A catalyst for PBAT polymerization and its preparation method and application

The catalyst preparation by titanium tetrachloride, ethanolamine and phosphate esters was solved, and the side reaction problem caused by the easy hydrolysis of tetrabutyl titanate catalyst in PBAT polymerization was improved, and the mechanical properties and bright color of PBAT were improved, which broadened its application areas.

CN118791721BActive Publication Date: 2024-12-06EAST CHINA ENGINEERING SCIENCE AND TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411269129.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-06
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The tetrabutyl titanate catalyst used during PBAT polymerization is easy to hydrolyze, resulting in side reactions, resulting in yellow and red color of PBAT polyester, high carboxyl value, and poor mechanical properties, which limits its application.

Method used

The catalyst is prepared by titanium tetrachloride, ethanolamine and phosphate. The first precursor solution is activated, the second precursor solution is formed by reacting, and reacting with the phosphate to form a catalyst. It is used for PBAT polymerization to form a stable complex and reduce the Reaction activation energy promotes polymerization reaction.

Benefits of technology

It improves the mechanical properties and physical chemical properties of PBAT polyester, with bright white color, low carboxylic value, tensile strength ≥30 MPa, and elongation at break ≥600%, broadening the application field of PBAT.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a catalyst for PBAT polymerization, a preparation method and application thereof. The catalyst is prepared from titanium tetrachloride, ethanolamine and phosphate. After testing, the PBAT polyester obtained by polymerization using the catalyst provided by the present invention has a bright white color, L≥78, a≤3, b≤8, and a terminal carboxyl content of less than 30 mol / t; the mechanical properties of PBAT: tensile strength ≥30 MPa, elongation at break ≥600%. It can be seen that the catalyst provided by the present invention improves the product performance of the PBAT masterbatch and broadens the use conditions and application fields of PBAT. In addition, the catalyst provided by the present invention can reduce the carboxyl content and improve the hue during the polymerization of PBAT, which has important guiding significance for the industrial production and application of PBAT.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts, and in particular relates to a catalyst for PBAT polymerization and a preparation method and application thereof. Background Art

[0002] With the vigorous development of the global plastic chemical industry, people's lives and work are full of plastic products, which provide a lot of convenience for human production and life. At present, the high molecular polyester materials developed mainly based on petroleum have the advantages of low price, stable performance, and special properties after modification. The plastic products prepared are widely used in all walks of life.

[0003] There are many types of polyester materials. According to their characteristics and application fields, they can be divided into the following categories: polyethylene terephthalate, referred to as PET polyester, has good physical properties and chemical stability, as well as high temperature resistance, corrosion resistance and high transparency. It is widely used in beverage bottles, food packaging, fibers, stationery, medical devices and other fields; polybutylene terephthalate, referred to as PBT polyester, has good mechanical properties, heat resistance, chemical resistance, conductivity and electrical insulation, and is widely used in automotive parts, electronic accessories, industrial equipment and other fields; poly (1,4-cyclohexanedimethanol terephthalate), referred to as PCT polyester, has good mechanical properties, heat resistance, chemical corrosion resistance, and can withstand high temperature conditions. It is used in electronic products, automotive parts and medical devices and other fields.

[0004] In order to reduce the harm caused by non-degradable plastics, a series of measures need to be taken, such as reducing the use of disposable plastic products, promoting garbage sorting and recycling, or developing degradable plastics to partially replace the use of non-degradable plastics, thereby reducing pollution and reducing harm to organisms. Among them, polybutylene terephthalate adipate (PBAT) is formed by the esterification polymerization of some aliphatic dibasic acids and short-chain diols, and aromatic dibasic acids are introduced to improve the rigidity of the product. Therefore, PBAT products have both the "flexibility" of aliphatic products and the "rigidity" of aromatic products. Downstream products prepared using PBAT masterbatch can have the characteristics of "rigidity and flexibility". In addition, in seawater or compost, aliphatic PBAT is easily degraded by natural weathering or microorganisms. Based on the above two points, PBAT has great advantages in product application areas and ecological environmental protection. At present, the preparation of PBAT can adopt the co-esterification process. The main reaction process is to add terephthalic acid, adipic acid and 1,4-butanediol into the reactor in a certain mass ratio, and then add a certain amount of catalyst to carry out esterification and polymerization under specific reaction conditions to obtain PBAT melt, and finally prepare PBAT particles by pelletizing through a pelletizer.

