High-performance silicon-based ceramic core capable of realizing balance of solid content and viscosity and preparation method of high-performance silicon-based ceramic core
Through the ratio of composite ceramic powder to photosensitive resin and powder surface modification, combined with carbide reinforcement, the problem of solid content and viscosity balance in the ceramic core is solved, its mechanical properties and dimensional accuracy are improved, and the ceramic core is ensured Core integrity.
Patent Information
- Application Number
- CN202411259368.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The existing technology is difficult to achieve a balance between solid content and viscosity in the preparation of ceramic cores, resulting in insufficient mechanical properties, sintering shrinkage and dimensional accuracy of the ceramic cores, and prone to defects such as interlayer cracking.
The ratio of composite ceramic powder and photosensitive resin is used to improve the dispersion and compatibility of ceramic particles in the slurry by modifying the powder surface and optimizing the viscosity auxiliary ratio, and combining carbide as a performance enhancer to optimize The sintering process to achieve a balance between solid content and viscosity.
It significantly improves the solid content and viscosity balance of the ceramic core, improves its mechanical properties, dimensional accuracy and interlayer strength, ensuring the integrity of the ceramic core in the subsequent casting process.
Smart Images

Figure CN118791291A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic core material design and preparation, and specifically relates to a high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity and a preparation method thereof. Background Art
[0002] As we all know, as a key component for precision casting, the main function of the ceramic core is to match the ceramic shell to provide a complex air-cooled inner cavity structure for the turbine blades of aircraft engines. Therefore, the performance and quality of the ceramic core are closely related to the performance, quality, dimensional accuracy and qualified rate of the turbine blades. At present, the preparation method of ceramic cores is mostly hot injection molding process, but in the face of today's increasingly complex ceramic cores, it is difficult to meet the quality and performance requirements of ceramic cores using traditional preparation methods.
[0003] As a new type of ceramic core preparation technology, photocuring 3D printing technology has the advantages of no need for molds, high molding accuracy, and short preparation cycle, and can prepare ceramic cores with complex structures. However, due to the layer-by-layer curing molding characteristics of photocuring 3D printing technology, defects such as large sintering shrinkage and interlayer cracking are prone to occur during the preparation of ceramic cores, which can easily lead to failure and fracture of the ceramic cores during the subsequent pouring process. In addition, the layer-by-layer curing molding characteristics of photocuring 3D printing technology have a significant impact on the mechanical properties of ceramic cores obtained in different printing directions. The bonding force between layers is much lower than the bonding force of ceramic particles within the layer, which leads to the anisotropy of ceramic core performance.
[0004] High solid content has a positive effect on the structural uniformity inside the ceramic core. In order to obtain a ceramic core with excellent comprehensive performance, a ceramic slurry with a high solid content is an indispensable key factor. However, with the increase of the solid content in the ceramic slurry, the flowability of the ceramic slurry will inevitably decrease, which is not conducive to photocuring molding. Therefore, how to prepare a high-performance silicon-based ceramic core with a balance of solid content and viscosity is a key issue that needs to be solved urgently.
[0005] The invention patent with application publication number CN118307311A discloses a photocurable ceramic core slurry and a preparation method thereof. The raw materials include: 40-70 parts by weight of ceramic matrix powder, 10-15 parts by weight of mineralizer, 6-20 parts by weight of viscosity regulator, 3-10 parts by weight of curing performance regulator, 10-20 parts by weight of slurry main solvent, 5-10 parts by weight of dispersant, and 1-3 parts by weight of photoinitiator; wherein the viscosity regulator is one or more of 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, and propoxylated neopentyl glycol diacrylate, the curing performance regulator is one or more of ethoxylated trimethylolpropane triacrylate, trimethylolpropane triacrylate, and ditrimethylolpropane tetraacrylate, and the slurry main solvent is one or more of 2-phenoxyethyl acrylate, isobornyl methacrylate, isooctyl acrylate, and isodecyl acrylate. The raw materials are mixed to obtain a light-cured ceramic core slurry. The purpose of this technical solution is to prepare a ceramic core slurry with high solid content and low viscosity. However, according to test data, the solid content still needs to be further increased, otherwise the mechanical properties, sintering shrinkage rate and dimensional accuracy of the ceramic core will be reduced.
[0006] The invention patent with application publication number CN118359426A discloses a photocurable 3D printing ceramic core slurry and preparation method, the raw materials include: 65-75 parts by weight of ceramic matrix powder, 10-20 parts by weight of mineralizer, 1-3 parts by weight of photoinitiator, 10-20 parts by weight of photosensitive resin, 3-8 parts by weight of dispersant. The ceramic matrix powder and the mineralizer are mixed and sintered in a reducing atmosphere to obtain a surface-modified solid phase powder, wherein the sintering temperature is 300-800°C and the sintering time is 2-12h; the surface-modified solid phase powder, photosensitive resin, dispersant, and photoinitiator are prepared into a photocurable 3D printing ceramic core slurry, wherein the dispersant is selected from at least two of BYK9076, KOS110, BYK111, KOS163, and BYK180. The purpose of this technical solution is to solve the problem that ceramic particles are difficult to disperse in photosensitive resin in order to prepare a ceramic core slurry with a high solid content. Although the solid content is increased, the fluidity of the ceramic slurry will be reduced, and it is also impossible to ensure that the ceramic core has good mechanical properties and sintering shrinkage. Summary of the invention
[0007] In order to solve the problems existing in the prior art, the present invention provides a high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity, wherein the mass percentage of each substance in the silicon-based ceramic core is 80-90wt% of a composite ceramic powder and 10-20wt% of a photosensitive resin; the mass percentage of each substance in the composite ceramic powder is 80-90wt% of a matrix skeleton material and 10-20wt% of a performance enhancer; the mass percentage of each substance in the matrix skeleton material is 80-90wt% of fused quartz, 5-10wt% of cristobalite and 5-10wt% of silicon dioxide; the mass percentage of each substance in the performance enhancer is 70-85wt% of silicon carbide, 5-15wt% of zirconium carbide and 10-15wt% of boron carbide.
[0008] Preferably, the fused quartz includes three particle sizes, namely 12.5-20 μm, 7.5-12.5 μm, and 0-7.5 μm, and the mass percentages of the fused quartz with particle sizes of 12.5-20 μm, 7.5-12.5 μm, and 0-7.5 μm are 20-30wt%, 20-30wt%, and 50-60wt% respectively; the cristobalite and the silica both include a particle size of 10-20 μm.
[0009] In any of the above schemes, it is preferred that the silicon carbide includes three particle sizes, namely 32.5-50μm, 17.5-32.5μm, and 0-17.5μm, and the silicon carbide with particle sizes of 32.5-50μm, 17.5-32.5μm, and 0-17.5μm accounts for 20-30wt%, 20-30wt%, and 50-60wt% of the silicon carbide respectively; the zirconium carbide and the boron carbide both include a particle size of 30-40μm.
