Electrocrack healing method for additive manufacturing of TC4 titanium alloy
By using pulse power supply to perform electro-crack healing on additively manufactured TC4 titanium alloy components in a vacuum environment, the problem of titanium alloy crack defects in additive manufacturing is solved, efficient and rapid material repair is achieved, and the strength of the material is improved. Plasticity and application range.
Patent Information
- Application Number
- CN202410894407.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-18
AI Technical Summary
During the additive manufacturing process, titanium alloy components are prone to crack defects, resulting in reduced material reliability. Existing repair methods such as traditional composite rolling and high-temperature heat treatment are time-consuming and labor-intensive, affecting material performance.
The pulse power supply is used in a vacuum environment to perform electrical crack healing on TC4 titanium alloy components. The pulse current generates thermal compressive stress to close the cracks and achieve rapid repair.
It achieves high-quality and high-efficiency healing of titanium alloys, improves the material's strong plasticity and application range, simplifies operations, saves energy and is environmentally friendly, and avoids adverse effects on the alloy structure and mechanical properties.
Smart Images

Figure CN118789154A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of titanium alloy defect repair, and specifically relates to an electro-crack healing method for additively manufactured TC4 titanium alloy. Background Art
[0002] In order to reduce the weight of the aircraft, increase the life of the aircraft, and reduce manufacturing costs, the use of large integral key structural parts in aircraft structures is increasing, and its forming and manufacturing technology is considered to be one of the core manufacturing technologies that have an important impact on the development and production of aircraft industrial equipment. TC4 titanium alloy is not only light in weight, but also has high strength and high temperature resistance. It is currently the largest titanium alloy material used in titanium alloy integral structural parts, such as the rear fuselage reinforcement frame of the US F-22, the central wing box of the F-14, and the central wing edge strip of the C919 aircraft.
[0003] In recent years, it has been found that titanium alloys prepared by additive manufacturing technology can effectively reduce material waste and processing costs, and have been used as load-bearing structures in the aviation field. However, during the additive manufacturing process, the components undergo periodic, non-steady-state cyclic heating and cooling, and steps, pores, microcracks, and unfused defects will inevitably appear in the molded parts. The presence of these defects will reduce the effective bearing area of the material, and as a typical source of stress concentration, they will induce fatigue crack nucleation and even promote crack propagation, causing the reliability of parts to decline rapidly. It is one of the most common causes of component failure, especially microcracks inside metal materials, which is regarded as a major problem in the reliability service of additively manufactured components, so certain control measures should be taken.
[0004] Traditional composite rolling process, hot isostatic pressing and high-temperature heat treatment methods are time-consuming, labor-intensive and expensive to solve the above problems. They also require additional stress or overall heating of the sample, affecting its microstructure and mechanical properties. As a result, it is currently impossible to achieve high-efficiency and high-quality defect repair of titanium alloy materials prepared by additive manufacturing technology. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention proposes an electro-crack healing method for additively manufactured TC4 titanium alloy, which quickly repairs crack defects of additively manufactured TC4 titanium alloy components through electric pulse technology, thereby improving their strength and plasticity and expanding their scope of application.
[0006] The present invention is achieved through the following technical solutions:
[0007] An electrical crack healing method for additively manufactured TC4 titanium alloy utilizes a pulse power supply to heat the TC4 titanium alloy to be crack-healed in a vacuum environment to achieve crack healing of the TC4 titanium alloy.
[0008] Preferably, the vacuum degree of the vacuum environment is ≤10 -3 Pa.
[0009] Preferably, the TC4 titanium alloy to be crack-healed is placed in a glove box, connected to a pulse power supply, and subjected to a heating treatment after being evacuated.
[0010] Furthermore, the TC4 titanium alloy placed in the glove box is connected to the positive electrode and the negative electrode of the pulse power supply respectively.
[0011] Furthermore, copper braided belts are used as electrodes to connect the TC4 titanium alloy to the positive electrode and the negative electrode of the pulse power supply respectively.
[0012] Preferably, the pulse power supply uses a pulse voltage of 55-60V to heat the TC4 titanium alloy whose cracks are to be healed.
[0013] Furthermore, the TC4 titanium alloy to be crack-healed is heated at a pulse voltage of 55-60V for 10-20min to achieve crack healing treatment of the TC4 titanium alloy.
[0014] Preferably, after the TC4 titanium alloy with cracks healed is heated, it is air-cooled to complete the crack healing process of the TC4 titanium alloy.
[0015] Furthermore, after the heating of the TC4 titanium alloy with healed cracks is completed, the pulse power supply is turned off and the alloy is air-cooled in a glove box to complete the crack healing process of the TC4 titanium alloy.