[0005] At present, tetrabutyl titanate is usually used as a catalyst in the PBAT polymerization process, but tetrabutyl titanate is easily hydrolyzed and easily causes side reactions during the polymerization process, resulting in yellow and red PBAT polyester, high carboxyl value, and poor mechanical properties, which limits the application and development of PBAT downstream products. Therefore, it is necessary to develop a catalyst to prepare PBAT with bright white color and excellent mechanical properties. Summary of the invention

[0006] In view of this, the object of the present invention is to provide a catalyst for PBAT polymerization and a preparation method and application thereof. The use of the catalyst can effectively improve the mechanical properties and physicochemical properties of PBAT polyester.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing a catalyst for PBAT polymerization, comprising the following steps:

[0009] S1: mixing titanium tetrachloride with a solvent at 30-50° C. and activating the mixture to obtain a first precursor solution;

[0010] S2: mixing and reacting the first precursor solution with ethanolamine at 50-80° C. to obtain a second precursor solution;

[0011] S3: mixing the second precursor solution with the phosphate ester at 60-80° C. and reacting to obtain a catalyst.

[0012] Preferably, the solvent is selected from any one or more of isopropanol, n-propanol, 1,4-butanediol or 1,3-butanediol.

[0013] Preferably, the mass ratio of titanium tetrachloride to solvent is 1:7-1:20.

[0014] Preferably, the mass ratio of the ethanolamine to the solvent is 1:0.7 to 1:1.86.

[0015] Preferably, the mass ratio of the phosphate ester to the solvent is 1:0.46 to 1:1.5.

[0016] Preferably, the phosphate ester is selected from any one or more of monoethyl phosphate, diethyl phosphate or triethyl phosphate.

[0017] Preferably, after the reaction in step S3 is completed, the following steps are further included:

[0018] The obtained solution was allowed to stand at 30-40° C. for 24-48 h, and filtered to obtain a catalyst.

[0019] In a second aspect, the present invention provides a catalyst prepared by the above preparation method, wherein the catalyst is a transparent liquid, the density of the catalyst is 1.2-1.7 g / mL, and the viscosity at 25°C is 96-130 mPa·s.

[0020] In a third aspect, the present invention also provides an application of the above catalyst in PBAT polymerization.

[0021] Preferably, in the above application, the preparation ratio of the catalyst to the reactant is (1-5):1000.

[0022] Preferably, the reactants include terephthalic acid, adipic acid and 1,4-butanediol.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The catalyst provided by the present invention is prepared from titanium tetrachloride, ethanolamine and phosphate, and does not introduce any heavy metal "antimony" and "germanium" chemical substances, which can reduce the pressure on the environment and is biofriendly;

[0025] (2) The catalyst provided by the present invention, wherein the phosphate ester substance can eliminate the free radicals generated by the degradation and oxidation during the polymerization of terephthalic acid, adipic acid and 1,4-butanediol, inhibit the degradation reaction, and thus improve the product color. At the same time, the catalyst of the present invention can provide active sites for the polymerization to obtain PBAT, wherein the titanium atom in titanium tetrachloride acts as a Lewis acid center and interacts with the carbonyl oxygen atom and the hydroxyl group in the reactant (i.e., terephthalic acid, adipic acid and 1,4-butanediol) molecules to form a stable complex. The formation of the complex makes the interaction between the reactant molecules closer, reduces the activation energy of the reaction, and makes the reaction easier to proceed. The catalyst undergoes an ester exchange reaction with the polymer chain end group, promoting the chain growth reaction. It can add new monomer molecules to the polymer chain. In addition, the catalyst can replace the hydrogen atoms on the polymerization intermediate to form a transition state of a ring structure. The coordination effect of the ring strengthens the positive charge of the carbonyl carbon atom and the negative charge of the carbonyl oxygen atom, thereby accelerating the nucleophilic reaction between the groups, promoting the polymerization reaction, and improving the mechanical properties and physicochemical properties of the product.

