High-frequency LCP glass fabric based hydrocarbon flexible copper-clad plate and preparation method thereof

By introducing an LCP fiberglass cloth layer and a hydrocarbon adhesive layer into the LCP flexible copper-clad laminate, and using a high-temperature lamination process, the problem of poor mechanical properties of the LCP flexible copper-clad laminate is solved, and the excellent electrical properties and performance of high-frequency and high-speed circuit boards are achieved. Stability, suitable for 5G communication systems.

CN118789902APending Publication Date: 2024-10-18ALLSTAE TECH ZHONGSHAN

Patent Information

Application Number
CN202410893557.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing LCP flexible copper-clad laminates have problems such as large differences in mechanical properties, low peel strength, difficulty in subsequent substrate processing, and high defective rates, making it difficult to meet the needs of high-frequency and high-speed circuit boards.

Method used

A hydrocarbon adhesive layer between the LCP fiberglass cloth layer and the copper foil layer is used. The hydrocarbon adhesive is composed of thermoplastic elastomer, TPI resin, LDM resin, LCP filler, ion capture agent and epoxy resin, combined with a high-temperature lamination process. , prepared a high-frequency LCP glass fiber cloth-based hydrocarbon flexible copper-clad laminate with a microporous structure.

Benefits of technology

The dielectric constant and dielectric loss characteristics are improved, the mechanical properties are enhanced, the water absorption rate is reduced, the frequency response capability and temperature stability are improved, and it is suitable for high-frequency and high-speed circuit boards, and the process is simple and convenient for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118789902A_ABST
    Figure CN118789902A_ABST
Patent Text Reader

Abstract

The invention discloses a high-frequency LCP glass fabric based hydrocarbon flexible copper-clad plate, which comprises an LCP glass fabric layer and copper foil layers positioned on the upper and lower surfaces of the LCP glass fabric layer, and hydrocarbon adhesive layers for bonding the LCP glass fabric layer and the copper foil layers on the upper and lower surfaces of the LCP glass fabric layer are arranged between the LCP glass fabric layer and the copper foil layers on the upper and lower surfaces of the LCP glass fabric layer; the LCP glass fiber cloth layer is formed by LCP glass fiber cloth with a micropore structure, and the thickness of the LCP glass fiber cloth layer is 15-25 microns. According to the flexible copper-clad plate, the problem of large mechanical property difference caused by large anisotropy of an LCP film is solved while low water absorption, excellent dielectric constant and excellent dielectric loss characteristics of the LCP are maintained. The invention further provides a preparation method of the high-frequency LCP glass fiber cloth based hydrocarbon flexible copper-clad plate, and the preparation method is simple in technological process, easy to implement and convenient for mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic materials, and in particular relates to a high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate and a preparation method thereof. Background Art

[0002] In recent years, with the in-depth and rapid development of the Internet of Things in many high-tech application fields such as mobile data communications, industrial automation, aerospace, etc., especially the advent of the 5G era, liquid crystal polymer (LCP) as a new generation of microwave millimeter wave substrate materials has good high-frequency characteristics and physical properties, excellent dielectric properties, low thermal expansion coefficient, high strength, good flexibility and low moisture absorption rate. It can replace polytetrafluoroethylene (PTEE) and polyimide (PI) substrate materials and become a key material for 5G devices. It is also an internationally recognized indispensable insulating material for 5G signal antennas. And with the miniaturization, high performance and universalization requirements of T / R components and microwave / millimeter wave modules in aerospace communication systems and phased array radar systems, as well as the sharp increase in the number of components in the RF front end of antennas in the 5G era, the need to embed and integrate components in LCP flexible substrates is becoming increasingly urgent. The integration of passive components in LCP flexible substrates can reduce the restrictions on installation location and quantity, greatly improving the reliability of microwave millimeter wave electronic systems.

[0003] Due to the small dielectric constant, low loss tangent, small thermal expansion coefficient, high strength, strong flame retardancy, wear resistance and flexibility of LCP substrate, it is widely used in high-frequency and high-speed circuit boards. However, the existing LCP flexible copper clad laminates have large differences in mechanical properties, low peel strength, difficulty in subsequent substrate processing and high defective rate. Summary of the invention

