Manganese-nickel-aluminum bronze alloy welding wire and preparation method and application thereof
Through the preparation of manganese-nickel-aluminum bronze alloy welding wire, the problems of insufficient strength and corrosion resistance of existing welding wires are solved, the high-performance performance of the welding wire in high-strength, highly corrosive environments is achieved, and the service life of the hydraulic support is extended.
Patent Information
- Application Number
- CN202411193708.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-10-18
AI Technical Summary
The existing aluminum bronze alloy welding wire used for coal machine welding has insufficient strength and corrosion resistance and cannot meet the use needs of coal machine equipment in high-strength and highly corrosive environments, resulting in a short service life of the hydraulic support.
The manganese-nickel-aluminum bronze alloy welding wire is prepared through vacuum melting, hot rolling, cold forging, forward hot extrusion, solution quenching and continuous variable diameter cold drawing to increase the Sn element and increase the content of Ni and Mn. , forming Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy and forming a precipitation strengthening phase to improve the strength and corrosion resistance of the welding wire.
Significantly improves the strength and corrosion resistance of the welding wire, prolongs the service life of the hydraulic support, and can maintain stable performance in harsh environments. It is suitable for overlay welding of cast iron, non-alloy steel and low alloy steel with high corrosion resistance requirements. .
Smart Images

Figure BDA0005015770140000101 
Figure HDA0005015770150000011 
Figure HDA0005015770150000012
Abstract
Description
Technical Field
[0001] The invention belongs to the field of advanced metal processing and relates to a manganese-nickel-aluminum bronze alloy welding wire and a preparation method and application thereof. Background Art
[0002] In the disposable energy structure, coal has always been in a dominant position. At present, coal resource consumption accounts for more than 70% of the total disposable energy. Although the country has vigorously developed new energy in recent years, the dominant position of coal as a disposable energy will not change in the future. According to the forecast of relevant departments, by 2030, coal will still account for 56% of the total energy demand, and even by 2050, it will still account for about 50%.
[0003] Due to the poor working conditions and harsh working conditions of coal mining equipment, the service life of coal mining equipment is generally low, generally about 5 years. In addition, the development of mechanized coal mining has higher and higher requirements for the performance and functions of coal mining products, resulting in a large number of coal mining products being scrapped or eliminated prematurely. Therefore, the performance improvement of coal mining equipment has become a major problem. The rapid development of coal mining equipment corresponds to the development and changes in coal demand. As the core hydraulic support in coal mining equipment, since the 1980s, the world's major coal mining countries have been working hard to reduce production, reduce manpower and improve efficiency, reduce costs, and realize centralized production in mines. They actively develop and apply new technologies to develop a new generation of high-performance and high-reliability heavy hydraulic supports for coal mining. After more than 20 years of development, although my country's hydraulic supports have achieved remarkable results, there is still a certain gap in the overall level with the world's advanced coal mining countries. The technical content of domestic hydraulic supports is low, and materials are the main problem.
[0004] At the same time, with the decrease in the proportion of equipment demand for new mines, the renovation of existing coal mining equipment has increased from 55% in 2011 to about 75% in 2015. How to effectively utilize a large number of scrapped and obsolete products, remanufacture coal mining equipment products, realize the secondary utilization of resources, effectively reduce resource waste, and avoid environmental pollution has become an effective way for my country's coal production enterprises to solve the problems of production equipment demand and capital shortage in the current predicament. At the same time, carrying out the research and development of key remanufacturing technologies and expanding the coal mining equipment remanufacturing business has also become a way for coal mining equipment R&D and manufacturing enterprises to enhance their competitiveness.
[0005] Welding technology is the most important processing technology in the manufacturing of hydraulic supports for coal mines. Due to the complex structure of hydraulic supports, the welding workload is large. The quality of welding work directly determines the quality of hydraulic support manufacturing and will also have a great impact on engineering safety. The most important factor affecting welding quality is welding materials. After the hydraulic support is welded, the first requirement is that the weld metal should have mechanical properties close to the parent material in the welding state, which is conducive to improving the comprehensive performance of the joint. Secondly, the selection of welding materials adopts the principle of "equal strength" combined with the principle of "low 1 to 2 levels" to ensure the plastic toughness of the weld. Therefore, when selecting welding materials, it is necessary to ensure that the strength, toughness and plasticity of the weld meet the design requirements. Selecting welding materials according to the principle of "equal strength" is the primary principle of welding material selection, which can help ensure that the hydraulic support has a higher welding stability and ensure that it can be used in actual production.