[0026] After testing, the PBAT polyester obtained by polymerization using the catalyst of the present invention has a bright white color, L≥78, a≤3, b≤8, and a terminal carboxyl content of less than 30 mol / t; the mechanical properties of PBAT: tensile strength ≥30 MPa, elongation at break ≥600%. It can be seen that the catalyst provided by the present invention improves the product performance of the PBAT masterbatch and broadens the use conditions and application fields of PBAT. In addition, the catalyst provided by the present invention can reduce the carboxyl content and improve the hue during the polymerization of PBAT, which has important guiding significance for the industrial production and application of PBAT. DETAILED DESCRIPTION

[0027] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In view of the problem that in the prior art, tetrabutyl titanate is used as a catalyst in the PBAT polymerization process, which easily causes side reactions during the polymerization process, resulting in the PBAT polyester being yellow and red in color, having a high carboxyl value, and having poor mechanical properties, the present invention provides a catalyst prepared from titanium tetrachloride, ethanolamine and phosphate.

[0029] In the present invention, the titanium tetrachloride, ethanolamine and phosphate ester are all commercially available products. The phosphate ester is selected from any one or more of monoethyl phosphate, diethyl phosphate or triethyl phosphate.

[0030] The present invention also provides a method for preparing the above catalyst, comprising the following steps:

[0031] S1: mixing titanium tetrachloride with a solvent at 30-50° C. and activating the mixture to obtain a first precursor solution;

[0032] S2: mixing and reacting the first precursor solution with ethanolamine at 50-80° C. to obtain a second precursor solution;

[0033] S3: mixing the second precursor solution with the phosphoric acid ester at 60-80° C. and reacting to obtain a third precursor solution, ie, a catalyst.

[0034] According to the present invention, titanium tetrachloride is first mixed with a solvent at 30-50°C and activated to obtain a first precursor solution. The mixing is preferably carried out under stirring. In some embodiments of the present invention, titanium tetrachloride is preferably added to a solvent according to a mass ratio of titanium tetrachloride to solvent of 1:7-1:20, more preferably 1:8-1:18, and further preferably 1:10-1:15, and stirred and heated at 30-50°C for 1-2 h, preferably stirred and heated at 35-45°C for 1.5-2 h. In this process, the first precursor solution is fully activated. Wherein, the solvent is selected from any one or more of isopropanol, n-propanol, 1,4-butanediol or 1,3-butanediol, preferably 1,4-butanediol.

[0035] Then, according to the present invention, the first precursor solution is mixed and reacted with ethanolamine at 50-80°C to obtain a second precursor solution. In some embodiments of the present invention, preferably, the mass ratio of ethanolamine to solvent is 1:0.7-1:1.86, more preferably 1:0.8-1:1.8, and further preferably 1:1.0-1:1.5, ethanolamine is added to the first precursor solution, and stirred and heated at 50-80°C for 1-2 h, preferably at 60-70°C for 1.5-2 h, to form a homogeneous second precursor solution.

[0036] Then, according to the present invention, the second precursor solution is mixed and reacted with a phosphate at 60 to 80°C to obtain a third precursor solution. In some embodiments of the present invention, preferably, the mass ratio of the phosphate to the solvent is 1:0.46 to 1:1.5, more preferably 1:0.7 to 1:1.17, and further preferably 1:1, and the phosphate is added to the second precursor solution, and stirred and heated at 60 to 80°C for 6 to 10 h to form a homogeneous third precursor solution. Wherein, the specific selection of the phosphate is as described in the above technical solution, which will not be repeated here.