[0010] In any of the above schemes, preferably, the mass percentage of each substance in the photosensitive resin is 80-90wt% of the curing crosslinking agent, 5-10wt% of the viscosity auxiliary agent, 0.5-5wt% of the surface modifier, and 0.5-5wt% of the photocuring auxiliary agent.
[0011] In any of the above schemes, it is preferred that the mass percentage of each substance in the curing cross-linking agent is 50-70wt% of 1,6-hexanediol diacrylate, 10-20wt% of dipropylene glycol diacrylate, 10-20wt% of isobornyl acrylate, and 10-20wt% of isobornyl methacrylate.
[0012] In any of the above schemes, it is preferred that the viscosity aid is any one of phosphate ester, polyphosphate ester, and alkylhydroxyl ammonium salt of an acidic group-containing copolymer.
[0013] In any of the above schemes, it is preferred that the mass percentage of each substance in the surface modifier is 75-85wt% of the silane coupling agent and 15-25wt% of the polyether-modified polydimethylsiloxane.
[0014] In any of the above schemes, it is preferred that the mass percentage of each substance in the photocuring aid is 50-65wt% of 2,4-dihydroxybenzophenone, 25-45wt% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and 5-15wt% of 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester.
[0015] The present invention also provides a method for preparing a high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity, which is used to prepare any of the above-mentioned high-performance silicon-based ceramic cores that achieves a balance between solid content and viscosity, and comprises the following steps in order: Step 1: Prepare silicon-based ceramic slurry according to design requirements; Step 2: placing the container containing the silicon-based ceramic slurry into a vacuum device, and performing vacuum treatment on the silicon-based ceramic slurry to make the interior of the silicon-based ceramic slurry completely free of bubbles; Step 3: Put the silicon-based ceramic slurry into the material tank of the inverted ceramic 3D printing equipment, and print the silicon-based ceramic core blank according to the design requirements; Step 4: Degreasing and sintering the silicon-based ceramic core blank can obtain the silicon-based ceramic core.
[0016] Preferably, in step 1, the method for preparing the silicon-based ceramic slurry comprises the following steps in order: Step (1): weigh and prepare the raw materials according to the design requirements; Step (2): placing fused quartz of various particle sizes in the matrix skeleton material and silicon carbide of various particle sizes in the performance enhancer into a ball mill for ball milling at a ball milling speed of 300-400 rpm and a ball milling time of 4-6 hours, then adding cristobalite and silicon dioxide in the matrix skeleton material and zirconium carbide and boron carbide in the performance enhancer into the ball mill for further ball milling at a ball milling speed of 300-400 rpm and a ball milling time of 4-6 hours. After the ball milling is completed, a composite ceramic powder can be obtained; Step (3): placing each substance in the surface modifier into a ball mill for ball milling, the ball milling speed is 300-400 rpm, and the ball milling time is 6-10 hours; after the ball milling is completed, placing the mixture in the ball mill into a drying box for drying, the drying temperature is 60-100° C., and the drying time is 4-6 hours; after the drying treatment is completed, sieving with a 100-mesh sieve to obtain a surface-modified composite ceramic powder; Step (4): Place the surface-modified composite ceramic powder, the substances in the curing cross-linking agent, the viscosity auxiliary agent, and the substances in the light curing auxiliary agent into a ball mill for ball milling. The ball milling speed is 300-400 rpm and the ball milling time is 6-10 hours. After the ball milling is completed, a silicon-based ceramic slurry can be obtained.
[0017] In step 2, the silicon-based ceramic slurry is subjected to vacuum treatment, the vacuum degree is -0.6 to -0.7 bar, and the pressure holding time is 5 to 10 minutes.
[0018] In step 3, during the printing of the silicon-based ceramic core blank, the main process parameters involved are: curing power 15-30mW / cm 2 , curing time 5-10s, curing thickness 200-300μm, UV light wavelength 405nm, slice layer thickness 50-150μm, paving thickness 150-300μm.
[0019] In step 4, the process system for degreasing and sintering the silicon-based ceramic core blank is as follows: placing the silicon-based ceramic core blank in a muffle furnace, heating the temperature from room temperature to 200-250°C at a heating rate of 0.5-2°C / min, and keeping it warm for 1-2h; continuing to heat it from 200-250°C to 400-450°C at a heating rate of 0.5-2°C / min, and keeping it warm for 1-2h; continuing to heat it from 400-450°C to 500-550°C at a heating rate of 0.1-0.5°C / min, and keeping it warm for 1-2h; continuing to heat it from 500-550°C to 600°C at a heating rate of 0.1-0.5°C / min, and keeping it warm for 1-2h; continuing to heat it from 600°C to 1100-1250°C at a heating rate of 1-3°C / min, and keeping it warm for 5-10h, and then cooling it with the furnace.
[0020] In the present invention, fused silica includes three particle sizes, namely 12.5-20 μm, 7.5-12.5 μm, and 0-7.5 μm, that is, 12.5 μm≤particle size<20 μm, 7.5 μm≤particle size<12.5 μm, and 0 μm≤particle size<7.5 μm; cristobalite and silicon dioxide both include a particle size of 10-20 μm, that is, 10 μm≤particle size<20 μm. m; silicon carbide includes three particle sizes, namely 32.5-50μm, 17.5-32.5μm, and 0-17.5μm, that is, 32.5μm≤particle size<50μm, 17.5μm≤particle size<32.5μm, and 0μm≤particle size<17.5μm; zirconium carbide and boron carbide both include one particle size, both of which are 30-40μm, that is, 30μm≤particle size<40μm. For each particle size, the material is passed through the upper and lower sieve holes in sequence to obtain a material with a particle size between the upper and lower sieve holes, for example: the particle size is 12.5-20μm (12.5μm≤particle size<20μm), that is, the material is passed through the 20μm sieve hole and the 12.5μm sieve hole in sequence to obtain a material with a particle size between 12.5-20μm.
[0021] In the present invention, the viscosity auxiliary agent is any one of phosphate, polyphosphate, and alkylhydroxyl ammonium salt of copolymer containing acidic groups, wherein the phosphate is selected as BYK111, the polyphosphate is selected as BYK110, and the alkylhydroxyl ammonium salt of copolymer containing acidic groups is selected as BYK180. The surface modifier contains silane coupling agent and polyether-modified polydimethylsiloxane, wherein the polyether-modified polydimethylsiloxane is selected as BYK306. The vacuum equipment, inverted ceramic 3D printing equipment, muffle furnace, ball mill, etc. used in the present invention are all commonly used equipment in the field, and no special requirements are made on the equipment model and structure. The ball milling medium is zirconium oxide, and the ball-to-material ratio is 3:2.
[0022] In the present invention, during the entire preparation process of the silicon-based ceramic core, the mass percentage of each component, the mass ratio of each particle size in each component, the order of adding each component, the process parameters of each step, etc. are all very critical. In particular, the grading of fused quartz and silicon carbide must be strictly controlled. Only by synergizing various parameters can the expected technical effect of the present invention be achieved.