[0016] Preferably, after the pulse power supply is turned off, the heated TC4 titanium alloy is air-cooled to room temperature in a glove box to complete the crack healing treatment of the TC4 titanium alloy.
[0017] Compared with the prior art, the present invention has the following beneficial technical effects:
[0018] The present invention discloses an electric crack healing method for additively manufactured TC4 titanium alloy. In a vacuum environment, pulse current treatment is performed on the additively manufactured crack-damaged TC4 titanium alloy. Due to the Joule heat effect and the tip flow effect, a certain thermal compressive stress is generated at the crack tip to make it close quickly, and finally the additively manufactured titanium alloy crack is healed with high quality and high efficiency, thereby improving its strength and plasticity and expanding its application range. Pulse current treatment can effectively improve the defects of the additively manufactured alloy structure, such as coarse β columnar crystals, pores and poor fusion, and can also achieve the effect of stress relief annealing. At the same time, this method can effectively inhibit the abnormal coarsening of β grains and weaken the continuous α phase at the grain boundary, and will neither increase the α / β transition temperature nor affect the matrix structure of the defect-free area. At present, traditional hot rolling, hot isostatic pressing and high-temperature heat treatment are mostly used for titanium alloy microstructure regulation and defect repair. Either additional stress needs to be applied or the entire sample needs to be heated, which will affect the alloy structure and mechanical properties to a certain extent. The present invention does not require external heating field and stress field. It can achieve the electro-healing effect of TC4 titanium alloy cracks in additive manufacturing in a short time by only adjusting the pulse voltage of electric pulse heating. The operation is simple, fast and efficient, and it is energy-saving and environmentally friendly. It has significant advantages and has good application prospects in the field of defect repair of additively manufactured metal materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Microstructure of the crack tip of additively manufactured TC4 titanium alloy before 55V / 10min pulse heating treatment.
[0020] Figure 2 Microstructure of crack tip of additively manufactured TC4 titanium alloy after pulse heating treatment at 55V / 10min.
[0021] Figure 3 Microstructure of the crack tip of additively manufactured TC4 titanium alloy after pulse heating treatment at 58V / 15min.
[0022] Figure 4 Microscopic morphology of cracks in additively manufactured TC4 titanium alloy before 60V / 20min energy pulse treatment.
[0023] Figure 5 Microscopic morphology of cracks in additively manufactured TC4 titanium alloy after 60V / 20min energy pulse treatment. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0025] The present invention provides an electric crack healing method for additively manufactured TC4 titanium alloy, taking a TC4 titanium alloy sample prepared by additive manufacturing technology as an example, and is specifically implemented according to the following steps:
[0026] Step 1: Place the crack-damaged TC4 titanium alloy sample in a glove box, and use copper braided belts as electrodes to connect the sample to the positive and negative electrodes of a pulse power supply;
[0027] Step 2: Evacuate the glove box to a vacuum level of 10 -3 Pa or less to prevent the sample from being oxidized during heating;
[0028] Step 3: Turn on the power of the pulse equipment, set the pulse voltage to 55-60V and the processing time to 10-20 minutes, use the pulse current to quickly heat the TC4 titanium alloy sample. After the heating is completed, turn off the pulse power and air cool to room temperature in the glove box to repair the crack defects of the TC4 titanium alloy;
[0029] Example 1
[0030] (1) Place the TC4 titanium alloy crack specimen in a glove box and connect the specimen to the positive and negative electrodes of the copper braided belt of a pulse power supply;
[0031] (2) Vacuum the glove box to a vacuum degree of 10 -3 Pa, this operation is to prevent the sample from being oxidized during pulse heating;
[0032] (3) Turn on the power of the pulse equipment, set the pulse voltage to 55V, continue heating for 10 minutes, perform rapid heating treatment on the TC4 titanium alloy crack specimen, turn off the power, wait for it to cool to room temperature, and then remove it;
[0033] (4) After the pulse treatment, the sample was ground and electropolished using HF and HNO 3 The mixed solution of HF, HNO 3 The volume ratio of MgO and deionized water is 1:2:5, and the microstructure of the sample is observed using a metallographic microscope.
[0034] After the initial sample is processed in step (4), Figure 1 It can be seen that the initial crack tip width is 30-50 μm. Figure 2 After high-energy pulse treatment, the crack tip width is sharply reduced or even closed, the crack tip width is reduced to 2-5μm, the total length of the crack healing area reaches 250μm, and the new crack tip no longer has a tendency to continue to expand, that is, the defect repair effect is achieved.