[0037] In some preferred embodiments of the present invention, after obtaining the third precursor solution, the following steps are further included:

[0038] The third precursor solution is allowed to stand at 30-40° C. for 24-48 hours, filtered, and a clear liquid is obtained to obtain a catalyst in the form of a transparent liquid.

[0039] In the present invention, the function of the above-mentioned standing is to remove floccules that may exist in the catalyst.

[0040] That is, in some embodiments of the present invention, the method for preparing the above catalyst comprises the following steps:

[0041] S1: mixing titanium tetrachloride with a solvent at 30-50° C. and activating the mixture to obtain a first precursor solution;

[0042] S2: mixing and reacting the first precursor solution with ethanolamine at 50-80° C. to obtain a second precursor solution;

[0043] S3: mixing and reacting the second precursor solution with the phosphate ester at 60-80° C. to obtain a third precursor solution.

[0044] S4: standing the third precursor solution at 30-40° C. for 24-48 hours, filtering, and preparing a catalyst.

[0045] The preparation method provided by the present invention has simple steps and is easy to implement, which is conducive to large-scale production or industrial production.

[0046] In the present invention, the catalyst obtained by the above preparation method is a transparent liquid. According to the test, the density of the catalyst is 1.2-1.7 g / mL, specifically 1.2 g / mL, 1.3 g / mL, 1.4 g / mL, 1.5 g / mL, 1.6 g / mL or 1.7 g / mL; the viscosity at 25°C is 96-130 mPa·s, specifically 96 mPa·s, 100 mPa·s, 105 mPa·s, 110 mPa·s, 115 mPa·s, 120 mPa·s, 125 mPa·s or 130 mPa·s, etc.

[0047] The point values ​​listed above are for illustrative purposes only and are not intended to be limiting. Other point values ​​within the numerical range may be applicable.

[0048] The present invention also provides an application of the catalyst in PBAT polymerization.

[0049] In the present invention, the preparation method of PBAT comprises the following steps:

[0050] The reactants (terephthalic acid, adipic acid and 1,4-butanediol) are added to a polyester reactor, and a catalyst is added, wherein the mass ratio of the catalyst to the reactants is (1-5):1000, preferably (2-4):1000, and the esterification reaction is carried out at 225°C for 3 hours to obtain an esterified product after the esterification is completed; the esterified product is reacted at a temperature of 225°C for 2 hours under a vacuum condition of 2 KPa; after the prepolymerization is completed, the esterified product is reacted at a temperature of 228°C for 4.5 hours under a vacuum condition of 100 Pa; after the reaction is completed, the PBAT melt is blown out with nitrogen, and pelletized using a pelletizer to obtain the obtained product.

[0051] It should be noted that the parameters such as temperature, time and pressure involved in the above method can also be adjusted accordingly within a reasonable range.

[0052] In the present invention, the hue (L value, a value and b value), terminal carboxyl group determination and mechanical properties of the obtained PBAT were measured. The results showed that the catalyst provided in the present invention can be used to efficiently prepare PBAT particles with bright white color and excellent mechanical properties.

[0053] After testing, the PBAT polyester prepared by the catalyst provided by the present invention has bright white color, L≥78, a≤3, b≤8, and a terminal carboxyl content of less than 30 mol / t; the mechanical properties of PBAT are: tensile strength ≥30 MPa, elongation at break ≥600%.

[0054] In summary, the catalyst provided by the present invention can provide active sites for the polymerization of reactants to prepare PBAT, reduce the initiation temperature of the reaction, wherein each active component can effectively increase the polarization of the carbonyl group, making it easier for the hydroxyl group to attack the carbonyl group nucleophilically, and chelate coordination occurs, and the hydroxyl hydrogen and carbonyl oxygen on the hydroxybutyl ester group in butylene terephthalate easily form intramolecular hydrogen bonds, thereby forming an internal cyclic complex. The catalyst can replace the hydrogen atom on the hydroxyl group to form a transition state of the ring structure, and the coordination effect of the ring structure strengthens the positive charge of the carbonyl carbon atom and the negative charge of the carbonyl oxygen atom, thereby accelerating the nucleophilic reaction between the groups, promoting the polymerization reaction, and inhibiting the occurrence of side reactions, thereby reducing the terminal carboxyl content and improving the color.

