Method for producing high-strength asphalt mixture by compounding steel slag
Through multi-step modification of steel slag and asphalt, the volume instability of steel slag aggregate and insufficient performance of asphalt mixture are solved, and the stability of asphalt mixture and road service life are improved.
Patent Information
- Application Number
- CN202410875054.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-18
AI Technical Summary
The free calcium oxide and magnesium oxide inside the steel slag aggregate cause volume expansion and cracking, affecting its stability and adhesion properties in asphalt mixtures, and existing asphalt mixtures have insufficient low-temperature brittleness and high-temperature deformation properties.
By controlling the morphology of steel slag, including crushing, magnetic field impurity removal and hydrothermal reaction, the modified asphalt is treated with low-pressure carbon dioxide and added with waste bio-oil and loaded polyurea fiber under negative pressure, combined with Arthrobacter fermentation bacteria liquid. Improve the bonding performance and flexibility of asphalt, and mix it with steel slag, mineral powder, limestone fine aggregate and other materials.
It improves the stability, water damage resistance, compressive strength and self-repair ability of the asphalt mixture, extends the service life of the road, and improves the drainage and skid resistance of the steel slag aggregate.
Smart Images

Figure CN118791252A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of asphalt mixtures, and in particular to a method for producing high-strength asphalt mixtures by compounding steel slag. Background Art
[0002] Asphalt mixture is a composite material used in road construction, mainly composed of asphalt, coarse aggregate, fine aggregate, mineral powder, and sometimes polymers and wood cellulose. Asphalt mixture is a mixture of these materials of different quality and quantity to form different structures and have different mechanical properties.
[0003] Aggregate is one of the main building materials used in road construction and maintenance. About 40,000 to 60,000 tons of gravel and other aggregates are consumed per kilometer of road, and the consumption of natural aggregates is large. This has not only led to the gradual reduction of natural aggregate resources, but also seriously damaged the natural ecological environment. In order to improve this situation, researchers have actively explored the utilization of industrial solid waste, such as using steel slag, mining waste and construction waste as aggregates for road construction and maintenance. Among them, steel slag has the advantages of high strength, wear resistance, anti-skid, high alkalinity and low cost, and has the potential to replace natural aggregates in road construction and maintenance.
[0004] However, there are free calcium oxide and magnesium oxide inside the steel slag aggregate, which is prone to volume expansion and cracking when absorbing water, resulting in poor volume stability; and the adhesion performance of steel slag aggregate and asphalt will directly affect the degree of water damage. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a method for producing high-strength asphalt mixture by compounding steel slag.
[0006] A method for producing high-strength asphalt mixture by compounding steel slag, characterized by comprising the following steps:
[0007] S1. Slag treatment:
[0008] The steel slag is crushed and then the morphology of the steel slag is controlled;
[0009] S2. Asphalt modification:
[0010] S2-1, firstly, the base asphalt is placed in a carbon dioxide gas atmosphere with a volume concentration of 98.9-99.9% and a pressure of 0.2-0.3 MPa for 10-20 minutes;
[0011] S2-2, the carbon dioxide gas pressure is adjusted to a negative pressure of -0.15 to -0.05 MPa, and waste bio-oil accounting for 7.5 to 9.5% of the mass of the base asphalt is added and stirred for 15 to 20 minutes at a stirring temperature of 155 to 160° C. and a stirring rate of 1550 to 1650 rpm;
[0012] S2-3, while maintaining the negative pressure state, adjust the volume concentration of carbon dioxide gas to 92.5-93.5%, add 16-20% of the mass of supported polyurea fiber to the matrix asphalt and stir for 30-40 minutes at a stirring temperature of 175-185°C and a stirring rate of 3500-4500 rpm;
[0013] After the mixing is completed, modified asphalt is obtained;
[0014] S3, Mixed:
[0015] Mix modified asphalt, steel slag, mineral powder filler, limestone fine aggregate, stabilizer and warm mix agent in a mass ratio of 1:6-7:0.8-2.5:3-6:0.1-0.15:0.3-0.4, and mix at 170-180°C for 120-150s.
[0016] Further, in step S1, the morphology control process is:
[0017] S1-1, firstly grind the steel slag to obtain powder A with a particle size of 15 to 20 mm, and then remove impurities from the powder A using a magnetic field of 620 to 650 Gs;
[0018] S1-2, further performing intermediate fine grinding on the powder A after impurities are removed in step S1-1 to obtain powder B with a particle size of 5 to 10 mm, and then removing impurities from the powder B using a magnetic field of 750 to 800 Gs;
[0019] S1-3, the powder B after impurities are removed in step S1-2 is subjected to advanced fine grinding to obtain powder C with a particle size of 1 to 2 mm, and then the powder C is subjected to impurities removal using a magnetic field of 900 to 950 Gs to obtain steel slag with a controlled morphology.