[0004] The purpose of the present invention is to provide a high-frequency, high-speed flexible copper-clad laminate-LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate for high-end 5G communication systems in view of the deficiencies in the prior art, which solves the problem of large differences in mechanical properties caused by large anisotropy of the LCP film while maintaining the low water absorption rate, excellent dielectric constant and dielectric loss characteristics of the LCP film. The present invention also provides a method for preparing the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate, which has a simple process, is easy to implement, and is convenient for mass production.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A high-frequency LCP glass fiber cloth-based hydrocarbon flexible copper-clad laminate comprises an LCP glass fiber cloth layer and copper foil layers located on the upper and lower surfaces of the LCP glass fiber cloth layer, wherein hydrocarbon adhesive layers for bonding the LCP glass fiber cloth layer and the copper foil layers on the upper and lower surfaces thereof are provided between the LCP glass fiber cloth layer and the copper foil layers on the upper and lower surfaces thereof; the LCP glass fiber cloth layer is composed of an LCP glass fiber cloth with a microporous structure, and the thickness of the LCP glass fiber cloth layer is 15 to 25 μm.

[0007] In the present invention, the dielectric constant Dk (10 GHz) of the LCP glass fiber cloth is ≤3.0, the dielectric loss Df (10 GHz) is ≤0.001, and the pore diameter of the micropores is 0.5-1.0 mm.

[0008] In the present invention, the hydrocarbon adhesive layer is formed by coating a hydrocarbon adhesive, and the hydrocarbon adhesive is prepared from the following components in parts by weight:

[0009]

[0010] The thickness of the two hydrocarbon adhesive layers is 25-50 μm.

[0011] In the present invention, the copper foil layer is made of high-frequency copper foil, and the surface roughness of the two copper foil layers is 0.6-1.5 μm. Furthermore, the high-frequency copper foil is one of electrolytic copper and rolled copper.

[0012] The present invention also provides a method for preparing the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate, comprising the following steps:

[0013] S1. Add the thermoplastic elastomer, TPI resin, LDM resin, LCP filler, ion capture agent and epoxy resin into a mixer and stir evenly to obtain a hydrocarbon adhesive;

[0014] S2. The hydrocarbon adhesive prepared in S1 is applied to the upper and lower surfaces of the LCP glass fiber cloth and dried to obtain a high-frequency LCP glass fiber cloth impregnated sheet;

[0015] S3. Copper foils of the same size were laid on the outside of the hydrocarbon adhesive in the high-frequency LCP glass fiber cloth impregnated sheet obtained in S2 to obtain a laminate;

[0016] S4. The laminate obtained in S3 is placed in a pressing device for high-temperature pressing to obtain the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate.

[0017] In S1 of the present invention, the stirring temperature is 25 to 40° C. and the stirring time is 4 to 6 hours.

[0018] In S2, the drying temperature is 100-140°C, and the drying time is 2-4 minutes.

[0019] In S4, the high temperature pressing adopts a continuous isostatic pressing method using a high temperature resistant steel belt; the temperature of the high temperature pressing is 260-300°C, the pressure is 2-8Mpa, the line speed of the high temperature pressing is 0.8-2.5m / min, and the pressing time is 4-7min.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate of the present invention has a small dielectric constant and a low loss tangent, and the loss tangent hardly changes with increasing frequency, and has better signal transmission performance and higher frequency response.

[0022] (2) The thermal expansion coefficient of the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate of the present invention is very small, and its stability is better under temperature changes. It can be widely used as an ideal packaging thermal conductive material for high-frequency thermal conductive soft boards.

[0023] (3) The high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate of the present invention has excellent properties such as high strength, high modulus, enhanced self-gravity, strong flame retardancy, strong heat resistance, corrosion resistance, and wear resistance, and also has outstanding technical performance in microwave hot and cold alternating performance testing.

[0024] (4) High-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper clad laminate is flexible and can save more space, making it more expressive in future wearable and miniaturized electronic devices.

[0025] (5) The process of the present invention is simple, easy to implement, and convenient for mass production.

[0026] (6) The continuous isostatic high-temperature steel belt pressing method used in the present invention presses the laminated body at high temperature, has a large pressing contact area, and can set heating and cooling intervals, which can effectively reduce the internal stress of the material during the high-temperature pressing process; BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic structural diagram of the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate of the present invention. DETAILED DESCRIPTION

[0028] The present invention will be further described below with reference to specific embodiments, but is not limited thereto.

[0029] Example

[0030] like Figure 1As shown, a high-frequency LCP glass fiber cloth-based hydrocarbon flexible copper-clad laminate according to an embodiment of the present invention comprises an LCP glass fiber cloth layer 1 and copper foil layers 3 located on the upper and lower surfaces of the LCP glass fiber cloth layer, and a hydrocarbon adhesive layer 2 for bonding the LCP glass fiber cloth layer 1 and the copper foil layers 3 on the upper and lower surfaces thereof is provided between the LCP glass fiber cloth layer 1 and the copper foil layers 3 on the upper and lower surfaces thereof; the LCP glass fiber cloth layer 1 is composed of an LCP glass fiber cloth having a microporous structure, and the thickness of the glass fiber cloth layer 1 is 15 to 25 μm. The pore size of the micropores of the LCP glass fiber cloth is 0.5 to 1.0 mm.