[0055] Therefore, the use of the catalyst of the present invention has important guiding significance for the industrial production and application of PBAT.

[0056] In order to further illustrate the present invention, the following examples are used to provide a detailed description. The experimental raw materials and reagents used in the following examples of the present invention were purchased from Sinopharm Group Co., Ltd. and were analytically pure.

[0057] Example 1

[0058] This embodiment provides a catalyst for polymerization of polybutylene terephthalate (PBAT), and the steps of the preparation method thereof are as follows:

[0059] (1) Add 4 g of titanium tetrachloride and 80 g of n-propanol into a three-necked flask (mass ratio is 1:20), heat and stir at 30°C for 2 h to prepare a first precursor solution;

[0060] (2) Add 50 g of ethanolamine to 84 g of the first precursor solution, heat and stir at 50 °C for 2 h to prepare a second precursor solution;

[0061] The mass ratio of ethanolamine to solvent n-propanol is 1:1.6;

[0062] (3) Add 80 g of monoethyl phosphate to 134 g of the second precursor solution, heat and stir at 60 °C for 8 h to prepare a third precursor solution;

[0063] The mass ratio of monoethyl phosphate to solvent n-propanol is 1:1;

[0064] (4) The third precursor solution was allowed to stand at 30° C. for 48 h, and a clear solution was obtained by filtration to prepare a homogeneous catalyst A;

[0065] The catalyst A in Example 1 is a transparent liquid with a density of 1.2 g / mL and a viscosity of 96 mPa·s at a temperature of 25°C.

[0066] Example 2

[0067] This embodiment provides a catalyst for polymerization of polybutylene terephthalate (PBAT), and the preparation method thereof has the following steps:

[0068] (1) Add 8 g of titanium tetrachloride and 60 g of isopropanol into a three-necked flask (mass ratio is 1:7.5), heat and stir at 50°C for 1 h to prepare a first precursor solution;

[0069] (2) Add 35 g of ethanolamine to 73 g of the first precursor solution, heat and stir at 80° C. for 1 h to prepare a second precursor solution;

[0070] The mass ratio of ethanolamine to solvent isopropanol is 1:1.71;

[0071] (3) Add 130 g of diethyl phosphate to 108 g of the second precursor solution, heat and stir at 80 °C for 6 h to prepare a third precursor solution;

[0072] The mass ratio of diethyl phosphate to solvent isopropanol is 1:0.46;

[0073] (4) The third precursor solution was allowed to stand at 40°C for 24 h, and a clear solution was obtained by filtration to prepare a homogeneous catalyst B;

[0074] The catalyst B in Example 2 is a transparent liquid with a density of 1.7 g / mL and a viscosity of 130 mPa·s at a temperature of 25°C.

[0075] Example 3

[0076] This embodiment provides a catalyst for polymerization of polybutylene terephthalate (PBAT), and the preparation method thereof has the following steps:

[0077] (1) Add 5 g of titanium tetrachloride and 90 g of 1,3-butanediol into a three-necked flask (mass ratio is 1:18), heat and stir at 40°C for 1.5 h to prepare a first precursor solution;

[0078] (2) Add 65 g of ethanolamine to 95 g of the first precursor solution, heat and stir at 60 °C for 1.5 h to prepare a second precursor solution;

[0079] The mass ratio of ethanolamine to solvent 1,3-butanediol is 1:1.38;

[0080] (3) Add 60 g of triethyl phosphate to 160 g of the second precursor solution, heat and stir at 70 °C for 7 h to prepare a third precursor solution.

