness and plasticity of the material and increases its brittleness, but also makes it more likely to cause fracture when subjected to impact or stress. The uneven distribution of hardness and strength further affects the overall performance of the material. In contrast, the metallographic image of the full-range power modulated laser welded joint ( Figure 6 c) and electron microscopy images ( Figure 6 d) reveals a completely different microstructure. Here, a large number of elongated ferrite and cementite are observed to be alternately stacked to form a uniform layered structure. This structure not only retains the plastic toughness of ferrite, but also optimizes the mechanical properties of the material through the strength contribution of cementite. This uniform microstructure significantly improves the stability and reliability of the weld under complex stress conditions, especially during the welding process, significantly improving the comprehensive mechanical properties of the weld. Figure 5This is further confirmed by the tensile displacement curve. The uneven Widmanstatten structure of arc welding leads to a significant decrease in weld plasticity, which is much lower than the uniform fine structure of full-range power modulated laser welding. The Gaussian heat source mode of arc welding is prone to coarsening due to the concentrated heat source and high unit heat input. The application of full-range power modulated laser welding technology effectively improves the reliability of welded joints by avoiding heat source concentration. The present invention not only provides a solid technical theoretical support for the welding of zinc-aluminum-magnesium steel, but also develops high-reliability and high-performance welding products. This opens up broader prospects for the application of zinc-aluminum-magnesium steel in the field of component connection, and foreshadows its important role and potential in modern industry.

[0117] Figure 6 This is the microstructure of the center area of ​​the weld of the TIG welding and power modulated laser welding joints. It can be seen from the figure that the microstructure of the power modulated laser welding joint is obviously smaller than that of the TIG welding joint. The fine microstructure can improve the mechanical properties of the welding joint. This also proves from the microstructural level that the mechanical properties of the power modulated laser welding joint are higher than those of the TIG welding joint.

[0118] In summary, power modulation laser welding can effectively improve the mechanical properties of welded joints, and the application of full-range power modulation laser welding technology effectively improves the quality of welded joints. The present invention not only provides a solid technical theoretical support for the welding of zinc-aluminum-magnesium steel, but also develops welding products with high reliability and high performance.

[0119] Figure 7 Element distribution on the weld surface of galvanized aluminum-magnesium steel under different welding methods

[0120] (a), (c), (e) Element distribution on arc weld surface

[0121] (b), (d), (f) Surface element distribution of full-domain power modulated laser weld

[0122] The experiment used a scanning electron microscope (SEM) combined with an energy dispersive spectrometer (EDS) to conduct qualitative and quantitative analysis of zinc (Zn), aluminum (Al), magnesium (Mg) and other elements on the weld surface. Figure 7 As shown, the arc welding joint surface ( Figure 7c and e) significantly show the distribution characteristics of these elements. In particular, low-melting-point metals Zn and Mg melt into the weld during welding, but due to the extremely low solid solubility between Mg and Fe and the absence of stable intermetallic compounds, the metallurgical bonding between the two is poor. In addition, the physical property parameters of Mg and Fe are significantly different, which easily generates thermal stress and thermal deformation during welding, making it easy for Mg to enter the weld in the form of slag inclusions, increasing the risk of crack formation at the magnesium alloy / steel interface. At the same time, due to its high melting point, ZnO is not easy to escape during welding and is prone to form slag inclusions, further affecting the plasticity of the weld. In contrast, the full-range power modulation laser welding technology is used to clean the surface coating of the galvanized aluminum-magnesium steel plate at a lower power at the beginning of welding, effectively removing the low-melting-point Zn and Mg metal coatings on the surface. Subsequently, the steel is welded by increasing the power to avoid the mixing of these insoluble metals and ZnO slag inclusions, thereby protecting the plastic toughness of the weld and improving the crack resistance of the weld. This can be seen from the surface of the full-range power modulation laser welding head ( Figure 7 d and f) was confirmed in the element distribution, and almost no Zn and Mg metal elements were detected in the weld area, ensuring the excellent mechanical properties of the welded joint. In addition, due to the characteristics of the Gaussian heat source distribution of arc welding, the heat-affected zone is large, which easily leads to burning and cracking of the zinc-aluminum-magnesium coating around the weld. The full-range power modulation laser welding technology not only reduces the heat input, but also reduces the impact on the protective coating. This experiment was welded on galvanized aluminum-magnesium steel without any grinding and polishing treatment. Although Al easily reacts with oxygen to form a high-melting-point aluminum oxide protective film, the full-range power laser can only remove part of the surface oxide film, but even so, the surface microstructure distribution of the resulting weld is still better than that of arc welding. The present invention provides technical guarantee for the welding of galvanized aluminum-magnesium steel, reduces the pretreatment requirements of the welding process, ensures that the sample can be smoothly welded even without pretreatment, significantly improves the application potential of galvanized aluminum-magnesium steel products in the manufacture of complex components, and greatly improves welding efficiency.

[0123] In summary, the present invention successfully achieves efficient welding of galvanized aluminum-magnesium steel through innovative welding cleaning technology. This technology uses a full-range power modulation laser welding system to accurately control the power size and speed of 36 phase points. First, in a circular scanning cycle of galvanometer laser welding, the weld area to be welded is pre-cleaned with lower power in the first half of the scanning cycle to effectively remove surface pollutants and oxide layers. Subsequently, in the second half of the scanning cycle, the power is increased to weld the galvanized aluminum-magnesium steel. This power modulation laser welding strategy significantly reduces the process requirements for surface treatment before welding, making the welding of complex components more feasible, while greatly improving the welding efficiency. Compared with traditional arc welding, the full-range power modulation laser welding technology significantly improves the comprehensive mechanical properties of the welded joint while achieving good metallurgical bonding, effectively overcoming the common defects of poor organizational properties in traditional welding methods. In addition, since the full-range power laser welding has a smaller heat-affected zone, it reduces the degree of damage to the base metal coating during welding, thereby reducing the coating spray width after welding, reducing the post-welding treatment process of zinc-aluminum-magnesium coated steel plates, and improving production efficiency. The present invention not only provides a solid technical theoretical basis for the welding of galvanized aluminum-magnesium steel, but also opens up a new path for the development of efficient and reliable welding products, greatly expanding the prospects of galvanized aluminum-magnesium steel materials in industrial applications.