[0023] The present invention solves the problem of the incompatibility of the outer surface of ceramic particles with oily photosensitive resins due to the hydrophilicity of hydroxyl groups by modifying the powder surface. At the same time, by optimizing the selection and proportion of viscosity auxiliary agents, the dispersibility of ceramic particles in the slurry is significantly improved. The use of silicone surface modifiers greatly enhances the compatibility of photosensitive resins with matrix skeleton materials, further reduces the viscosity of ceramic slurries, and successfully realizes the preparation of low-viscosity, high-solid content, and high-performance photocuring additive manufacturing silicon-based ceramic cores.
[0024] The present invention improves the compatibility of the matrix through the organic silicon surface modifier, which is beneficial to the dispersion of the composite ceramic powder in the photosensitive resin. At the same time, during the sintering process, the organic silicon resin can react to generate nano-level silicon oxide, which is beneficial to improving the physical properties of the silicon-based ceramic core. Assisted by the increase in solid content, the uniformity of the ceramic microstructure and the consistency of the macroscopic sintering shrinkage are successfully achieved, which is beneficial to improving the comprehensive performance of the silicon-based ceramic core.
[0025] The present invention adopts carbide as a performance enhancer. Carbide is easy to produce oxidation reaction during the sintering process of the ceramic core, and compensates for the sintering shrinkage through volume change, thereby improving the dimensional accuracy of the ceramic core. At the same time, volume expansion will hinder the densification process of ceramic sintering and produce a relatively loose internal structure, thereby increasing the porosity of the ceramic core, which is beneficial to the subsequent removal process of the ceramic core.
[0026] The present invention provides a high-performance silicon-based ceramic core and a preparation method thereof that achieves a balance between solid content and viscosity, and has the following beneficial effects: (1) The material ratio design and preparation process of the silicon-based ceramic core of the present invention can achieve a balance between the solid content and viscosity of the silicon-based ceramic core slurry, which not only significantly increases the solid content of the ceramic slurry but also maintains a relatively low viscosity of the ceramic slurry. At the same time, the prepared silicon-based ceramic core has higher performance.
[0027] (2) The silicon-based ceramic core prepared by the present invention has high dimensional accuracy and high interlayer strength. The interlayer strength of the entire silicon-based ceramic core is uniform and consistent with the intralayer strength, and there are no defects between the layers, thereby ensuring that the ceramic core will not break during the subsequent casting process. Carbide is used in the composite ceramic powder of the present invention. The carbide has a high absorption rate of ultraviolet light, which can significantly inhibit the over-curing area of the silicon-based ceramic core, thereby improving the accuracy of the 3D printing curing forming stage. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 A comparison chart of test results of sintering shrinkage of silicon-based ceramic core specimens in five preferred embodiments of a high-performance silicon-based ceramic core and a preparation method for achieving a balance between solid content and viscosity according to the present invention; Figure 2 This is a microscopic morphology photo of the silicon-based ceramic core in Example 1; Figure 3 This is a microscopic morphology photograph of the silicon-based ceramic core in Example 2; Figure 4 This is a microscopic morphology photo of the silicon-based ceramic core in Example 3; Figure 5 This is a microscopic morphology photograph of the silicon-based ceramic core in Example 4; Figure 6This is a microscopic morphology photograph of the silicon-based ceramic core in Example 5; Figure 7 The surface roughness test results of the silicon-based ceramic core in Example 1; Figure 8 The surface roughness test results of the silicon-based ceramic core in Example 2; Fig. 9 The surface roughness test results of the silicon-based ceramic core in Example 3; Fig.10 The surface roughness test results of the silicon-based ceramic core in Example 4; Fig.11 These are the surface roughness test results of the silicon-based ceramic core in Example 5. DETAILED DESCRIPTION
[0029] In order to further understand the content of the present invention, the present invention will be described in detail below in conjunction with specific embodiments.
[0030] Embodiment 1: According to a preferred embodiment of the high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity of the present invention, the mass percentage of each substance in the silicon-based ceramic core is 85wt% for the composite ceramic powder and 15wt% for the photosensitive resin; the mass percentage of each substance in the composite ceramic powder is 85wt% for the matrix skeleton material and 15wt% for the performance enhancer; the mass percentage of each substance in the matrix skeleton material is 85wt% for fused quartz, 8wt% for cristobalite and 7wt% for silicon dioxide; the mass percentage of each substance in the performance enhancer is 78wt% for silicon carbide, 10wt% for zirconium carbide and 12wt% for boron carbide.
[0031] The fused quartz includes three particle sizes, which are 12.5-20μm, 7.5-12.5μm, and 0-7.5μm, respectively. The mass percentages of the fused quartz with particle sizes of 12.5-20μm, 7.5-12.5μm, and 0-7.5μm are 25wt%, 25wt%, and 50wt% of the fused quartz, respectively; the cristobalite and the silica both include a particle size of 10-20μm.
[0032] The silicon carbide includes three particle sizes, which are 32.5-50μm, 17.5-32.5μm, and 0-17.5μm, respectively. The silicon carbide with particle sizes of 32.5-50μm, 17.5-32.5μm, and 0-17.5μm accounts for 25wt%, 25wt%, and 50wt% of the silicon carbide respectively; the zirconium carbide and the boron carbide both include a particle size of 30-40μm.
[0033] The mass percentage of each substance in the photosensitive resin is 86wt% of the curing crosslinking agent, 8wt% of the viscosity auxiliary agent, 3wt% of the surface modifier, and 3wt% of the light curing auxiliary agent. The mass percentage of each substance in the curing crosslinking agent is 60wt% of 1,6-hexanediol diacrylate, 15wt% of dipropylene glycol diacrylate, 15wt% of isobornyl acrylate, and 10wt% of isobornyl methacrylate. The viscosity auxiliary agent is a phosphate ester, which is selected as BYK111. The mass percentage of each substance in the surface modifier is 80wt% of the silane coupling agent, and 20wt% of the polyether-modified polydimethylsiloxane, wherein the polyether-modified polydimethylsiloxane is selected as BYK306. The mass percentage of each substance in the photocuring aid is 57wt% of 2,4-dihydroxybenzophenone, 35wt% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and 8wt% of 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester.
[0034] This embodiment also provides a method for preparing a high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity, which is used to prepare the high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity, and includes the following steps in order: Step 1: Prepare silicon-based ceramic slurry according to design requirements; Step 2: placing the container containing the silicon-based ceramic slurry into a vacuum device, and performing vacuum treatment on the silicon-based ceramic slurry to make the interior of the silicon-based ceramic slurry completely free of bubbles; Step 3: Put the silicon-based ceramic slurry into the material tank of the inverted ceramic 3D printing equipment, and print the silicon-based ceramic core blank according to the design requirements; Step 4: Degreasing and sintering the silicon-based ceramic core blank can obtain the silicon-based ceramic core.