[0020] Description: First, coarse grinding is mainly to break the large particles of steel slag into smaller particles. This step can remove large pieces of hard matter in the steel slag, such as metallic iron; the first fine grinding will further refine the steel slag particles. This step can increase the specific surface area of the steel slag and increase its contact area with asphalt, thereby improving the bonding effect between the steel slag and asphalt, and the shape of the steel slag particles will be more regular and the size will be more consistent; the second fine grinding process is to further increase the specific surface area of the steel slag and enhance its bonding effect with asphalt, thereby improving the performance of the asphalt mixture; the impurity content of the steel slag after magnetic separation is greatly reduced, which can ensure the purity and quality of the asphalt mixture. High-purity steel slag can better blend with asphalt, thereby improving the stability and durability of the asphalt mixture.
[0021] Furthermore, it also includes step S1-4,
[0022] S1-4: Mix the powder C obtained in S1-3, tetraethyl orthosilicate, and deionized water according to a mass ratio of 1:8-10:150-180, place them in a hydrothermal reaction vessel for hydrothermal reaction at a temperature of 150-180°C for 12-14 h; then separate, wash, and dry the product in sequence to obtain steel slag with further morphology control.
[0023] Note: Through hydrothermal synthesis, the steel slag is transformed into a nanomaterial with a specific morphology, thereby increasing the specific surface area and activity of the steel slag, enhancing its adhesion to materials such as asphalt, and improving the application value of the steel slag.
[0024] Further, in step S2, the waste bio-oil is one of swill oil, palm acidified oil, and kitchen waste oil.
[0025] Note: The components in swill oil, palm acidified oil, and kitchen waste oil can increase the softness of asphalt, making it maintain fluidity within a wider temperature range, which helps reduce the brittleness of asphalt at low temperatures and improve its deformation performance at high temperatures; some components in the waste bio-oil can improve the adhesion between asphalt and mineral powder fillers, etc., thereby improving the performance of asphalt mixtures and extending the service life of the road surface.
[0026] Further, in step S2-3, the preparation method of the supported polyurea fiber is as follows:
[0027] S2-3-1: Completely dry the polyurea fiber and grind it into powder for standby.
[0028] S2-3-2: Centrifuge the Arthrobacter fermentation broth with a mass concentration of 0.6-0.8% at a speed of 5100-5200 r / min for 25-30 min at room temperature to obtain a precipitate, mix the precipitate with trehalose at a mass ratio of 1:1, and then vacuum freeze-dry under sterile conditions to obtain solid-state fermented Arthrobacter and crush and sieve it.
[0029] S2-3-3: Then immerse the solid-state fermented Arthrobacter in a sodium hydroxide solution with a mass concentration of 9-10% for 2.5-4.5 h, and simultaneously apply sunlight illumination during the immersion, with an illumination intensity of 30-40 mW. After the immersion, obtain the activated solid-state fermented Arthrobacter.
[0030] S2-3-4: Mix the solid-state fermented Arthrobacter obtained in S2-3-3 and the polyurea fiber at a mass ratio of 1:10-20, add them to sterile ultrapure deionized water with a solid-liquid ratio of 1 g:22-24 mL, then oscillate at a rotation speed of 250-450 rpm at room temperature for 12-13 h, and then dry to constant weight to obtain the polyurea fiber loaded with Arthrobacter.
[0031] Description: After being immersed in alkali solution, the acidic components on the cell wall of Arthrobacter can be removed, and the permeability of the cell can be increased, so that Arthrobacter can be more easily exposed to harmful substances in asphalt. The irradiation of sunlight can make Arthrobacter more easily adsorbed on polyurea fiber, thereby improving the loading efficiency of Arthrobacter and enabling it to better play the role of modified asphalt; Arthrobacter can produce more biocompatible substances under the action of alkali solution and sunlight, which can be mixed with asphalt to enhance the bonding properties of asphalt, improve the environmental performance of asphalt, and enhance the pavement performance of asphalt; and polyurea fiber itself has good elasticity and self-healing properties, combined with the biodegradation characteristics of Arthrobacter, it can further enhance the self-repairing ability of asphalt pavement and extend the service life of the road.