[0006] Chinese patent application CN116921919A discloses an aluminum bronze alloy welding wire for coal machine welding and a preparation method thereof. The welding wire has insufficient strength and corrosion resistance and cannot adapt to high-strength requirements and high-corrosive use environments. Summary of the invention
[0007] In order to solve the above problems of the prior art, the present invention provides a manganese-nickel-aluminum-bronze alloy welding wire and a preparation method and application thereof. The welding wire has higher strength and corrosion resistance and can extend the service life of the hydraulic support.
[0008] The present invention is achieved through the following technical solutions:
[0009] A manganese-nickel-aluminum bronze alloy welding wire comprises, by mass percentage, 7% to 15% of Al, 0.5% to 2.5% of Fe, 0.1% to 0.3% of Si, 2% to 6.5% of Ni, 5% to 15% of Mn, 0.5% to 3.5% of Sn, 0.03% to 0.07% of Mg, and the balance is Cu.
[0010] The method for preparing the manganese-nickel-aluminum-bronze alloy welding wire comprises:
[0011] Step 1: The ingredients are prepared according to the ratio of each element and vacuum melted, and then cast into a bar blank. The bar blank is treated at 400-650°C for component homogenization;
[0012] Step 2: Processing the bar blank obtained in step 1 into a copper alloy bar by hot rolling, turning, and cold rotary forging;
[0013] Step 3: subjecting the copper alloy rod to forward hot extrusion deformation;
[0014] Step 4: subjecting the copper alloy rod obtained in step 3 to solid solution quenching;
[0015] Step 5: The copper alloy rod obtained in step 4 is subjected to continuous diameter-changing cold drawing deformation to obtain welding wire;
[0016] Step 6: Perform aging treatment on the welding wire obtained in step 5 to obtain a manganese-nickel-aluminum bronze alloy welding wire.
[0017] Preferably, the step 1 of batching and vacuum melting according to the ratio of each element specifically comprises: preparing CuAl, CuFe, NiSi, CuMn and CuMg master alloys, batching and vacuum melting the CuAl, CuFe, NiSi, CuMn and CuMg master alloys and metal copper and tin.
[0018] Preferably, the molten metal obtained by vacuum melting in step 1 is added with (0.05-0.3) wt.% Ce and stirred during the static process, and then cast into a rod blank.
[0019] Preferably, in step 2, the hot rolling temperature is 850-950°C.
[0020] Preferably, step 3 specifically comprises: heating the copper alloy rod to 850-1000° C., keeping the temperature for 0.5-1 hour, and then performing forward hot extrusion deformation.
[0021] Preferably, step 4 specifically comprises: heating the copper alloy rod to 900-1000° C., keeping the temperature for 0.5-1 hour, and then solution quenching in water.
[0022] Preferably, in step 5, annealing and grinding and polishing are performed during the continuous variable diameter cold drawing process, and the annealing temperature is 750-900°C.
[0023] Preferably, in step 6, the aging treatment temperature is 400-550°C.
[0024] The invention also provides application of the manganese-nickel-aluminum bronze alloy welding wire in coal machine welding.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention designs a manganese-nickel-aluminum bronze alloy welding wire Cu-Al-Fe-Si-Ni-Mn-Sn-Mg, adds Sn element, and increases the addition amount of Ni and Mn, and the three synergistically enhance the strength and corrosion resistance of the welding wire. The main strengthening mode of the alloy of the present invention is that Cu forms a precipitation strengthening phase with Al, Ni, Sn and Si, so that the alloy welding wire has high strength, strong wear resistance and strong corrosion resistance, and is very suitable for layer welding on cast iron, non-alloy steel and low-alloy steel with high corrosion resistance requirements, and can extend the service life of the hydraulic support in more harsh environments.
[0027] The welding wire preparation method of the present invention has obvious strengthening effect after the strengthening phase formed by Cu, Al, Ni, Sn and Si is refined after unidirectional deformation by extrusion and drawing, and the strength is greatly improved, which is close to the base material, and can effectively improve the temperature rise problem of the weld during the long-term use of the hydraulic support. The alloy weld has good acid and alkali corrosion resistance and can well meet the stable use requirements of the hydraulic support in harsh environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 The welding wire preparation flow chart of the present invention is as follows;
[0030] Figure 2 The CuSn complex strengthening phase is precipitated in the Cu matrix of the present invention;
[0031] Figure 3 The CuNiSi complex strengthening phase is precipitated in the Cu matrix of the present invention;
[0032] Figure 4 It is a solid solution formed by Al dissolving in the Cu matrix according to the present invention. DETAILED DESCRIPTION
[0033] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0034] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0035] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0036] The manganese-nickel-aluminum bronze alloy welding wire described in the present invention is a Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy, and its components include, by mass percentage, 7% to 15% Al, 0.5% to 2.5% Fe, 0.1% to 0.3% Si, 2% to 6.5% Ni, 5% to 15% Mn, 0.5% to 3.5% Sn, 0.03% to 0.07% Mg, and the balance is Cu.