[0035] In step 1, the method for preparing the silicon-based ceramic slurry comprises the following steps in order: Step (1): weigh and prepare the raw materials according to the design requirements; Step (2): placing fused quartz of various particle sizes in the matrix skeleton material and silicon carbide of various particle sizes in the performance enhancer into a ball mill for ball milling at a ball milling speed of 350 rpm and a ball milling time of 5 h, then adding cristobalite and silicon dioxide in the matrix skeleton material and zirconium carbide and boron carbide in the performance enhancer into the ball mill for further ball milling at a ball milling speed of 350 rpm and a ball milling time of 5 h. After the ball milling is completed, a composite ceramic powder can be obtained; Step (3): placing each substance in the surface modifier into a ball mill for ball milling at a ball milling speed of 350 rpm and a ball milling time of 8 hours; after the ball milling is completed, placing the mixture in the ball mill into a drying oven for drying at a drying temperature of 80° C. and a drying time of 5 hours; after the drying is completed, sieving with a 100-mesh sieve to obtain a surface-modified composite ceramic powder; Step (4): Place the surface-modified composite ceramic powder, the substances in the curing cross-linking agent, the viscosity auxiliary agent, and the substances in the light curing auxiliary agent into a ball mill for ball milling. The ball milling speed is 350 rpm and the ball milling time is 8 hours. After the ball milling is completed, a silicon-based ceramic slurry can be obtained.
[0036] In step 2, the silicon-based ceramic slurry is subjected to vacuum treatment, the vacuum degree is -0.65 bar, and the pressure holding time is 8 minutes.
[0037] In step 3, during the printing of the silicon-based ceramic core blank, the main process parameters involved are: curing power 22mW / cm 2 , curing time 8s, curing thickness 250μm, UV light wavelength 405nm, slice layer thickness 100μm, and material thickness 220μm.
[0038] In step four, the process system for degreasing and sintering the silicon-based ceramic core blank is as follows: place the silicon-based ceramic core blank in a muffle furnace, heat the temperature from room temperature to 225°C at a heating rate of 1.2°C / min, and keep it warm for 1.5 hours; continue to heat the temperature from 225°C to 425°C at a heating rate of 1.2°C / min, and keep it warm for 1.5 hours; continue to heat the temperature from 425°C to 525°C at a heating rate of 0.3°C / min, and keep it warm for 1.5 hours; continue to heat the temperature from 525°C to 600°C at a heating rate of 0.3°C / min, and keep it warm for 1.5 hours; continue to heat the temperature from 600°C to 1175°C at a heating rate of 2°C / min, keep it warm for 8 hours, and then cool it with the furnace.
[0039] In this embodiment, fused quartz includes three particle sizes, namely 12.5-20 μm, 7.5-12.5 μm, and 0-7.5 μm, that is, 12.5 μm ≤ particle size < 20 μm, 7.5 μm ≤ particle size < 12.5 μm, and 0 μm ≤ particle size < 7.5 μm; cristobalite and silicon dioxide both include a particle size of 10-20 μm, that is, 10 μm ≤ particle size < 20 μm. m; silicon carbide includes three particle sizes, namely 32.5-50μm, 17.5-32.5μm, and 0-17.5μm, that is, 32.5μm≤particle size<50μm, 17.5μm≤particle size<32.5μm, and 0μm≤particle size<17.5μm; zirconium carbide and boron carbide both include one particle size, both of which are 30-40μm, that is, 30μm≤particle size<40μm. For each particle size, the material is passed through the upper and lower sieve holes in sequence to obtain a material with a particle size between the upper and lower sieve holes, for example: the particle size is 12.5-20μm (12.5μm≤particle size<20μm), that is, the material is passed through the 20μm sieve hole and the 12.5μm sieve hole in sequence to obtain a material with a particle size between 12.5-20μm.
[0040] In this embodiment, in the entire preparation process of the silicon-based ceramic core, the mass percentage of each component, the mass ratio of each particle size in each component, the order of addition of each component, the process parameters of each step, etc. are very critical, especially the gradation of fused quartz and silicon carbide must be strictly controlled. Only by synergizing various parameters can the expected technical effect of this embodiment be achieved. The vacuum equipment, inverted ceramic 3D printing equipment, muffle furnace, ball mill, etc. used are all commonly used equipment in this field, and no special requirements are made on the equipment model and structure. The ball milling medium is zirconium oxide, and the ball-to-material ratio is 3:2.
[0041] The high-performance silicon-based ceramic core and preparation method of this embodiment that achieves a balance between solid content and viscosity have the following beneficial effects: (1) It can balance the solid content and viscosity of the silicon-based ceramic core slurry, significantly increasing the solid content of the ceramic slurry while maintaining a relatively low viscosity of the ceramic slurry, while making the silicon-based ceramic core have higher performance. (2) It can make the silicon-based ceramic core have higher dimensional accuracy and interlayer strength, and there are no defects between the layers. (3) The use of carbides in the composite ceramic powder can significantly inhibit the over-curing area of the silicon-based ceramic core, thereby improving the accuracy of the 3D printing curing forming stage.
[0042] Embodiment 2: According to another preferred embodiment of the high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity of the present invention, its material formula, preparation process, equipment used, technical principles and beneficial effects are basically the same as those of the first embodiment, except that: The mass percentage of each substance in the silicon-based ceramic core is: 80wt% of the composite ceramic powder and 20wt% of the photosensitive resin; the mass percentage of each substance in the composite ceramic powder is: 80wt% of the matrix skeleton material and 20wt% of the performance enhancer; the mass percentage of each substance in the matrix skeleton material is: 80wt% of fused quartz, 10wt% of cristobalite and 10wt% of silicon dioxide; the mass percentage of each substance in the performance enhancer is: 70wt% of silicon carbide, 15wt% of zirconium carbide and 15wt% of boron carbide.
[0043] The fused quartz includes three particle sizes, which are 12.5-20μm, 7.5-12.5μm, and 0-7.5μm, respectively. The mass percentages of the fused quartz with particle sizes of 12.5-20μm, 7.5-12.5μm, and 0-7.5μm are 20wt%, 20wt%, and 60wt% of the fused quartz, respectively; the cristobalite and the silica both include a particle size of 10-20μm.
[0044] The silicon carbide includes three particle sizes, which are 32.5-50μm, 17.5-32.5μm, and 0-17.5μm, respectively. The silicon carbide with particle sizes of 32.5-50μm, 17.5-32.5μm, and 0-17.5μm accounts for 20wt%, 20wt%, and 60wt% of the silicon carbide respectively; the zirconium carbide and the boron carbide both include a particle size of 30-40μm.
[0045] The mass percentage of each substance in the photosensitive resin is 80wt% of the curing crosslinking agent, 10wt% of the viscosity auxiliary agent, 5wt% of the surface modifier, and 5wt% of the light curing auxiliary agent. The mass percentage of each substance in the curing crosslinking agent is 50wt% of 1,6-hexanediol diacrylate, 10wt% of dipropylene glycol diacrylate, 20wt% of isobornyl acrylate, and 20wt% of isobornyl methacrylate. The viscosity auxiliary agent is a polyphosphate solution, which is selected as BYK110. The mass percentage of each substance in the surface modifier is 75wt% of the silane coupling agent, and 25wt% of the polyether-modified polydimethylsiloxane, wherein the polyether-modified polydimethylsiloxane is selected as BYK306. The mass percentage of each substance in the photocuring aid is 50wt% of 2,4-dihydroxybenzophenone, 45wt% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and 5wt% of 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester.