[0031] The hydrocarbon adhesive layer of this embodiment is formed by coating a hydrocarbon adhesive, wherein the hydrocarbon adhesive is prepared from the following components in parts by weight:

[0032]

[0033] The thickness of the two hydrocarbon adhesive layers is 25-50 μm.

[0034] In the embodiments and comparative examples of the present invention, the thermoplastic elastomer is selected from Kraton FG1901, the TPI resin is selected from Silver Jubilee SP1T03H, the LDM resin is selected from Denka's LDM-02-C, the LCP filler is selected from Mitsubishi Chemical LF-31P, and the epoxy resin is selected from Mitsubishi Chemical JER630; the copper foil is selected from JXEFL-BHM, with a thickness of 1 / 3oz, a type of electrolytic copper, and a basis weight of 100g / cm 2 , the surface roughness (Rz value) is 1.2μm; the LCP film is selected from Kuraray; the pressing equipment is a German double steel belt pressing equipment, model E166-42 "Alice".

[0035] The preparation method of the above-mentioned high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate comprises the following steps:

[0036] S1. Add the thermoplastic elastomer, TPI resin, LDM resin, LCP filler, ion scavenger and epoxy resin into a mixer according to the ratio, and stir at a temperature of 25 to 40° C. for 4 to 6 hours to obtain a hydrocarbon adhesive;

[0037] S2. The adhesive prepared in S1 is applied to the upper and lower surfaces of the high-frequency LCP glass fiber cloth, and dried at a temperature of 100 to 140°C for 2 to 4 minutes to obtain a high-frequency LCP glass fiber cloth impregnated sheet;

[0038] S3. Copper foils of the same size were laid on the outside of the hydrocarbon adhesive layer in the high-frequency LCP glass fiber cloth impregnated sheet obtained in S2 to obtain a laminate;

[0039] S4. Place the laminate obtained in S3 into a laminating device for high-temperature laminating for 4 to 7 minutes to obtain the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate. The high-temperature laminating adopts a continuous isostatic high-temperature steel belt laminating method; the high-temperature laminating temperature is 260 to 300°C, the pressure is 2 to 8 MPa, the high-temperature laminating line speed is 0.8 to 2.5 m / min, and the laminating time is 4 to 7 minutes.

[0040] Example 1

[0041] like Figure 1 As shown, in this embodiment, a high-frequency LCP glass fiber cloth-based hydrocarbon flexible copper-clad laminate comprises an LCP glass fiber cloth layer 1 and copper foil layers 3 located on the upper and lower surfaces of the LCP glass fiber cloth layer, and a hydrocarbon adhesive layer 2 for bonding the LCP glass fiber cloth layer 1 and the copper foil layers 3 on the upper and lower surfaces thereof is provided between the LCP glass fiber cloth layer 1 and the copper foil layers 3 on the upper and lower surfaces thereof; the LCP glass fiber cloth layer 1 is composed of an LCP glass fiber cloth having a microporous structure, and the thickness of the glass fiber cloth layer 1 is 15 μm. The pore size of the micropores of the LCP glass fiber cloth is 0.8 mm.

[0042] The hydrocarbon adhesive layer of this embodiment is formed by coating a hydrocarbon adhesive, and the hydrocarbon adhesive is prepared by 100 parts by weight of a thermoplastic elastomer, 9 parts by weight of a TPI resin, 7.5 parts by weight of a LDM resin, 40 parts by weight of a LCP filler, 2 parts by weight of an ion capture agent, and 4 parts by weight of an epoxy resin.

[0043] The thickness of the upper and lower hydrocarbon adhesive layers is 25 μm;

[0044] The surface roughness of the upper and lower copper foil layers is 0.6-1.5 μm, and the thickness is 12 μm.