[0035] Example 2
[0036] (1) A crack-damaged TC4 titanium alloy sample was placed in a glove box and connected to the positive and negative electrodes of a copper braided belt of a high-energy pulse power supply;
[0037] (2) To prevent the sample from being oxidized during heating, the glove box was evacuated to a vacuum degree of 7×10 -4 Pa;
[0038] (3) Turn on the power of the pulse equipment, set the pulse voltage to 58 V, and perform rapid heating treatment on the cracked specimen for 15 minutes. Turn off the power and wait for it to cool to room temperature before removing it;
[0039] (4) After the cracked specimens were treated with pulse current, they were ground and electropolished using HF and HNO 3 The mixed solution of HF, HNO 3 The volume ratio of MgO and deionized water is 1:2:5, and the microstructure of the sample is observed using a metallographic microscope.
[0040] Figure 3 This is a metallographic photograph of the crack after 58V / 15min pulse heating treatment. Crack bridging and closure appear in this area, and holes of varying sizes are formed in some areas. The crack healing length shown in the figure is about 180μm. In addition, after high-voltage long-term pulse treatment, the newly generated grains cross the original cracks to form a whole, indicating that the pulse current treatment has effectively caused partial healing of the through cracks in the material.
[0041] Example 3
[0042] (1) Place the crack-damaged TC4 titanium alloy specimen in a glove box and connect it to the positive and negative electrodes of the copper braided belt of a pulse power supply;
[0043] (2) The glove box was evacuated to a vacuum degree of 4×10 -4 Pa;
[0044] (3) Turn on the power of the pulse equipment, set the pulse voltage to 60 V, and perform rapid heating treatment on the cracked specimen for 20 minutes. After the heating is completed, air cool to room temperature and then remove the specimen;
[0045] (4) The samples after electric pulse treatment are polished and the microstructure of the samples is observed using a metallographic microscope.
[0046] Figure 4 and Figure 5 These are the microscopic morphologies of the original long crack of the crack-damaged sample and the healed area after pulse treatment. It can be seen that the initial crack is slender, and the width between the crack surfaces gradually decreases from the middle to the lower end of the crack. By observing the enlarged morphology of the crack after pulse treatment, it can be found that multiple healing areas appear at the original crack position, and the healing lengths vary from 100 to 200 μm. This is because the thermal-compressive stress generated by the Joule heating effect and the tip flow effect causes obvious healing.
[0047] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that this is only for illustration and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.
Claims
1. A method for electrically induced crack healing in additively manufactured TC4 titanium alloy, characterized in that: The TC4 titanium alloy to be crack-healed is heated in a vacuum environment by using a pulse power supply to achieve crack healing treatment of the TC4 titanium alloy.
2. The electric crack healing method for additively manufacturing TC4 titanium alloy according to claim 1, wherein the vacuum degree of the vacuum environment is ≤10 -3 Pa.
3. According to the electro-crack healing method of additively manufactured TC4 titanium alloy according to claim 1, the TC4 titanium alloy to be crack-healed is placed in a glove box, then connected to a pulse power supply, and subjected to a heating treatment after vacuuming.
4. According to the electric crack healing method of additively manufactured TC4 titanium alloy according to claim 3, the TC4 titanium alloy placed in the glove box is connected to the positive electrode and the negative electrode of the pulse power supply respectively.
5. According to the electro-crack healing method of additively manufactured TC4 titanium alloy according to claim 4, copper braided belts are used as electrodes, and the TC4 titanium alloy is connected to the positive electrode and the negative electrode of a pulse power supply respectively.
6. According to the electrical crack healing method of additively manufactured TC4 titanium alloy according to claim 1, the pulse power supply uses a pulse voltage of 55-60V to heat the TC4 titanium alloy to be crack-healed.
7. According to the electric crack healing method for additively manufactured TC4 titanium alloy according to claim 6, the TC4 titanium alloy to be crack-healed is heated at a pulse voltage of 55-60V for 10-20min to achieve crack healing treatment of the TC4 titanium alloy.
8. According to the electric crack healing method for additively manufactured TC4 titanium alloy according to claim 3, after the TC4 titanium alloy with cracks healed is heated, it is air-cooled to complete the crack healing process of the TC4 titanium alloy.
9. According to the electrical crack healing method for additively manufactured TC4 titanium alloy as described in claim 8, after the heating of the TC4 titanium alloy with cracks healed is completed, the pulse power supply is turned off and air-cooled in a glove box to complete the crack healing treatment of the TC4 titanium alloy.
10. According to the electric crack healing method for additively manufactured TC4 titanium alloy according to claim 9, after the pulse power supply is turned off, the heated TC4 titanium alloy is air-cooled to room temperature in a glove box to complete the crack healing treatment of the TC4 titanium alloy.
Citation Information
Cited By
Nickel-based hard-surface alloy layer defect healing method
CN122322816A
Electric pulse in-situ self-repairing method for fatigue early cracks of aluminum alloy component