[0037] like Figure 1 As shown, the preparation method of the manganese-nickel-aluminum bronze alloy welding wire comprises:
[0038] (1) Vacuum melting and composition homogenization
[0039] High-purity CuAl, CuFe, NiSi, CuMn, CuMg master alloys are prepared by vacuum melting equipment, and the impurity content of the raw materials is not more than 0.01%. Then the master alloy, high-purity electrolytic copper plate and high-purity metallic tin are mixed according to the mass percentage of Cu-(7-15)wt.%Al-(0.5-2.5)wt.%Fe-(0.1-0.3)wt.%Si-(2-6.5)wt.%Ni-(5-15) wt.% Mn-(0.5~3.5)wt.% Sn-(0.03~0.07)wt.% Mg are prepared by smelting, (0.05-0.3)wt.% Ce is added to the molten liquid during the stagnant state, and then electromagnetic stirring is performed for 30 minutes, and the molten liquid is cast into rods with a diameter of 210-230 mm and a length of 1.5-3 m. The surface of the rods has no obvious defects such as looseness and shrinkage cavities. After the rods are cast, they are kept at 400-650°C for 4-8 hours for component homogenization.
[0040] (2) Sawing, cold forging and hot rolling
[0041] After keeping at 850-950℃ for 0.5-1h, roll to 180-190mm, lathe the bar surface by 1-2mm, then cold forge to 140-160mm, the length after sawing is not less than 200mm, and there is no crack on the surface of the bar;
[0042] (3) Hot extrusion
[0043] The Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy rod is heated to 850-1000°C, kept warm for 0.5-1h, and then conveyed into the extrusion cylinder by a conveyor belt for large-diameter forward hot extrusion deformation, and the diameter is reduced to 15-30mm. There is no defect on the surface of the rod, and the rod head and tail are cut off;
[0044] (4) Online solution quenching
[0045] The Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy rod is heated to 900-1000°C, kept at this temperature for 0.5-1h, and then solution quenched in water;
[0046] (5) Cold drawing
[0047] Use a 3-5 ton hydraulic automatic drawing machine to continuously change the diameter and cold draw deformation, and perform multiple drawing passes, successively changing the diameter by 2mm until the diameter is 1-3mm. Perform two annealing treatments in the middle, the annealing temperature is 750-900℃, the insulation time is 1h, and finally the wire is drawn and coiled into welding wire that meets the specifications of the electrical connector;
[0048] (6) Aging treatment
[0049] The welding wire is aged at 400-550°C for 60-90 minutes under inert atmosphere protection, and the coil is cut into fixed sizes for packaging.
[0050] Example 1
[0051] Step 1: prepare high-purity CuAl, CuFe, NiSi, CuMn, CuMg master alloys by vacuum melting equipment, the impurity content of the raw materials is not more than 0.01%, and then melt the master alloy, high-purity electrolytic copper plate and high-purity metal tin according to the mass percentage of Cu-9wt.%Al-1.2wt.%Fe-0.2wt.%Si-4.5wt.%Ni-10wt.%Mn-1.5wt.%Sn-0.03wt.%Mg, add 0.05wt.%Ce during the molten liquid standing, and then stir it by electromagnetic for 30 minutes, cast it into a rod billet with a diameter of 210mm, and keep it at 500℃ for 4h for component homogenization;
[0052] Step 2: After keeping at 850℃ for 1h, roll to 180mm, lathe the bar surface by 1mm, then cold forge to 140mm, the length after sawing is not less than 200mm, and there is no crack on the surface of the bar;
[0053] Step 3: Heat the Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy rod to 850°C, keep it warm for 1 hour, and then perform a large-diameter forward hot extrusion deformation, and cut off the rod head and tail;
[0054] Step 4: Heat the Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy rod to 900°C, keep it at this temperature for 1 hour, and then solution quench it in water;
[0055] Step 5: Continuously reduce the diameter by cold drawing and deformation, reduce the diameter by 2 mm, undergo solution annealing (750℃ for 1h) and grinding and polishing in the middle, and finally draw into manganese-nickel-aluminum bronze alloy welding wires for coal machine hydraulic support welding of different specifications;
[0056] Step 6: The manganese-nickel-aluminum-bronze alloy welding wire is aged at 400°C for 60 minutes under atmosphere protection, and the coil is cut into fixed-length packages.