[0032] Furthermore, in step S2-3-1, the particle size of the polyurea fiber is 90-100 μm; in step S2-3-2, the particle size of the solid-state fermentation Arthrobacter is 70-80 μm.
[0033] Description: Smaller particle size polyurea fibers can achieve better dispersion in asphalt, which helps to improve the mechanical properties and durability of asphalt mixtures. The appropriate particle size can ensure that the polyurea fibers are better integrated with asphalt, thereby improving the modification effect. Secondly, the particle size of Arthrobacter will affect its distribution and activity in asphalt. Larger particle size may lead to uneven distribution of Arthrobacter in asphalt. The appropriate particle size can increase the contact area between Arthrobacter and asphalt, thereby improving its biodegradation activity.
[0034] Furthermore, the stabilizer comprises, by mass, 10 to 20 parts of sulfur, 3 to 4 parts of dicumyl peroxide and 1 to 3 parts of glycerol.
[0035] Description: Sulfur-modified asphalt mixture has good high-temperature stability and low-temperature crack resistance, which can reduce the amount of asphalt used and reduce costs; dicumyl peroxide can be used as an initiator to improve the polymerization and bonding properties of modified asphalt and materials such as steel slag; glycerol can be used as a plasticizer to improve the properties of asphalt.
[0036] Furthermore, the mineral powder filler is limestone mineral powder that has passed a 200-mesh sieve, and the particle size of the limestone fine aggregate is 0.05 to 0.07 mm.
[0037] Description: Fillers with smaller particle size can provide better compressive strength and compressive strength, can be more tightly packed in the asphalt matrix, enhance the overall strength of the mixture, and reduce the intrusion of moisture and other harmful substances, thereby extending the service life of the mixture.
[0038] Furthermore, the warm mix agent is Sasobit warm mix agent.
[0039] Description: Sasobit warm mix agent can improve the high temperature performance of asphalt, reduce temperature sensitivity, significantly increase the softening point, and reduce needle penetration. Adding Sasobit warm mix agent can improve the road surface's resistance to deformation and rutting, keep the asphalt mixture's low temperature performance unchanged, and improve the road's resistance to water damage and UV rays.
[0040] Compared with the existing asphalt mixture, the beneficial effects of the present invention are:
[0041] (1) The present invention performs morphology control on steel slag, first coarse grinding and then fine grinding, to increase the specific surface area of steel slag and increase its contact area with asphalt, thereby improving the bonding effect between steel slag and asphalt. After each grinding, the steel slag is subjected to magnetic field impurity removal, and the impurity content is greatly reduced. In this way, the purity and quality of the asphalt mixture can be ensured. High-purity steel slag can be better integrated with asphalt, thereby improving the stability and durability of the asphalt mixture.
[0042] (2) The present invention first places the base asphalt in a low-pressure carbon dioxide atmosphere to change the chemical structure and properties of the asphalt, thereby improving its adhesion to aggregates and making the asphalt softer, which makes it less likely to become brittle in a low-temperature environment, thereby improving its flexibility and ductility; then placing it under negative pressure and adding waste bio-oil to it, so that the asphalt absorbs more carbon dioxide, further changing its chemical structure and improving its biodegradability and durability; finally, the concentration of carbon dioxide is reduced and loaded polyurea fibers are added. Since polyurea fibers themselves have good elasticity and self-healing properties, combined with the biodegradation characteristics of Bacillus, the self-repairing ability of the asphalt pavement can be further improved and the service life of the road can be extended.
[0043] (3) The present invention mixes the morphology-controlled steel slag and the bio-modified asphalt to increase the penetration of the asphalt into the pores of the steel slag, thereby improving the bonding performance of the two and improving the water damage resistance of the asphalt mixture. The treated steel slag aggregate has better adhesion with asphalt, which can improve the volume stability of the asphalt mixture to a certain extent. In addition, the morphology control treatment can also improve the drainage and anti-skid properties of the steel slag aggregate, further improving the overall strength of the asphalt mixture. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 is a comparison chart of the splitting compressive strength ratio results of the study 1 in the experimental example of the present invention;
[0045] Figure 2 is a comparison chart of the compressive strength results of Study 1 in the experimental example of the present invention;
[0046] Figure 3 is a comparison chart of the splitting compressive strength ratio results of the investigation 2 in the experimental example of the present invention;
[0047] Figure 4 is a comparison chart of the compressive strength results of Study 2 in the experimental example of the present invention;
[0048] Figure 5 is a comparison chart of the splitting compressive strength ratio results of Study 3 in the experimental example of the present invention;
[0049] Figure 6 It is a comparison chart of the compressive strength results of Investigation 3 in the experimental example of the present invention. DETAILED DESCRIPTION
[0050] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.