[0045] The preparation method of the above-mentioned high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate comprises the following steps:

[0046] S1. Add the thermoplastic elastomer, TPI resin, LDM resin, LCP filler, ion scavenger and epoxy resin into a mixer according to the ratio, and stir at a temperature of 25 to 40° C. for 4 to 6 hours to obtain a hydrocarbon adhesive;

[0047] S2. The adhesive prepared in S1 is applied to the upper and lower surfaces of the high-frequency LCP glass fiber cloth, and dried at a temperature of 100 to 140°C for 2 to 4 minutes to obtain a high-frequency LCP glass fiber cloth impregnated sheet;

[0048] S3. Copper foils of the same size were laid on the outside of the hydrocarbon adhesive layer in the high-frequency LCP glass fiber cloth impregnated sheet obtained in S2 to obtain a laminate;

[0049] S4. Put the laminated body obtained in S3 into a laminating device for high-temperature laminating for 4 to 7 minutes to obtain the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate, wherein the laminating temperature is 280°C, the pressure is 3Mpa, the unwinding tension is 10N, the winding tension is 30N, and the laminating line speed is 1.6m / min.

[0050] Example 2

[0051] The difference between Example 2 and Example 1 is that the thickness of the LCP glass fiber cloth is 25 μm, and the thickness of the upper and lower hydrocarbon adhesive layers are both 35 μm.

[0052] The hydrocarbon adhesive layer of this embodiment is formed by coating with a hydrocarbon adhesive, and the hydrocarbon adhesive is prepared by weight of 120 parts of thermoplastic elastomer, 6 parts of TPI resin, 10 parts of LDM resin, 30 parts of LCP filler, 2 parts of ion capture agent, and 6 parts of epoxy resin.

[0053] The remaining compositions and preparation methods are the same as those in Example 1.

[0054] Example 3

[0055] The difference between Example 3 and Example 1 is that the thickness of the LCP glass fiber cloth is 20 μm, and the thickness of the upper and lower hydrocarbon adhesive layers are both 50 μm.

[0056] The hydrocarbon adhesive layer of this embodiment is formed by coating with a hydrocarbon adhesive, and the hydrocarbon adhesive is prepared by 80 parts by weight of a thermoplastic elastomer, 9 parts by weight of a TPI resin, 5 parts by weight of a LDM resin, 40 parts by weight of a LCP filler, 3 parts by weight of an ion capture agent, and 2 parts by weight of an epoxy resin.

[0057] The remaining compositions and preparation methods are the same as those in Example 1.

[0058] Comparative Example

[0059] Comparative Example 1

[0060] The difference between Comparative Example 1 and Example 1 is that the thickness of the LCP glass fiber cloth layer is 30 μm; and the thickness of the upper and lower hydrocarbon adhesive layers are both 25 μm.

[0061] The remaining compositions and preparation methods are the same as those in Example 1.

[0062] Comparative Example 2

[0063] The difference between Comparative Example 2 and Example 1 is that the thickness of the LCP glass fiber cloth layer is 10 μm; the thickness of the upper and lower hydrocarbon adhesive layers are both 25 μm.

[0064] The remaining compositions and preparation methods are the same as those in Example 1.

[0065] Comparative Example 3

[0066] The difference between Comparative Example 3 and Comparative Example 1 is that in the comparative example, the hydrocarbon adhesive layer and the LCP glass fiber cloth layer are replaced by an LCP film layer (the specific component is a liquid crystal polymer film, and the LCP film layer is from Japan's Kuraray LCP film), the thickness of the LCP film layer is 30 μm, and the other structures and preparation methods are the same as those in Comparative Example 1.

[0067] Performance Testing

[0068] The performance tests were performed on the flexible copper clad laminates prepared in Example 1-2 and Comparative Example 1-2.

[0069] Test method:

[0070] The performance tests such as peel strength, dielectric constant (Dk), dielectric loss (Df), tensile strength, elongation, water absorption and dimensional stability are carried out according to the test methods specified in IPC-TM-650, JIS C6471 and SPDR.

[0071] The test results are shown in Table 1.

[0072] Table 1 Performance results of flexible copper clad laminate

[0073]

[0074]

[0075] It can be seen from Table 1 that the dielectric constant (Dk value) of the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminates prepared in Examples 1-3 of the present invention is small, being only about 2.3 at 10 GHz; the loss tangent (Df value) is also very low, being about 0.001 at 10 GHz and only about 0.0035 at 110 GHz, and there is almost no change with the increase of frequency, and the laminates have better signal transmission performance and higher frequency response.

[0076] The peel strength, dielectric constant, dielectric loss, water absorption and dimensional stability of the flexible copper-clad laminates prepared in Examples 1-3 and Comparative Examples 1-2 are significantly better than those of the flexible copper-clad laminate prepared in Comparative Example 3 using LCP film materials. However, as the thickness of the LCP glass fiber cloth increases, the bending performance of Comparative Example 1 decreases, and when the thickness of the LCP glass fiber cloth is 25 μm or less, the bending performance is significantly better than that of Comparative Example 1; as the thickness of the LCP glass fiber cloth decreases, the tensile strength of Comparative Example 2 decreases, and when the thickness of the LCP glass fiber cloth is 15 μm or more, the tensile strength is significantly better than that of Comparative Example 2.