[0081] The mass ratio of triethyl phosphate to solvent 1,3-butanediol is 1:1.5;

[0082] (4) The third precursor solution was allowed to stand at 35°C for 36 h, and a clear solution was obtained by filtration to prepare a homogeneous catalyst C;

[0083] The catalyst C in Example 3 is a transparent liquid with a density of 1.3 g / mL and a viscosity of 107 mPa·s at a temperature of 25°C.

[0084] Example 4

[0085] This embodiment provides a catalyst for polymerization of polybutylene terephthalate (PBAT), and the preparation method thereof has the following steps:

[0086] (1) Add 7 g of titanium tetrachloride and 49 g of 1,4-butanediol into a three-necked flask (mass ratio is 1:7), heat and stir at 35°C for 1.5 h to prepare a first precursor solution;

[0087] (2) Add 70 g of ethanolamine to 56 g of the first precursor solution, heat and stir at 70 °C for 1.5 h to prepare a second precursor solution;

[0088] The mass ratio of ethanolamine to solvent 1,4-butanediol is 1:0.7;

[0089] (3) Add 30 g of monoethyl phosphate and 40 g of diethyl phosphate to 126 g of the second precursor solution, heat and stir at 75 °C for 6 h to prepare a third precursor solution;

[0090] The mass ratio of monoethyl phosphate, diethyl phosphate and solvent 1,4-butanediol is 1:0.7;

[0091] (4) The third precursor solution was allowed to stand at 30°C for 40 h, and a clear solution was obtained by filtration to prepare a homogeneous catalyst D;

[0092] The catalyst D in Example 4 is a transparent liquid with a density of 1.6 g / mL and a viscosity of 121 mPa·s at a temperature of 25°C.

[0093] Example 5

[0094] This embodiment provides a catalyst for polymerization of polybutylene terephthalate (PBAT), and the preparation method thereof has the following steps:

[0095] (1) Add 6 g of titanium tetrachloride, 35 g of 1,4-butanediol and 35 g of 1,3-butanediol into a three-necked flask (mass ratio is 1:11.67), heat and stir at 45°C for 1 h to prepare a first precursor solution;

[0096] (2) Add 40 g of ethanolamine to 76 g of the first precursor solution, heat and stir at 65 °C for 1.2 h to prepare a second precursor solution;

[0097] The mass ratio of ethanolamine to solvent 1,4-butanediol and 1,3-butanediol is 1:1.75;

[0098] (3) Add 20 g of diethyl phosphate and 40 g of triethyl phosphate to 116 g of the second precursor solution, heat and stir at 65 °C for 7 h to prepare a third precursor solution;

[0099] The mass ratio of diethyl phosphate, triethyl phosphate and solvent 1,4-butanediol, 1,3-butanediol is 1:1.17.

[0100] (4) The third precursor solution was allowed to stand at 35° C. for 45 h, and a clear solution was obtained by filtration to prepare a homogeneous catalyst E;

[0101] The catalyst E in Example 5 is a transparent liquid with a density of 1.5 g / mL and a viscosity of 113 mPa·s at a temperature of 25°C.

[0102] The following application examples 1-5 are respectively used to prepare polybutylene terephthalate adipate (PBAT) using catalysts A-E obtained in the above examples 1-5. Among them, comparative application example 1-2 is used to prepare polybutylene terephthalate adipate (PBAT) using a traditional catalyst - tetrabutyl titanate.

[0103] Application Example 1

[0104] The raw materials of terephthalic acid, adipic acid and 1,4-butanediol were added to the polyester reactor, and catalyst A was added, wherein the mass ratio of catalyst to reactant was 3:1000. The esterification reaction was carried out at 225°C for 3 h, and the esterification product was obtained after the esterification was completed; the esterification product was reacted at 225°C for 2 h under the vacuum condition of 2 KPa; after the prepolymerization was completed, the temperature was reacted at 228°C for 4.5 h under the vacuum condition of 100 Pa; after the reaction was completed, the PBAT melt was blown out with nitrogen, and pelletized using a pelletizer.