[0051] Embodiment 1: A method for producing high-strength asphalt mixture by compounding steel slag, comprising the following steps:
[0052] S1. Slag treatment:
[0053] The steel slag is crushed and then the morphology of the steel slag is controlled;
[0054] The morphology control process is as follows:
[0055] S1-1, firstly grind the steel slag to obtain powder A with a particle size of 16-18 mm, and then remove impurities from the powder A using a magnetic field of 635 Gs;
[0056] S1-2, further performing intermediate fine grinding on the powder A after impurity removal in step S1-1 to obtain powder B with a particle size of 6 to 8 mm, and then removing impurities from the powder B using a magnetic field of 775 Gs;
[0057] S1-3, further performing advanced fine grinding on the powder B after impurities removal in step S1-2 to obtain powder C with a particle size of 1.2 to 1.6 mm, and then removing impurities from the powder C using a magnetic field of 925 Gs to obtain steel slag with morphology control;
[0058] S2. Asphalt modification:
[0059] S2-1, firstly, the base asphalt is placed in a carbon dioxide gas atmosphere with a volume concentration of 99.2% and a pressure of 0.25 MPa for 15 minutes;
[0060] S2-2, adjusting the carbon dioxide gas pressure to a negative pressure of -0.10 MPa, and adding 8.0% of waste bio-oil by mass to the matrix asphalt and stirring for 18 minutes at a stirring temperature of 158° C. and a stirring rate of 1600 rpm; the waste bio-oil is swill oil;
[0061] S2-3, while maintaining the negative pressure, adjust the volume concentration of carbon dioxide gas to 93.0%, add 16-20% of the mass of supported polyurea fiber to the matrix asphalt and stir for 35 minutes at a stirring temperature of 180°C and a stirring rate of 4000 rpm;
[0062] The preparation method of the loaded polyurea fiber is:
[0063] S2-3-1, completely drying the polyurea fiber and grinding it into powder for later use, wherein the particle size of the polyurea fiber is 92 to 96 μm;
[0064] S2-3-2, centrifuging the fermented Arthrobacter broth with a mass concentration of 0.6-0.8% at 5150 r / min for 28 min at room temperature to obtain a precipitate, mixing the precipitate with trehalose at a mass ratio of 1:1, and then vacuum freeze-drying under sterile conditions to obtain solid-state fermented Arthrobacter, which is crushed and sieved, and the particle size of the solid-state fermented Arthrobacter is 72-76 μm;
[0065] S2-3-3, soaking the solid-state fermentation Arthrobacter in a sodium hydroxide solution with a mass concentration of 9.5% for 3.5 hours, and applying sunlight illumination during the soaking period, with a light intensity of 35mW, and obtaining the activated solid-state fermentation Arthrobacter after the soaking;
[0066] S2-3-4, the solid-state fermented Arthrobacter and polyurea fiber obtained in S2-3-3 were mixed in a mass ratio of 1:15 and added to sterile ultrapure deionized water, with a solid-liquid ratio of 1 g:23 mL, and then oscillated at 300 rpm for 12.5 h at room temperature, and then dried to constant weight to obtain polyurea fiber loaded with Arthrobacter;
[0067] After the mixing is completed, modified asphalt is obtained;
[0068] S3, Mixed:
[0069] Modified asphalt, steel slag, mineral powder filler, limestone fine aggregate, stabilizer, and Sasobit warm mix agent were mixed in a mass ratio of 1:6.5:1.6:4.5:0.12:0.35 at 175°C for 135s;
[0070] The stabilizer comprises, by mass, 10 to 20 parts of sulfur, 3 to 4 parts of dicumyl peroxide and 1 to 3 parts of glycerol; the mineral powder filler is limestone mineral powder passing through a 200-mesh sieve, and the particle size of the limestone fine aggregate is 0.055 to 0.065 mm.