[0077] It can be seen that the high-frequency LCP glass fiber cloth-based hydrocarbon flexible copper-clad laminate prepared in the embodiment of the present invention effectively solves the influence between the mechanical properties, dimensional stability and dielectric loss of the LCP film flexible copper-clad laminate. The prepared flexible copper-clad laminate has good mechanical properties and dimensional stability, low water absorption, and low dielectric loss. At the same time, it also ensures higher electrical properties and has good application prospects.

Claims

1. A high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate, characterized in that The invention comprises an LCP glass fiber cloth layer (1) and copper foil layers (3) located on the upper and lower surfaces of the LCP glass fiber cloth layer, wherein hydrocarbon adhesive layers (2) for bonding the LCP glass fiber cloth layer (1) and the copper foil layers (3) on the upper and lower surfaces are provided between the LCP glass fiber cloth layer (1) and the copper foil layers (3) on the upper and lower surfaces thereof; the LCP glass fiber cloth layer (1) is composed of an LCP glass fiber cloth having a microporous structure, and the thickness of the LCP glass fiber cloth layer (1) is 15 to 25 μm.

2. The high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate according to claim 1 is characterized in that The dielectric constant Dk (10 GHz) of the LCP glass fiber cloth is ≤3.0, the dielectric loss Df (10 GHz) is ≤0.001, and the pore diameter of the micropores is 0.5-1.0 mm.

3. The high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate according to claim 1 is characterized in that The hydrocarbon adhesive layer is formed by coating a hydrocarbon adhesive, and the hydrocarbon adhesive is prepared from the following components in parts by weight:

4. The high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate according to claim 3 is characterized in that The thickness of the two hydrocarbon adhesive layers is 25-50 μm.

5. The high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate according to claim 1 is characterized in that The material of the copper foil layer is high-frequency copper foil, and the surface roughness of the two copper foil layers is 0.6-1.5 μm.

6. The high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate according to claim 5, characterized in that The high-frequency copper foil is one of electrolytic copper and rolled copper.

7. A method for preparing a high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate according to any one of claims 1 to 6, characterized in that The following steps are involved: S1. Add the thermoplastic elastomer, TPI resin, LDM resin, LCP filler, ion catcher and epoxy resin into a mixer and stir evenly to obtain a hydrocarbon adhesive; S2. The hydrocarbon adhesive prepared in S1 is applied to the upper and lower surfaces of the LCP glass fiber cloth and dried to obtain a high-frequency LCP glass fiber cloth impregnated sheet; S3. Copper foils of the same size were laid on the outside of the hydrocarbon adhesive in the high-frequency LCP glass fiber cloth impregnated sheet obtained in S2 to obtain a laminate; S4. The laminate obtained in S3 is placed in a pressing device for high-temperature pressing to obtain the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate.

8. The method for preparing the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate according to claim 7, characterized in that In S1, the stirring temperature is 25-40° C., and the stirring time is 4-6 hours.

9. The method for preparing the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate according to claim 7, characterized in that In S2, the drying temperature is 100-140° C., and the drying time is 2-4 minutes.

10. The method for preparing the high-frequency LCP glass fiber cloth-based carbon-hydrogen flexible copper-clad laminate according to claim 7, characterized in that In S4, the temperature of high temperature pressing is 260-300° C., the pressure is 2-8 MPa, the line speed of high temperature pressing is 0.8-2.5 m / min, and the pressing time is 4-7 min.

Citation Information

Patent Citations

  • Single-component epoxy resin flowing type underfill adhesive and preparation method thereof

    CN111560232A

  • Liquid crystal polymer resin composition and copper-clad plate prepared from same

    CN114479419A

  • Polytetrafluoroethylene flexible copper-clad plate containing glass fabric and preparation method thereof

    CN114670512A

  • High-frequency double-sided flexible copper-clad plate and preparation method thereof

    CN115972708A

  • Heat-resistant flexible copper-clad plate and preparation method thereof

    CN117087208A

Cited By

  • High-frequency copper-clad plate manufacturing method and high-frequency copper-clad plate

    CN119521557A

  • High-frequency copper clad laminate manufacturing method and high-frequency copper clad laminate

    CN119521557B