[0046] In step 1, the preparation method of the silicon-based ceramic slurry comprises the following steps in order: step (1): weighing each raw material according to the design requirements for use; step (2): putting fused quartz of various particle sizes in the matrix skeleton material and silicon carbide of various particle sizes in the performance enhancer into a ball mill for ball milling, the ball milling speed is 300 rpm, and the ball milling time is 6 hours, then adding cristobalite and silicon dioxide in the matrix skeleton material and zirconium carbide and boron carbide in the performance enhancer into the ball mill for further ball milling, the ball milling speed is 300 rpm, and the ball milling time is 6 hours. After the ball milling is completed, a composite ceramic powder can be obtained; step (3): adding the surface modifier The substances in the mixture are put into a ball mill for ball milling at a speed of 300 rpm and a ball milling time of 10 h. After the ball milling is completed, the mixture in the ball mill is put into a drying oven for drying at a temperature of 60° C. and a drying time of 6 h. After the drying is completed, the mixture is sieved using a 100-mesh sieve to obtain a surface-modified composite ceramic powder. Step (4): the surface-modified composite ceramic powder, the substances in the curing cross-linking agent, the viscosity auxiliary agent, and the substances in the light curing auxiliary agent are put into a ball mill for ball milling at a speed of 300 rpm and a ball milling time of 10 h. After the ball milling is completed, a silicon-based ceramic slurry is obtained.
[0047] In step 2, the silicon-based ceramic slurry is subjected to vacuum treatment, the vacuum degree is -0.6 bar, and the pressure holding time is 10 minutes.
[0048] In step 3, during the printing of the silicon-based ceramic core blank, the main process parameters involved are: curing power 15mW / cm 2 , curing time 5s, curing thickness 200μm, UV light wavelength 405nm, slice layer thickness 50μm, and material thickness 150μm.
[0049] In step four, the process system for degreasing and sintering the silicon-based ceramic core blank is as follows: the silicon-based ceramic core blank is placed in a muffle furnace, and the temperature is increased from room temperature to 200°C at a heating rate of 0.5°C / min, and kept warm for 2 hours; the temperature is continued to be increased from 200°C to 400°C at a heating rate of 0.5°C / min, and kept warm for 2 hours; the temperature is continued to be increased from 400°C to 500°C at a heating rate of 0.1°C / min, and kept warm for 2 hours; the temperature is continued to be increased from 500°C to 600°C at a heating rate of 0.1°C / min, and kept warm for 2 hours; the temperature is continued to be increased from 600°C to 1100°C at a heating rate of 1°C / min, and kept warm for 10 hours, and then cooled with the furnace.
[0050] Embodiment three: According to another preferred embodiment of the high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity of the present invention, its material formula, preparation process, equipment used, technical principles and beneficial effects are basically the same as those of the first embodiment, except that: The mass percentage of each substance in the silicon-based ceramic core is: 90wt% of the composite ceramic powder and 10wt% of the photosensitive resin; the mass percentage of each substance in the composite ceramic powder is: 90wt% of the matrix skeleton material and 10wt% of the performance enhancer; the mass percentage of each substance in the matrix skeleton material is: 90wt% of fused quartz, 5wt% of cristobalite and 5wt% of silicon dioxide; the mass percentage of each substance in the performance enhancer is: 85wt% of silicon carbide, 5wt% of zirconium carbide and 10wt% of boron carbide.
[0051] The fused quartz includes three particle sizes, which are 12.5-20μm, 7.5-12.5μm, and 0-7.5μm, respectively. The mass percentages of the fused quartz with particle sizes of 12.5-20μm, 7.5-12.5μm, and 0-7.5μm are 30wt%, 20wt%, and 50wt% of the fused quartz, respectively; the cristobalite and the silica both include a particle size of 10-20μm.
[0052] The silicon carbide includes three particle sizes, which are 32.5-50μm, 17.5-32.5μm, and 0-17.5μm, respectively. The silicon carbide with particle sizes of 32.5-50μm, 17.5-32.5μm, and 0-17.5μm accounts for 30wt%, 20wt%, and 50wt% of the silicon carbide respectively; the zirconium carbide and the boron carbide both include a particle size of 30-40μm.
[0053] The mass percentage of each substance in the photosensitive resin is 90wt% of the curing crosslinking agent, 5wt% of the viscosity auxiliary agent, 1wt% of the surface modifier, and 4wt% of the light curing auxiliary agent. The mass percentage of each substance in the curing crosslinking agent is 70wt% of 1,6-hexanediol diacrylate, 10wt% of dipropylene glycol diacrylate, 10wt% of isobornyl acrylate, and 10wt% of isobornyl methacrylate. The viscosity auxiliary agent is an alkylhydroxyl ammonium salt solution of an acidic group copolymer, which is selected as BYK180. The mass percentage of each substance in the surface modifier is 85wt% of the silane coupling agent, and 15wt% of the polyether-modified polydimethylsiloxane, wherein the polyether-modified polydimethylsiloxane is selected as BYK306. The mass percentage of each substance in the photocuring aid is 65wt% of 2,4-dihydroxybenzophenone, 25wt% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and 10wt% of 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester.
[0054] In step 1, the preparation method of the silicon-based ceramic slurry comprises the following steps in order: step (1): weighing each raw material according to the design requirements for use; step (2): putting fused quartz of various particle sizes in the matrix skeleton material and silicon carbide of various particle sizes in the performance enhancer into a ball mill for ball milling, the ball milling speed is 400 rpm, and the ball milling time is 4 hours, then adding cristobalite and silicon dioxide in the matrix skeleton material and zirconium carbide and boron carbide in the performance enhancer into the ball mill for further ball milling, the ball milling speed is 400 rpm, and the ball milling time is 4 hours. After the ball milling is completed, a composite ceramic powder can be obtained; step (3): The various substances in the curing agent are placed in a ball mill for ball milling at a speed of 400 rpm and a ball milling time of 6 hours; after the ball milling is completed, the mixture in the ball mill is placed in a drying oven for drying at a temperature of 100°C and a drying time of 4 hours; after the drying is completed, the mixture is sieved using a 100-mesh sieve to obtain a surface-modified composite ceramic powder; step (4): the surface-modified composite ceramic powder, the various substances in the curing cross-linking agent, the viscosity auxiliary agent, and the various substances in the light curing auxiliary agent are placed in a ball mill for ball milling at a speed of 400 rpm and a ball milling time of 6 hours. After the ball milling is completed, a silicon-based ceramic slurry can be obtained.
[0055] In step 2, the silicon-based ceramic slurry is subjected to vacuum treatment, the vacuum degree is -0.7 bar, and the pressure holding time is 5 minutes.