[0071] Embodiment 2: This embodiment differs from Embodiment 1 in that, in step S1, the morphology control process is:
[0072] S1-1, firstly grind the steel slag to obtain powder A with a particle size of 15-16 mm, and then remove impurities from the powder A using a 650 Gs magnetic field;
[0073] S1-2, further performing intermediate fine grinding on the powder A after impurities removal in step S1-1 to obtain powder B with a particle size of 5 to 6 mm, and then removing impurities from the powder B using a magnetic field of 800 Gs;
[0074] S1-3. The powder B after impurities are removed in step S1-2 is subjected to advanced fine grinding to obtain a powder C with a particle size of 1 to 1.2 mm. The powder C is then subjected to impurities removal using a 950 Gs magnetic field to obtain steel slag with a controlled morphology.
[0075] Embodiment 3: This embodiment differs from Embodiment 1 in that, in step S1, the morphology control process is:
[0076] S1-1, firstly grind the steel slag to obtain powder A with a particle size of 18 to 20 mm, and then remove impurities from the powder A using a 620 Gs magnetic field;
[0077] S1-2, further performing intermediate fine grinding on the powder after impurity removal in step S1-1 to obtain powder B with a particle size of 8 to 10 mm, and then removing impurities from powder B using a magnetic field of 750 Gs;
[0078] S1-3. The powder B after impurities are removed in step S1-2 is subjected to advanced fine grinding to obtain a powder C with a particle size of 1.6 to 2 mm. The powder C is then subjected to impurities removal using a 900 Gs magnetic field to obtain steel slag with a controlled morphology.
[0079] Example 4: The difference between this example and Example 1 is that, S2-1, the base asphalt is first placed in a carbon dioxide gas atmosphere with a volume concentration of 98.9% and a pressure of 0.2 MPa for 10 minutes.
[0080] Example 5: The difference between this example and Example 1 is that, S2-1, the base asphalt is first placed in a carbon dioxide gas atmosphere with a volume concentration of 99.9% and a pressure of 0.3 MPa for 20 minutes.
[0081] Example 6: The difference between this example and Example 1 is that, S2-2, the carbon dioxide gas pressure is adjusted to a negative pressure of -0.05MPa, and 7.5% of palmitic acid oil by mass is added to the base asphalt and stirred for 15 minutes. The stirring temperature is 155°C and the stirring rate is 1550rpm.
[0082] Example 7: The difference between this example and Example 1 is that, S2-2, the carbon dioxide gas pressure is adjusted to a negative pressure of -0.15 MPa, and 9.5% of the mass of waste cooking oil is added to the base asphalt and stirred for 20 minutes. The stirring temperature is 160°C and the stirring rate is 1650rpm.
[0083] Example 8: The difference between this example and Example 1 is that, S2-3, the negative pressure state is maintained again, the volume concentration of carbon dioxide gas is adjusted to 92.5%, and 16% of the mass of loaded polyurea fiber is added to the base asphalt and stirred for 30 minutes. The stirring temperature is 175°C and the stirring rate is 3500rpm.
[0084] Example 9: The difference between this example and Example 1 is that, S2-3, the negative pressure state is maintained again, the volume concentration of carbon dioxide gas is adjusted to 93.5%, and 20% of the mass of loaded polyurea fiber is added to the base asphalt and stirred for 40 minutes. The stirring temperature is 185°C and the stirring rate is 4500rpm.
[0085] Example 10: This example is different from Example 1 in that, S2-3-2, the fermentation bacteria liquid of Arthrobacter with a concentration of 0.6% is centrifuged at 5100 r / min for 25 min at room temperature to obtain a precipitate, the precipitate is mixed with trehalose in a mass ratio of 1:1, and then vacuum-freeze-dried under sterile conditions to obtain solid-state fermented Arthrobacter and crushed and sieved.
[0086] Example 11: This example is different from Example 1 in that, S2-3-2, the fermentation bacteria liquid of Arthrobacter with a concentration of 0.8% is centrifuged at 5200 r / min for 30 min at room temperature to obtain a precipitate, the precipitate is mixed with trehalose in a mass ratio of 1:1, and then vacuum-freeze-dried under sterile conditions to obtain solid-state fermented Arthrobacter and crushed and sieved.
[0087] Example 12: This example is different from Example 1 in that, S2-3-3, the solid-state fermentation Bacillus is immersed in a sodium hydroxide solution with a mass concentration of 9% for 2.5 hours, and sunlight is applied during the immersion period, and the light intensity is 30mW. After the immersion, the activated solid-state fermentation Bacillus is obtained.
[0088] Example 13: The difference between this example and Example 1 is that, S2-3-3, the solid-state fermentation Bacillus is immersed in a sodium hydroxide solution with a mass concentration of 10% for 4.5 hours, and sunlight is applied during the immersion period, and the light intensity is 40mW. After the immersion, the activated solid-state fermentation Bacillus is obtained.