[0105] Application Example 2

[0106] The raw materials of terephthalic acid, adipic acid and 1,4-butanediol were added to the polyester reactor, and catalyst B was added, wherein the mass ratio of catalyst to reactant was 1:1000. The esterification reaction was carried out at 225°C for 3 h, and the esterification product was obtained after the esterification was completed; the esterification product was reacted at 225°C for 2 h under the vacuum condition of 2 KPa; after the prepolymerization was completed, the temperature was reacted at 228°C for 3 h under the vacuum condition of 95 Pa; after the reaction was completed, the PBAT melt was blown out with nitrogen, and pelletized using a pelletizer.

[0107] Application Example 3

[0108] The raw materials of terephthalic acid, adipic acid and 1,4-butanediol were added to the polyester reactor, and catalyst C was added, wherein the mass ratio of catalyst to reactant was 2.5:1000. The esterification reaction was carried out at 225°C for 3 h, and the esterification product was obtained after the esterification was completed; the esterification product was reacted at 225°C for 2 h under the vacuum condition of 2 KPa; after the prepolymerization was completed, the temperature was reacted at 228°C for 4 h under the vacuum condition of 90 Pa; after the reaction was completed, the PBAT melt was blown out with nitrogen, and pelletized using a pelletizer.

[0109] Application Example 4

[0110] The raw materials of terephthalic acid, adipic acid and 1,4-butanediol were added to the polyester reactor, and catalyst D was added, wherein the mass ratio of catalyst to reactant was 2:1000. The esterification reaction was carried out at 225°C for 3 h, and the esterification product was obtained after the esterification was completed; the esterification product was reacted at 225°C for 2 h under the vacuum condition of 2 KPa; after the prepolymerization was completed, the temperature was reacted at 228°C for 3 h under the vacuum condition of 130 Pa; after the reaction was completed, the PBAT melt was blown out with nitrogen, and pelletized using a pelletizer.

[0111] Application Example 5

[0112] The raw materials of terephthalic acid, adipic acid and 1,4-butanediol were added to the polyester reactor, and catalyst E was added, wherein the mass ratio of catalyst to reactant was 1.5:1000. The esterification reaction was carried out at 225°C for 3 h, and the esterification product was obtained after the esterification was completed; the esterification product was reacted at 225°C for 2 h under the vacuum condition of 2 KPa; after the prepolymerization was completed, the temperature was reacted at 228°C for 3.5 h under the vacuum condition of 110 Pa; after the reaction was completed, the PBAT melt was blown out with nitrogen, and pelletized using a pelletizer.

[0113] Comparative application example 1

[0114] The raw materials of terephthalic acid, adipic acid and 1,4-butanediol were added to the polyester reactor, and tetrabutyl titanate was added, wherein the mass ratio of the catalyst to the reactant was 1:1000. The esterification reaction was carried out at 225°C for 3 hours, and the esterification was completed. The esterification was reacted at 225°C for 2 hours under the vacuum condition of 2 KPa; after the prepolymerization was completed, the temperature was reacted at 228°C for 4 hours under the vacuum condition of 120 Pa; after the reaction was completed, the PBAT melt was blown out with nitrogen, and the pelletizer was used to complete the pelletizing.

[0115] Comparative Application Example 2

[0116] The raw materials of terephthalic acid, adipic acid and 1,4-butanediol were added to the polyester reactor, and tetrabutyl titanate was added, wherein the mass ratio of the catalyst to the reactant was 0.5:1000. The esterification reaction was carried out at 225°C for 3 hours, and the esterification was completed. The esterification was reacted at 225°C for 2 hours under the vacuum condition of 2 KPa; after the prepolymerization was completed, the temperature was reacted at 228°C for 6 hours under the vacuum condition of 105 Pa; after the reaction was completed, the PBAT melt was blown out with nitrogen, and the pelletizer was used to complete the pelletizing.

[0117] Performance Testing

[0118] The test method is as follows:

[0119] The hue (L value, a value and b value) of PBAT was automatically measured using an automatic colorimeter (color35 model) from BYKGardner.