[0056] In step 3, during the printing of the silicon-based ceramic core blank, the main process parameters involved are: curing power 30mW / cm 2 , curing time 10s, curing thickness 300μm, UV light wavelength 405nm, slice layer thickness 150μm, and material thickness 300μm.
[0057] In step four, the process system for degreasing and sintering the silicon-based ceramic core blank is as follows: place the silicon-based ceramic core blank in a muffle furnace, heat the temperature from room temperature to 250°C at a heating rate of 2°C / min, and keep it warm for 1 hour; continue to heat the temperature from 250°C to 450°C at a heating rate of 2°C / min, and keep it warm for 1 hour; continue to heat the temperature from 450°C to 550°C at a heating rate of 0.5°C / min, and keep it warm for 1 hour; continue to heat the temperature from 550°C to 600°C at a heating rate of 0.5°C / min, and keep it warm for 1 hour; continue to heat the temperature from 600°C to 1250°C at a heating rate of 3°C / min, and keep it warm for 5 hours, and then cool with the furnace.
[0058] Embodiment 4: According to another preferred embodiment of the high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity of the present invention, its material formula, preparation process, equipment used, technical principles and beneficial effects are basically the same as those of the first embodiment, except that: The mass percentage of each substance in the silicon-based ceramic core is: 82wt% of the composite ceramic powder and 18wt% of the photosensitive resin; the mass percentage of each substance in the composite ceramic powder is: 82wt% of the matrix skeleton material and 18wt% of the performance enhancer; the mass percentage of each substance in the matrix skeleton material is: 82wt% of fused quartz, 9wt% of cristobalite and 9wt% of silicon dioxide; the mass percentage of each substance in the performance enhancer is: 74wt% of silicon carbide, 13wt% of zirconium carbide and 13wt% of boron carbide.
[0059] The fused quartz includes three particle sizes, which are 12.5-20μm, 7.5-12.5μm, and 0-7.5μm, respectively. The mass percentages of the fused quartz with particle sizes of 12.5-20μm, 7.5-12.5μm, and 0-7.5μm are 22wt%, 23wt%, and 55wt% of the fused quartz, respectively; the cristobalite and the silica both include a particle size of 10-20μm.
[0060] The silicon carbide includes three particle sizes, which are 32.5-50μm, 17.5-32.5μm, and 0-17.5μm, respectively. The silicon carbide with particle sizes of 32.5-50μm, 17.5-32.5μm, and 0-17.5μm accounts for 22wt%, 23wt%, and 55wt% of the silicon carbide respectively; the zirconium carbide and the boron carbide both include a particle size of 30-40μm.
[0061] The mass percentage of each substance in the photosensitive resin is 83wt% of the curing crosslinking agent, 12wt% of the viscosity auxiliary agent, 4wt% of the surface modifier, and 1wt% of the light curing auxiliary agent. The mass percentage of each substance in the curing crosslinking agent is 55wt% of 1,6-hexanediol diacrylate, 20wt% of dipropylene glycol diacrylate, 12wt% of isobornyl acrylate, and 13wt% of isobornyl methacrylate. The viscosity auxiliary agent is a polyphosphate solution, which is selected as BYK110. The mass percentage of each substance in the surface modifier is 78wt% of the silane coupling agent, and 22wt% of the polyether-modified polydimethylsiloxane, wherein the polyether-modified polydimethylsiloxane is selected as BYK306. The mass percentage of each substance in the photocuring aid is 54wt% of 2,4-dihydroxybenzophenone, 40wt% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and 6wt% of 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester.
[0062] In step 1, the preparation method of the silicon-based ceramic slurry comprises the following steps in order: step (1): weighing each raw material according to the design requirements for use; step (2): putting fused quartz of various particle sizes in the matrix skeleton material and silicon carbide of various particle sizes in the performance enhancer into a ball mill for ball milling, the ball milling speed is 320 rpm, and the ball milling time is 5.5 hours, then adding cristobalite and silicon dioxide in the matrix skeleton material and zirconium carbide and boron carbide in the performance enhancer into the ball mill for further ball milling, the ball milling speed is 320 rpm, and the ball milling time is 5.5 hours. After the ball milling is completed, a composite ceramic powder can be obtained; step (3): The substances in the curing agent are placed in a ball mill for ball milling at a speed of 320 rpm and a ball milling time of 9 hours. After the ball milling is completed, the mixture in the ball mill is placed in a drying oven for drying at a temperature of 70° C. and a drying time of 5.5 hours. After the drying is completed, the mixture is sieved using a 100-mesh sieve to obtain a surface-modified composite ceramic powder. Step (4): The surface-modified composite ceramic powder, the substances in the curing cross-linking agent, the viscosity auxiliary agent, and the substances in the light curing auxiliary agent are placed in a ball mill for ball milling at a speed of 320 rpm and a ball milling time of 9 hours. After the ball milling is completed, a silicon-based ceramic slurry is obtained.
[0063] In step 2, the silicon-based ceramic slurry is subjected to vacuum treatment, the vacuum degree is -0.7 bar, and the pressure holding time is 9 minutes.
[0064] In step 3, during the printing of the silicon-based ceramic core blank, the main process parameters involved are: curing power 20mW / cm 2, curing time 7s, curing thickness 220μm, UV light wavelength 405nm, slice layer thickness 80μm, and material thickness 180μm.
[0065] In step 4, the process system for degreasing and sintering the silicon-based ceramic core blank is as follows: placing the silicon-based ceramic core blank in a muffle furnace, heating the temperature from room temperature to 210°C at a heating rate of 0.8°C / min, and keeping it warm for 1.8 hours; continuing to heat the temperature from 210°C to 410°C at a heating rate of 0.8°C / min, and keeping it warm for 1.8 hours; continuing to heat the temperature from 410°C to 510°C at a heating rate of 0.2°C / min, and keeping it warm for 1.8 hours; continuing to heat the temperature from 510°C to 600°C at a heating rate of 0.2°C / min, and keeping it warm for 1.8 hours; continuing to heat the temperature from 600°C to 1150°C at a heating rate of 1.5°C / min, keeping it warm for 9 hours, and then cooling with the furnace.
[0066] Embodiment five: According to another preferred embodiment of the high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity of the present invention, its material formula, preparation process, equipment used, technical principles and beneficial effects are basically the same as those of the first embodiment, except that: The mass percentage of each substance in the silicon-based ceramic core is: 88wt% of the composite ceramic powder and 12wt% of the photosensitive resin; the mass percentage of each substance in the composite ceramic powder is: 88wt% of the matrix skeleton material and 12wt% of the performance enhancer; the mass percentage of each substance in the matrix skeleton material is: 88wt% of fused quartz, 6wt% of cristobalite and 6wt% of silicon dioxide; the mass percentage of each substance in the performance enhancer is: 82wt% of silicon carbide, 7wt% of zirconium carbide and 11wt% of boron carbide.