[0089] Example 14: This example is different from Example 1 in that the solid-state fermented Bacillus and polyurea fiber obtained in S2-3-3 are mixed in a mass ratio of 1:10 and added to sterile ultrapure deionized water with a solid-liquid ratio of 1 g:22 mL. The mixture is then oscillated at 250 rpm at room temperature for 12 h and then dried to constant weight to obtain polyurea fibers loaded with Bacillus.
[0090] Example 15: The difference between this example and Example 1 is that the solid-state fermentation Bacillus and polyurea fiber obtained in S2-3-3 are mixed in a mass ratio of 1:20 and added to sterile ultrapure deionized water with a solid-liquid ratio of 1 g:24 mL. The mixture is then oscillated at 450 rpm at room temperature for 13 h and then dried to constant weight to obtain polyurea fiber loaded with Bacillus.
[0091] Example 16: This example is different from Example 1 in that the particle size of the polyurea fiber is 90-92 μm, and the particle size of the solid-state fermentation Arthrobacter is 76-80 μm.
[0092] Example 17: This example is different from Example 1 in that the particle size of the polyurea fiber is 96-100 μm, and the particle size of the solid-state fermentation Arthrobacter is 70-72 μm.
[0093] Example 18: This example is different from Example 1 in that modified asphalt, steel slag, mineral powder filler, limestone fine aggregate, stabilizer, and Sasobit warm mix agent are mixed in a mass ratio of 1:6:2.5:6:0.15:0.4, and the particle size of the limestone fine aggregate is 0.05-0.055 mm.
[0094] Example 19: This example is different from Example 1 in that modified asphalt, steel slag, mineral powder filler, limestone fine aggregate, stabilizer, and Sasobit warm mix agent are mixed in a mass ratio of 1:7:0.8:3:0.1:0.3; the particle size of the limestone fine aggregate is 0.065-0.07 mm.
[0095] Example 20: This example is different from Example 1 in that the stabilizer comprises, by mass, 10 parts of sulfur, 4 parts of diisopropylbenzene peroxide and 3 parts of glycerol.
[0096] Example 21: This example is different from Example 1 in that the stabilizer comprises, by mass, 20 parts of sulfur, 3 parts of diisopropylbenzene peroxide and 1 part of glycerol.
[0097] Example 22: This example is different from Example 1 in that, in step S3, mixing is performed at 170°C for 120 seconds.
[0098] Example 23: This example is different from Example 1 in that, in step S3, stirring is performed at 180°C for 150 seconds.
[0099] Example 24: This example differs from Example 1 in that it further includes step S1-4. S1-4: Powder C obtained in S1-3, tetraethyl orthosilicate, and deionized water are mixed in a mass ratio of 1:9:165, placed in a hydrothermal reaction vessel for hydrothermal reaction at a temperature of 165°C for 13 hours; the products are then separated, washed, and dried in turn to obtain steel slag with further morphology control.
[0100] Example 25: This example is different from Example 24 in that the temperature of the hydrothermal reaction is 150°C and the reaction time is 12 hours.
[0101] Example 26: This example is different from Example 24 in that the temperature of the hydrothermal reaction is 180°C and the reaction time is 14 hours.
[0102] Example 27: This example differs from Example 24 in that powder C, tetraethyl orthosilicate, and deionized water are mixed in a mass ratio of 1:8:180.
[0103] Example 28: This example differs from Example 24 in that powder C, ethyl orthosilicate, and deionized water are mixed in a mass ratio of 1:10:150.
[0104] Experimental Example: The description of this experimental example is based on the scheme described in Example 1, and is intended to illustrate the practical application effect of the present invention. For the asphalt mixture prepared in each example, its splitting compressive strength ratio and compressive strength are tested. The splitting compressive strength ratio is tested by the asphalt mixture freeze-thaw splitting test (T0729-2000), and the test is carried out in accordance with the "Testing Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTGE20-2011). Each example is tested five times and the test results are averaged as the test results of this example. The specific exploration is as follows:
[0105] 1. To explore the effect of slag morphology control on the splitting compressive strength ratio and compressive strength of asphalt mixture.