[0057] Example 2
[0058] Step 1: prepare high-purity CuAl, CuFe, NiSi, CuMn, CuMg master alloys by vacuum melting equipment, the impurity content of the raw materials is not more than 0.01%, and then melt the master alloy, high-purity electrolytic copper plate and high-purity metal tin according to the mass percentage of Cu-9wt.%Al-1.2wt.%Fe-0.2wt.%Si-4.5wt.%Ni-15wt.%Mn-1.5wt.%Sn-0.03wt.%Mg, add 0.05wt.%Ce during the standing process of the molten liquid, stir it electromagnetically for 30 minutes, cast it into a rod billet with a diameter of 210mm, and keep it at 500℃ for 4h for component homogenization;
[0059] Step 2: After keeping at 850℃ for 1h, roll to 180mm, lathe the bar surface by 1mm, then cold forge to 140mm, the length after sawing is not less than 200mm, and there is no crack on the surface of the bar;
[0060] Step 3: Heat the Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy rod to 850°C, keep it warm for 1 hour, and then perform large-diameter forward hot extrusion deformation, and cut off the rod head and tail;
[0061] Step 4: Heat the Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy bar at 900°C, keep it at this temperature for 1 hour, and then solution quench it in water;
[0062] Step 5: Continuously reduce the diameter by cold drawing and deformation, reduce the diameter by 2 mm, undergo solution annealing (750℃ for 1h) and grinding and polishing in the middle, and finally draw into manganese-nickel-aluminum bronze alloy welding wires for coal machine hydraulic support welding of different specifications;
[0063] Step 6: The manganese-nickel-aluminum-bronze alloy welding wire is aged at 400°C for 60 minutes under atmosphere protection, and the coil is cut into fixed-length packages.
[0064] Example 3
[0065] Step 1: prepare high-purity CuAl, CuFe, NiSi, CuMn, CuMg master alloys by vacuum melting equipment, the impurity content of the raw materials is not more than 0.01%, and then melt the master alloy, high-purity electrolytic copper plate and high-purity metal tin according to the mass percentage of Cu-9wt.%Al-1.2wt.%Fe-0.2wt.%Si-5.5wt.%Ni-10wt.%Mn-1.5wt.%Sn-0.03wt.%Mg, add 0.05wt.%Ce during the molten liquid standing, and then stir it by electromagnetic for 30 minutes, cast it into a rod billet with a diameter of 210-230mm, and keep it at 500°C for 4h for component homogenization;
[0066] Step 2: After keeping at 850℃ for 1h, roll to 180mm, lathe the bar surface by 1mm, then cold forge to 140mm, the length after sawing is not less than 200mm, and there is no crack on the surface of the bar;
[0067] Step 3: Heat the Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy rod to 850°C, keep it warm for 1 hour, and then perform large-diameter forward hot extrusion deformation, and cut off the rod head and tail;
[0068] Step 4: Heat the Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy bar at 900°C, keep it at this temperature for 1 hour, and then solution quench it in water;
[0069] Step 5: Continuously reduce the diameter by cold drawing and deformation, reduce the diameter by 2 mm, undergo solution annealing (750℃ for 1h) and grinding and polishing in the middle, and finally draw into manganese-nickel-aluminum bronze alloy welding wires for coal machine hydraulic support welding of different specifications;
[0070] Step 6: The manganese-nickel-aluminum-bronze alloy welding wire is aged at 400°C for 60 minutes under atmosphere protection, and the coil is cut into fixed-length packages.