[0067] The fused quartz includes three particle sizes, which are 12.5-20μm, 7.5-12.5μm, and 0-7.5μm, respectively. The mass percentages of the fused quartz with particle sizes of 12.5-20μm, 7.5-12.5μm, and 0-7.5μm are 20wt%, 30wt%, and 50wt% of the fused quartz, respectively; the cristobalite and the silica both include a particle size of 10-20μm.
[0068] The silicon carbide includes three particle sizes, which are 32.5-50μm, 17.5-32.5μm, and 0-17.5μm, respectively. The silicon carbide with particle sizes of 32.5-50μm, 17.5-32.5μm, and 0-17.5μm accounts for 20wt%, 30wt%, and 50wt% of the silicon carbide respectively; the zirconium carbide and the boron carbide both include a particle size of 30-40μm.
[0069] The mass percentage of each substance in the photosensitive resin is 88wt% of the curing crosslinking agent, 6wt% of the viscosity auxiliary agent, 3wt% of the surface modifier, and 3wt% of the light curing auxiliary agent. The mass percentage of each substance in the curing crosslinking agent is 65wt% of 1,6-hexanediol diacrylate, 12wt% of dipropylene glycol diacrylate, 10wt% of isobornyl acrylate, and 13wt% of isobornyl methacrylate. The viscosity auxiliary agent is a phosphate ester, which is selected as BYK111. The mass percentage of each substance in the surface modifier is 82wt% of the silane coupling agent, and 18wt% of the polyether-modified polydimethylsiloxane, wherein the polyether-modified polydimethylsiloxane is selected as BYK306. The mass percentage of each substance in the photocuring aid is 60wt% of 2,4-dihydroxybenzophenone, 25wt% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and 15wt% of 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester.
[0070] In step 1, the preparation method of the silicon-based ceramic slurry comprises the following steps in order: step (1): weighing each raw material according to the design requirements for use; step (2): putting fused quartz of various particle sizes in the matrix skeleton material and silicon carbide of various particle sizes in the performance enhancer into a ball mill for ball milling, the ball milling speed is 380 rpm, and the ball milling time is 4.5 hours, then adding cristobalite and silicon dioxide in the matrix skeleton material and zirconium carbide and boron carbide in the performance enhancer into the ball mill for further ball milling, the ball milling speed is 380 rpm, and the ball milling time is 4.5 hours. After the ball milling is completed, a composite ceramic powder can be obtained; step (3): The substances in the curing agent are placed in a ball mill for ball milling at a speed of 380 rpm and a ball milling time of 7 hours. After the ball milling is completed, the mixture in the ball mill is placed in a drying oven for drying at a temperature of 90° C. and a drying time of 4.5 hours. After the drying is completed, the mixture is sieved using a 100-mesh sieve to obtain a surface-modified composite ceramic powder. Step (4): The surface-modified composite ceramic powder, the substances in the curing cross-linking agent, the viscosity auxiliary agent, and the substances in the light curing auxiliary agent are placed in a ball mill for ball milling at a speed of 380 rpm and a ball milling time of 7 hours. After the ball milling is completed, a silicon-based ceramic slurry is obtained.
[0071] In step 2, the silicon-based ceramic slurry is subjected to vacuum treatment, the vacuum degree is -0.6 bar, and the pressure holding time is 7 minutes.
[0072] In step 3, during the printing of the silicon-based ceramic core blank, the main process parameters involved are: curing power 28mW / cm 2, curing time 9s, curing thickness 280μm, UV light wavelength 405nm, slice layer thickness 120μm, and material thickness 260μm.
[0073] In step four, the process system for degreasing and sintering the silicon-based ceramic core blank is as follows: placing the silicon-based ceramic core blank in a muffle furnace, heating the temperature from room temperature to 240°C at a heating rate of 1.6°C / min, and keeping it warm for 1.2 hours; continuing to heat it from 240°C to 440°C at a heating rate of 1.6°C / min, and keeping it warm for 1.2 hours; continuing to heat it from 440°C to 540°C at a heating rate of 0.4°C / min, and keeping it warm for 1.2 hours; continuing to heat it from 540°C to 600°C at a heating rate of 0.4°C / min, and keeping it warm for 1.2 hours; continuing to heat it from 600°C to 1200°C at a heating rate of 2.5°C / min, and keeping it warm for 7 hours, and then cooling it with the furnace.
[0074] The silicon-based ceramic cores prepared in the above five embodiments were subjected to various performance tests, and the test methods, test environments, and specimen sizes were the same. The sintering shrinkage test was conducted using specimens with a length of 60 mm, a width of 4 mm, and a height of 10 mm. The test results of the sintering shrinkage are shown in Tables 1 and Figure 1 The viscosity of the ceramic core slurry was tested by rheological test, and the interlaminar strength and intralaminar strength of the silicon-based ceramic core after sintering were tested by three-point bending method. The loading rate was 0.5 mm / s. The test results are shown in Table 2.
[0075] The microscopic morphology of the silicon-based ceramic cores prepared in the five embodiments was tested by scanning electron microscopy, and the microscopic morphology photos thereof are shown in FIG. Figure 2-6 The surface roughness of the silicon-based ceramic cores prepared in the five embodiments was tested using a surface roughness measuring instrument. The test results are shown in Tables 3 and Figure 7-11 shown.
[0076] According to the above Tables 1-3, Figure 1-11 It can be seen from the experimental data that the technical solution of the above embodiment can achieve a balance between the solid content and viscosity of the silicon-based ceramic core slurry, which not only significantly increases the solid content of the ceramic slurry but also maintains a relatively low viscosity of the ceramic slurry. At the same time, the prepared silicon-based ceramic core has high dimensional accuracy and interlayer strength. The interlayer strength and intralayer strength of the entire silicon-based ceramic core are uniform and consistent, and there are no defects between the layers, thereby ensuring that the ceramic core will not break during the subsequent casting process. The chemical reagents, powder materials, etc. used in the above embodiments were purchased from Aladdin Reagent Co., Ltd. and Sinopharm Chemical Reagent Co., Ltd.
[0077] Special note: The technical solution of the present invention involves many parameters, and the synergistic effects between the various parameters need to be comprehensively considered to obtain the beneficial effects and significant progress of the present invention. Moreover, the value ranges of the various parameters in the technical solution are obtained after a large number of experiments. For each parameter and the combination of each parameter, the inventor has recorded a large amount of experimental data. Due to space limitations, the specific experimental data will not be disclosed here.
[0078] It is not difficult for those skilled in the art to understand that the high-performance silicon-based ceramic core and preparation method for achieving a balance between solid content and viscosity of the present invention include any combination of the invention content and specific implementation methods of the above-mentioned invention specification and the various parts shown in the drawings. Due to the limited space and to make the specification concise, the various schemes composed of these combinations are not described one by one. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity, characterized in that: The mass percentages of each substance in the silicon-based ceramic core are: 80-90wt% of the composite ceramic powder and 10-20wt% of the photosensitive resin; the mass percentages of each substance in the composite ceramic powder are: 80-90wt% of the matrix skeleton material and 10-20wt% of the performance enhancer; the mass percentages of each substance in the matrix skeleton material are: 80-90wt% of fused quartz, 5-10wt% of cristobalite and 5-10wt% of silicon dioxide; the mass percentages of each substance in the performance enhancer are: 70-85wt% of silicon carbide, 5-15wt% of zirconium carbide and 10-15wt% of boron carbide.