[0106] The difference between the comparative example 1 and the embodiment 1 is that the magnetic field impurity removal is not performed;
[0107] Depend on Figure 1 and Figure 2The results show that the control example 1 lacks magnetic field impurity removal, and the performance is significantly lower than that of examples 1 to 3. Therefore, magnetic field impurity removal has a certain effect on improving the performance of asphalt mixtures. Compared with examples 1 to 3, the slightly larger particle size of the steel slag powder and the corresponding small magnetic field in example 2 will reduce the splitting compressive strength ratio and compressive strength of the asphalt mixture. The performance of example 3 is improved compared with that of example 1, but the improvement rate is small, and smaller powder and larger magnetic field strength are required. Therefore, from the perspective of economy, the parameter effect of example 1 is relatively better.
[0108] By comparing Example 1 and Examples 24 to 28, it can be seen that further regulating the morphology of steel slag powder through hydrothermal reaction can further significantly improve the splitting compressive strength ratio and compressive strength of the asphalt mixture, and the higher the hydrothermal reaction temperature, the better the effect. However, the improvement effect of Example 26 is lower than that of Example 24, and too small or too large a proportion of C powder in the hydrothermal reaction will reduce the splitting compressive strength ratio and compressive strength of the asphalt mixture. Therefore, on the whole, the parameter effect of Example 24 is relatively better.
[0109] 2. Explore the influence of relevant parameters of asphalt modification on the splitting compressive strength ratio and compressive strength of asphalt mixture.
[0110] The difference between Comparative Example 2 and Example 1 is that the volume concentration of carbon dioxide remains unchanged;
[0111] The difference between Comparative Example 3 and Example 1 is that the pressure of carbon dioxide remains unchanged;
[0112] The difference between Control Example 4 and Example 1 is that the solid-state fermentation Arthrobacter is not activated;
[0113] The difference between Control Example 5 and Example 1 is that the polyurea fiber does not carry solid-state fermentation Arthrobacter;
[0114] Depend on Figure 3 and Figure 4 As can be seen from the results, the control examples 2 and 3 lack the parameter changes of carbon dioxide, the control example 4 lacks the activation treatment, and the control example 5 lacks the loaded polyurea fiber. Compared with the asphalt mixtures of Examples 1 and 4 to 17, the performance is significantly reduced. Therefore, the above conditions are all helpful to improve the performance of asphalt mixtures.
[0115] By comparing Examples 1, 4 to 17, it can be seen that the relevant parameters of carbon dioxide are too small or too large, the stirring parameters are too small, the centrifugation parameters of Bacillus are too small, the activation parameters are too small or too large, the parameters of step S2-3-3 are too small or too large, and the particle size ratio of polyurea fiber and solid-state fermentation Bacillus is too small or too large, which will reduce the splitting compressive strength ratio and compressive strength of the asphalt mixture. Examples 7, 9, 11 and 14 have better performance than Example 1, but Examples 7, 9, 11 and 14 require a larger rate and the improvement is relatively low. Therefore, in comparison, the parameter effect of Example 1 is relatively better.
[0116] 3. Investigate the influence of relevant parameters of asphalt modification on the splitting compressive strength ratio and compressive strength of asphalt mixture.
[0117] Depend on Figure 5 and Figure 6 The results show that, compared with Examples 1 and 18 to 23, too small or too large a proportion of modified asphalt, too small or too large a proportion of sulfur in the stabilizer, and too low a mixing temperature will reduce the splitting compressive strength ratio and compressive strength of the asphalt mixture. The performance of Example 23 is better than that of Example 1, but Example 23 requires a higher temperature and a longer time. From the comparison of the improvement range, the parameter effect of Example 1 is relatively better.
[0118] In summary, the splitting compressive strength ratio of the asphalt mixture prepared by the present invention is higher than 92%, and the compressive strength is higher than 73 MPa.
Claims
1. A method for producing high-strength asphalt mixture by compounding steel slag. It is characterized in that The following steps are involved: S1. Slag treatment: The steel slag is crushed and then the morphology of the steel slag is controlled; S2. Asphalt modification: S2-1, firstly, the base asphalt is placed in a carbon dioxide gas atmosphere with a volume concentration of 98.9-99.9% and a pressure of 0.2-0.3 MPa for 10-20 minutes; S2-2, the carbon dioxide gas pressure is adjusted to a negative pressure of -0.15 to -0.05 MPa, and waste bio-oil accounting for 7.5 to 9.5% of the mass of the base asphalt is added and stirred for 15 to 20 minutes at a stirring temperature of 155 to 160° C. and a stirring rate of 1550 to 1650 rpm; S2-3, while maintaining the negative pressure state, adjust the volume concentration of carbon dioxide gas to 92.5-93.5%, add 16-20% of the mass of supported polyurea fiber to the matrix asphalt and stir for 30-40 minutes at a stirring temperature of 175-185°C and a stirring rate of 3500-4500 rpm; After the mixing is completed, modified asphalt is obtained; S3, Mixed: Mix modified asphalt, steel slag, mineral powder filler, limestone fine aggregate, stabilizer and warm mix agent in a mass ratio of 1:6-7:0.8-2.5:3-6:0.1-0.15:0.3-0.4, and mix at 170-180°C for 120-150s.