[0071] Example 4
[0072] Step 1: prepare high-purity CuAl, CuFe, NiSi, CuMn, CuMg master alloys by vacuum melting equipment, the impurity content of the raw materials is not more than 0.01%, and then melt the master alloy, high-purity electrolytic copper plate and high-purity metal tin according to the mass percentage of Cu-9wt.%Al-1.2wt.%Fe-0.2wt.%Si-5.5wt.%Ni-15wt.%Mn-1.5wt.%Sn-0.03wt.%Mg, add 0.05wt.%Ce during the molten liquid standing, and then stir it by electromagnetic for 30 minutes, cast it into a rod billet with a diameter of 210mm, and keep it at 500℃ for 4h for component homogenization;
[0073] Step 2: After keeping at 850℃ for 1h, roll to 180mm, lathe the bar surface by 1mm, then cold forge to 140mm, the length after sawing is not less than 200mm, and there is no crack on the surface of the bar;
[0074] Step 3: Heat the Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy rod to 850°C, keep it warm for 1 hour, and then perform large-diameter forward hot extrusion deformation, and cut off the rod head and tail;
[0075] Step 4: Heat the Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy bar at 900°C, keep it at this temperature for 1 hour, and then solution quench it in water;
[0076] Step 5: Continuously reduce the diameter by cold drawing and deformation, reduce the diameter by 2 mm, undergo solution annealing (750℃ for 1h) and grinding and polishing in the middle, and finally draw into manganese-nickel-aluminum bronze alloy welding wires for coal machine hydraulic support welding of different specifications;
[0077] Step 6: The manganese-nickel-aluminum-bronze alloy welding wire is aged at 400°C for 60 minutes under atmosphere protection, and the coil is cut into fixed-length packages.
[0078] Example 5
[0079] Step 1: prepare high-purity CuAl, CuFe, NiSi, CuMn, CuMg master alloys by vacuum melting equipment, the impurity content of the raw materials is not more than 0.01%, and then melt the master alloy, high-purity electrolytic copper plate and high-purity metal tin according to the mass percentage of Cu-9wt.%Al-1.2wt.%Fe-0.2wt.%Si-5.5wt.%Ni-15wt.%Mn-1.5wt.%Sn-0.03wt.%Mg, add 0.05wt.%Ce during the molten liquid standing, and then stir it electromagnetically for 30 minutes, cast it into a rod billet with a diameter of 210mm, and keep it at 600℃ for 4h for component homogenization;
[0080] Step 2: After keeping at 850℃ for 1h, roll to 180mm, lathe the bar surface by 1mm, then cold forge to 140mm, the length after sawing is not less than 200mm, and there is no crack on the surface of the bar;
[0081] Step 3: Heat the Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy rod to 850°C, keep it warm for 1 hour, and then perform large-diameter forward hot extrusion deformation, and cut off the rod head and tail;
[0082] Step 4: Heat the Cu-Al-Fe-Si-Ni-Mn-Sn-Mg alloy bar at 900°C, keep it at this temperature for 1 hour, and then solution quench it in water;
[0083] Step 5: Continuously reduce the diameter by cold drawing and deformation, reduce the diameter by 2 mm, undergo solution annealing (750℃ for 1h) and grinding and polishing in the middle, and finally draw into manganese-nickel-aluminum bronze alloy welding wires for coal machine hydraulic support welding of different specifications;
[0084] Step 6: The manganese-nickel-aluminum-bronze alloy welding wire is aged at 400°C for 60 minutes under atmosphere protection, and the coil is cut into fixed-length packages.
[0085] Comparative Example 1
[0086] Basically the same as Example 5, except that the composition is Cu-9wt.%Al-1.2wt.%Fe-0.2wt.%Si-0.3wt.%Ni-0.05wt.%Mn-0.03wt.%Mg.
[0087] Comparative Example 2
[0088] It is basically the same as Example 5, except that the step of homogenizing the components is omitted in step 1.
[0089] The welding wires obtained in Examples 1 to 5 and Comparative Examples 1 to 2 were subjected to performance tests, and the results are shown in Table 1. In the salt spray test, the concentration of the hydrochloric acid and sodium chloride mixed solution used was 20%.
[0090] Table 1 Performance of welding wires obtained in Examples 1 to 5 and Comparative Examples 1 to 2
[0091]
[0092] It can be seen from Table 1 that the weld seam hardness of the welding wire obtained in the embodiment of the present invention is significantly higher than that of the comparative example 1, and the welding wire of the present invention can pass the salt spray test, while the welding wire of the comparative example 1 cannot pass the salt spray test. This is because the present invention increases the content of Ni and Mn and adds Sn, and the three work together to improve the strength and corrosion resistance of the welding wire. Therefore, the welding wire of the present invention can pass the salt spray test with a sodium chloride concentration of up to 20%, while the welding wire of the comparative example 1 cannot pass the salt spray test with a sodium chloride concentration of 20%.