2. The high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity according to claim 1, characterized in that: The fused quartz includes three particle sizes, which are 12.5-20μm, 7.5-12.5μm, and 0-7.5μm, respectively. The mass percentages of the fused quartz with particle sizes of 12.5-20μm, 7.5-12.5μm, and 0-7.5μm are 20-30wt%, 20-30wt%, and 50-60wt% of the fused quartz, respectively; the cristobalite and the silica both include a particle size of 10-20μm.
3. The high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity according to claim 2, characterized in that: The silicon carbide includes three particle sizes, which are 32.5-50μm, 17.5-32.5μm, and 0-17.5μm, respectively. The silicon carbide with particle sizes of 32.5-50μm, 17.5-32.5μm, and 0-17.5μm accounts for 20-30wt%, 20-30wt%, and 50-60wt% of the silicon carbide, respectively; the zirconium carbide and the boron carbide both include a particle size of 30-40μm.
4. The high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity according to claim 3, characterized in that: The mass percentage of each substance in the photosensitive resin is 80-90wt% of the curing cross-linking agent, 5-10wt% of the viscosity auxiliary agent, 0.5-5wt% of the surface modifier, and 0.5-5wt% of the light curing auxiliary agent.
5. The high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity according to claim 4, characterized in that: The mass percentage of each substance in the curing cross-linking agent is 50-70wt% of 1,6-hexanediol diacrylate, 10-20wt% of dipropylene glycol diacrylate, 10-20wt% of isobornyl acrylate, and 10-20wt% of isobornyl methacrylate.
6. The high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity according to claim 5, characterized in that: The viscosity auxiliary agent is any one of phosphate ester, polyphosphate ester, and alkylhydroxyl ammonium salt of an acidic group-containing copolymer.
7. The high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity according to claim 6, characterized in that: The mass percentage of each substance in the surface modifier is 75-85wt% of the silane coupling agent and 15-25wt% of the polyether-modified polydimethylsiloxane.
8. The high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity according to claim 7, characterized in that: The mass percentage of each substance in the photocuring aid is 50-65wt% of 2,4-dihydroxybenzophenone, 25-45wt% of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and 5-15wt% of 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester.
9. A method for preparing a high-performance silicon-based ceramic core that achieves a balance between solid content and viscosity, characterized in that: The method for preparing a high-performance silicon-based ceramic core having a balance between solid content and viscosity according to any one of claims 1 to 8 comprises the following steps in chronological order: Step 1: Prepare silicon-based ceramic slurry according to design requirements; Step 2: placing the container containing the silicon-based ceramic slurry into a vacuum device, and performing vacuum treatment on the silicon-based ceramic slurry to make the interior of the silicon-based ceramic slurry completely free of bubbles; Step 3: Put the silicon-based ceramic slurry into the material tank of the inverted ceramic 3D printing equipment, and print the silicon-based ceramic core blank according to the design requirements; Step 4: Degreasing and sintering the silicon-based ceramic core blank can obtain the silicon-based ceramic core.
10. The method for preparing a high-performance silicon-based ceramic core with a balanced solid content and viscosity according to claim 9, characterized in that: In step 1, the method for preparing the silicon-based ceramic slurry comprises the following steps in order: Step (1): weigh and prepare the raw materials according to the design requirements; Step (2): placing fused quartz of various particle sizes in the matrix skeleton material and silicon carbide of various particle sizes in the performance enhancer into a ball mill for ball milling at a ball milling speed of 300-400 rpm and a ball milling time of 4-6 hours, then adding cristobalite and silicon dioxide in the matrix skeleton material and zirconium carbide and boron carbide in the performance enhancer into the ball mill for further ball milling at a ball milling speed of 300-400 rpm and a ball milling time of 4-6 hours. After the ball milling is completed, a composite ceramic powder can be obtained; Step (3): placing each substance in the surface modifier into a ball mill for ball milling, the ball milling speed is 300-400 rpm, and the ball milling time is 6-10 hours; after the ball milling is completed, placing the mixture in the ball mill into a drying box for drying, the drying temperature is 60-100° C., and the drying time is 4-6 hours; after the drying treatment is completed, sieving with a 100-mesh sieve to obtain a surface-modified composite ceramic powder; Step (4): placing the surface-modified composite ceramic powder, the substances in the curing cross-linking agent, the viscosity auxiliary agent, and the substances in the light curing auxiliary agent into a ball mill for ball milling at a ball milling speed of 300-400 rpm for a ball milling time of 6-10 hours. After the ball milling is completed, a silicon-based ceramic slurry can be obtained; In step 2, the silicon-based ceramic slurry is subjected to vacuum treatment, the vacuum degree is -0.6 to -0.7 bar, and the pressure holding time is 5 to 10 minutes; In step 3, during the printing of the silicon-based ceramic core blank, the main process parameters involved are: curing power 15-30mW / cm 2 , curing time 5-10s, curing thickness 200-300μm, UV wavelength 405nm, slice layer thickness 50-150μm, paving thickness 150-300μm; In step 4, the process system for degreasing and sintering the silicon-based ceramic core blank is as follows: placing the silicon-based ceramic core blank in a muffle furnace, heating the temperature from room temperature to 200-250°C at a heating rate of 0.5-2°C / min, and keeping it warm for 1-2h; continuing to heat it from 200-250°C to 400-450°C at a heating rate of 0.5-2°C / min, and keeping it warm for 1-2h; continuing to heat it from 400-450°C to 500-550°C at a heating rate of 0.1-0.5°C / min, and keeping it warm for 1-2h; continuing to heat it from 500-550°C to 600°C at a heating rate of 0.1-0.5°C / min, and keeping it warm for 1-2h; continuing to heat it from 600°C to 1100-1250°C at a heating rate of 1-3°C / min, and keeping it warm for 5-10h, and then cooling it with the furnace.
Citation Information
Patent Citations
Silicon-based ceramic core slurry and application thereof
CN112500143A
3D printing silicon oxide ceramic slurry formula and silicon oxide powder preparation process thereof
CN113860859A
Fused quartz photocuring forming method based on introduction of ZrO2-B4C
CN116444282A
Method for manufacturing aluminum powder reinforced silicon-based ceramic core through photocuring additive
CN118026711A
Preparation method of cristobalite content controllable photocuring 3D printing silicon-based ceramic core
CN118359425A
Cited By
Ceramic core surface modification method for improving quality of inner cavity of single crystal hollow blade
CN119035461A
Photo-curing silicon-based ceramic core slurry for investment casting and preparation method and application of photo-curing silicon-based ceramic core slurry
CN119387496A