2. A method for producing high-strength asphalt mixture by compounding steel slag as claimed in claim 1, It is characterized in that In step S1, the morphology control process is: S1-1, firstly grind the steel slag to obtain powder A with a particle size of 15 to 20 mm, and then remove impurities from the powder A using a magnetic field of 620 to 650 Gs; S1-2, further performing intermediate fine grinding on the powder A after impurities are removed in step S1-1 to obtain powder B with a particle size of 5 to 10 mm, and then removing impurities from the powder B using a magnetic field of 750 to 800 Gs; S1-3, further performing advanced fine grinding on the powder B after impurities are removed in step S1-2 to obtain powder C with a particle size of 1 to 2 mm, and then removing impurities from the powder C using a magnetic field of 900 to 950 Gs to obtain steel slag with controlled morphology.
3. A method for producing high-strength asphalt mixture by compounding steel slag as claimed in claim 2, It is characterized in that Also step S1-4, S1-4: Mix the powder C obtained in S1-3, ethyl orthosilicate and deionized water in a mass ratio of 1:8-10:150-180, place in a hydrothermal reaction vessel for hydrothermal reaction at a temperature of 150-180°C for 12-14 hours; then separate, wash and dry the product in turn to obtain steel slag with further morphology control.
4. A method for producing high-strength asphalt mixture by compounding steel slag as claimed in claim 1, It is characterized in that In step S2, the waste bio-oil is one of swill oil, palmitic acid oil and kitchen waste oil.
5. A method for producing high-strength asphalt mixture by compounding steel slag as claimed in claim 1, It is characterized in that In step S2-3, the preparation method of the supported polyurea fiber is: S2-3-1, completely drying the polyurea fiber and grinding it into powder for later use, wherein the particle size of the polyurea fiber is 90 to 100 μm; S2-3-2, centrifuging the fermented Arthrobacter soln with a mass concentration of 0.6-0.8% at 5100-5200 r / min for 25-30 min at room temperature to obtain a precipitate, mixing the precipitate with trehalose at a mass ratio of 1:1, and then vacuum freeze-drying under sterile conditions to obtain solid-state fermented Arthrobacter, which was then crushed and sieved; S2-3-3, soaking the solid-state fermentation Arthrobacter in a sodium hydroxide solution with a mass concentration of 9-10% for 2.5-4.5 hours, and applying sunlight illumination during the soaking period, with a light intensity of 30-40 mW, and obtaining the activated solid-state fermentation Arthrobacter after the soaking; S2-3-4. Mix the solid-state fermented Bacillus and polyurea fiber obtained in S2-3-3 in a mass ratio of 1:10-20 and add them into sterile ultrapure deionized water with a solid-liquid ratio of 1g:22-24mL. Oscillate at room temperature at a speed of 250-450rpm for 12-13h, and then dry to constant weight to obtain polyurea fiber loaded with Bacillus.
6. A method for producing high-strength asphalt mixture by compounding steel slag as claimed in claim 5, It is characterized in that In step S2-3-1, the particle size of the polyurea fiber is 90-100 μm; in step S2-3-2, the particle size of the solid-state fermentation Arthrobacter is 70-80 μm.
7. A method for producing high-strength asphalt mixture by compounding steel slag as claimed in claim 1, It is characterized in that The stabilizer comprises, by weight, 10 to 20 parts of sulfur, 3 to 4 parts of dicumyl peroxide and 1 to 3 parts of glycerol.
8. A method for producing high-strength asphalt mixture by compounding steel slag as claimed in claim 1, It is characterized in that The mineral powder filler is limestone mineral powder that passes through a 200-mesh sieve, and the particle size of the limestone fine aggregate is 0.05-0.07 mm.
9. A method for producing high-strength asphalt mixture by compounding steel slag as claimed in claim 1, It is characterized in that The warm mix agent is Sasobit warm mix agent.