[0093] Compared with Example 1, Example 2 increases the content of Mn. It can be seen from Table 1 that the hardness of Example 2 is higher than that of Example 1, so the strength is also higher than that of Example 1. Similarly, compared with Example 3, Example 4 increases the content of Mn. It can be seen from Table 1 that the hardness of Example 4 is higher than that of Example 3. This shows that the increase in Mn content can increase the hardness of the welding wire, thereby increasing the strength.
[0094] Compared with Example 1, Example 3 increases the Ni content. It can be seen from Table 1 that the hardness of Example 3 is higher than that of Example 1. Similarly, compared with Example 2, Example 4 increases the Ni content. It can be seen from Table 1 that the hardness of Example 4 is higher than that of Example 2. This shows that the increase in Ni content can increase the hardness of the welding wire, thereby improving the strength.
[0095] Compared with Example 4, Example 5 increases the temperature of the composition homogenization treatment. As can be seen from Table 1, the hardness of Example 5 is higher than that of Example 4. This shows that the increase in the temperature of the composition homogenization treatment can increase the hardness of the welding wire.
[0096] Figure 2 , Figure 3 and Figure 4 The metallographic photographs of the welding wire prepared in Example 5 after different corrosion treatments are shown. It can be seen that the alloy welding wire prepared in the present invention contains CuSn complex strengthening phase, CuNiSi complex strengthening phase and solid solution formed by Al solid solution in Cu matrix, and these strengthening phases jointly improve the strength and corrosion resistance of the alloy.
Claims
1. A manganese-nickel-aluminum-bronze alloy welding wire, characterized in that: Calculated by mass percentage, its components include: 7% to 15% Al, 0.5% to 2.5% Fe, 0.1% to 0.3% Si, 2% to 6.5% Ni, 5% to 15% Mn, 0.5% to 3.5% Sn, 0.03% to 0.07% Mg, and the balance is Cu.
2. The method for preparing the manganese-nickel-aluminum bronze alloy welding wire according to claim 1, characterized in that: include: Step 1: The ingredients are prepared according to the ratio of each element and vacuum melted, and then cast into a bar blank. The bar blank is treated at 400-650°C for component homogenization; Step 2: Processing the bar blank obtained in step 1 into a copper alloy bar by hot rolling, turning, and cold rotary forging; Step 3: subjecting the copper alloy rod to forward hot extrusion deformation; Step 4: subjecting the copper alloy rod obtained in step 3 to solid solution quenching; Step 5: The copper alloy rod obtained in step 4 is subjected to continuous diameter-changing cold drawing deformation to obtain welding wire; Step 6: Perform aging treatment on the welding wire obtained in step 5 to obtain a manganese-nickel-aluminum bronze alloy welding wire.
3. The method for preparing the manganese-nickel-aluminum bronze alloy welding wire according to claim 2, characterized in that: The step 1 of batching and vacuum melting according to the ratio of each element is specifically as follows: preparing CuAl, CuFe, NiSi, CuMn and CuMg master alloys, batching and vacuum melting the CuAl, CuFe, NiSi, CuMn and CuMg master alloys and metal copper and tin.
4. The method for preparing the manganese-nickel-aluminum bronze alloy welding wire according to claim 2, characterized in that: In step 1, the molten metal obtained by vacuum melting is added with (0.05-0.3) wt.% Ce during the static process and stirred, and then cast into a rod blank.
5. The method for preparing the manganese-nickel-aluminum bronze alloy welding wire according to claim 2, characterized in that: In step 2, the hot rolling temperature is 850-950°C.
6. The method for preparing the manganese-nickel-aluminum bronze alloy welding wire according to claim 2, characterized in that: Step 3 is specifically as follows: heating the copper alloy rod to 850-1000° C., keeping the temperature for 0.5-1 hour, and then performing forward hot extrusion deformation.
7. The method for preparing the manganese-nickel-aluminum-bronze alloy welding wire according to claim 2, characterized in that: Step 4 is specifically as follows: heating the copper alloy rod to 900-1000° C., keeping the temperature for 0.5-1 hour, and then solution quenching in water.
8. The method for preparing the manganese-nickel-aluminum bronze alloy welding wire according to claim 2, characterized in that: In step 5, annealing and grinding and polishing are performed during the continuous diameter-changing cold drawing process, and the annealing temperature is 750-900°C.
9. The method for preparing the manganese-nickel-aluminum bronze alloy welding wire according to claim 2, characterized in that: In step 6, the aging treatment temperature is 400-550°C.
10. Application of the manganese-nickel-aluminum bronze alloy welding wire according to claim 1 in coal machine welding.