[0124] The specific application field of the present invention is the manufacturing of new energy storage cabinets. In addition, various fields that require the use of galvanized aluminum-magnesium steel plates for production and manufacturing, such as photovoltaic manufacturing, automobile manufacturing, equipment manufacturing, light steel construction, etc., can use this technical solution to perform laser welding manufacturing of galvanized aluminum-magnesium steel plates, such as photovoltaic brackets and 5G base station construction in the photovoltaic manufacturing field, Huawei's new energy storage equipment, light steel structure buildings, underground pipe galleries, etc.

[0125] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for efficient and reliable welding of zinc-aluminum-magnesium coated steel, characterized in that: Through the global power modulation laser technology, several phase points are precisely controlled within a circular scanning cycle of the laser. Low-power laser is used to clean the coating at some phase points, and high-power laser is used for welding at other phase points. At the same time, combined with precise laser head height adjustment, optimized setting of the protective gas device and synchronous operation of the mobile welding platform, the welding quality and efficiency are significantly improved, and weld oxidation is effectively prevented.

2. The method for efficient and reliable welding of zinc-aluminum-magnesium coated steel as claimed in claim 1, characterized in that: The following steps are involved: Step 1: Assemble two zinc-aluminum-magnesium coated steel plates on a welding test platform in a butt-jointed manner, with a reserved gap of less than 0.5 mm between the two test plates, and fix them with a clamping device; Step 2, adjust the height of the laser welding head so that the upper surface of the test plate is located at a laser beam defocus amount of 0; Step 3, set up the welding gas protection device on the welding platform, set the protective gas nozzle to align with the welding pool area and form an angle of 45° with the test plate plane; Step 4, set the global power modulation laser control parameters: laser power 3.6kW, welding speed 30mm / s, oscillation amplitude 0.4mm, three sets of scanning frequencies 100Hz, 150Hz, 200Hz respectively, and set the laser beam scanning trajectory to a circle; Step 5, changing the laser power modulation mode, and regulating 36 phase points of the global power laser within a circular scanning cycle of the galvanometer laser; Step 6: During laser welding, along the welding forward direction, 18 phase points in the first half of the circular scanning cycle are set to a lower laser power to clean the surface coating of the zinc-aluminum-magnesium steel plate; Step 7, 18 phase points in the second half of the circular scanning cycle are set to a higher laser power to weld the steel plate after the coating is cleaned; Step 8, during welding, the laser welding head is fixed, and a welding test is performed using a mobile welding test platform, and the laser and the welding test platform are started and stopped synchronously; Step 9: The shielding gas is turned on 5 seconds before the laser is started, and the shielding gas is stopped for 10 seconds after the laser is stopped to continue to protect the weld surface and prevent it from oxidation.

3. The method for efficient and reliable welding of zinc-aluminum-magnesium coated steel as claimed in claim 2, characterized in that: The zinc-aluminum-magnesium steel plate has a size of 160×70×1.5 mm, and the welding method is butt welding.

4. The method for efficient and reliable welding of zinc-aluminum-magnesium coated steel as claimed in claim 1, characterized in that: The welding equipment adopts a full-range power modulation laser welding system with dual functions of "laser galvanometer + power modulation".

5. The method for efficient and reliable welding of zinc-aluminum-magnesium coated steel as claimed in claim 1, characterized in that: During welding, the welding shielding gas is argon with a purity of 99.99% and a gas flow rate of 15L·min -1 .

6. The method for efficient and reliable welding of zinc-aluminum-magnesium coated steel as claimed in claim 1, characterized in that: For the global power modulation laser parameter control: laser power 3.6kW, welding speed 30mm / s, defocus 0mm, global power modulation laser scanning frequencies are 100Hz, 150Hz, 200Hz respectively, and the oscillation amplitude is 0.4mm.

7. The method for efficient and reliable welding of zinc-aluminum-magnesium coated steel as claimed in claim 1, characterized in that: During a circular scanning cycle of the galvanometer laser, 36 phase points of the global power laser are regulated; the laser power of 18 phase points in the first half of the scanning cycle is set to 40%-50% of the full power, that is, low-power laser is used to clean the zinc-aluminum-magnesium steel plate coating; the laser power of 18 phase points in the second half of the scanning cycle is set to 100% of the full power, that is, high-power laser is used to weld the steel plate.

8. A system for efficient and reliable welding of zinc-aluminum-magnesium coated steel for implementing the method for efficient and reliable welding of zinc-aluminum-magnesium coated steel as claimed in any one of claims 1 to 7, characterized in that: The system for efficient and reliable welding of zinc-aluminum-magnesium coated steel comprises: The control module is used to change the laser power modulation mode and control the 36 phase points of the global power laser within a circular scanning cycle of the galvanometer laser; The cleaning module is used to clean the zinc-aluminum-magnesium steel plate coating with a low-power laser in the first half of the circular scanning cycle along the welding forward direction during laser welding; The welding module is used to weld the steel plates with a higher power in the second half of the scanning cycle.

Citation Information

Cited By

  • Dissimilar metal power modulation galvanometer laser welding method

    CN119566523A