[0120] The following methods are used to test the terminal carboxyl groups and mechanical properties of PBAT:

[0121] Determination of terminal carboxyl groups: Weigh 0.5 g of PBAT, dissolve it in phenol-chloroform solution, and titrate it using a potentiometric titrator (Mettler T50) with a 0.01 mol / L potassium hydroxide-benzyl alcohol solution as the titrant.

[0122] Mechanical properties test: The tensile properties were determined using a universal mechanical testing machine (Instron 5960) at a tensile rate of 50 mm / min.

[0123] The test results are shown in Table 1 below, where the data L, a, and b values ​​correspond to the brightness, chromaticity, and hue of the PBAT color, respectively. L represents brightness, indicating the lightness or darkness of an object; a represents red-greenness, indicating the color bias of an object between red and green; b represents yellow-blueness, indicating the color bias of an object between yellow and blue, where the national standard (GB∕T 32366-2015) is L≥75, a≤5, and b≤10; the terminal carboxyl group represents the content of the terminal carboxyl group of the polyester molecular chain, and a high terminal carboxyl group value indicates that there are many side reactions during the polymerization of the product, and it is also easy to hydrolyze and degrade; the tensile strength represents the maximum tensile stress during the process of stretching the sample to break, reflecting the rigidity of the material; the elongation at break represents the percentage of the elongation of the original gauge length to the original gauge length after the sample is stretched to break, reflecting the toughness of the material:

[0124] Table 1

[0125]

[0126] It can be seen from the data in Table 1 that the catalysts AE prepared by the present invention can efficiently prepare PBAT particles with bright white color and excellent mechanical properties. Compared with the traditional PBAT polymerization using tetrabutyl titanate as a catalyst, under similar reaction conditions, although PBAT particles can also be prepared, the product has a high carboxyl value, many side reactions, the product is yellow and red, and the mechanical properties are poor. Therefore, the PBAT catalyst of the present invention has obvious advantages in product hue, terminal carboxyl value and mechanical properties compared to the traditional tetrabutyl titanate catalyst.

[0127] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a catalyst for PBAT polymerization, characterized in that: The following steps are involved: S1: mixing titanium tetrachloride with a solvent at 30-50° C. and activating the mixture to obtain a first precursor solution; The solvent is selected from any one or more of isopropanol, n-propanol, 1,4-butanediol or 1,3-butanediol; S2: mixing and reacting the first precursor solution with ethanolamine at 50-80° C. to obtain a second precursor solution; S3: mixing the second precursor solution with the phosphate ester at 60-80° C. and reacting to obtain a catalyst; The phosphate ester is selected from any one or more of monoethyl phosphate, diethyl phosphate or triethyl phosphate.

2. The preparation method according to claim 1, characterized in that: The solvent is selected from any one or more of isopropanol, n-propanol, 1,4-butanediol or 1,3-butanediol.

3. The preparation method according to claim 1, characterized in that: The mass ratio of titanium tetrachloride to solvent is 1:7 to 1:20; The mass ratio of the ethanolamine to the solvent is 1:0.7 to 1:1.86; The mass ratio of the phosphate ester to the solvent is 1:0.46 to 1:1.

5.

4. The preparation method according to claim 1, characterized in that: After the reaction in step S3 is completed, the following steps are also included: The obtained solution was allowed to stand at 30-40° C. for 24-48 h, and filtered to obtain a catalyst.

5. The catalyst prepared by the preparation method according to any one of claims 1 to 4, characterized in that: The catalyst is a transparent liquid, the density of the catalyst is 1.2-1.7 g / mL, and the viscosity at 25° C. is 96-130 mPa·s.

6. Use of the catalyst prepared by the preparation method according to any one of claims 1 to 4 in PBAT polymerization.

7. The use according to claim 6, characterized in that: The mass ratio of the catalyst to the reactant is (1-5):1000; The reactants include terephthalic acid, adipic acid, and 1,4-butanediol.

Citation Information

Patent Citations

  • Synthetic method and application for polydentate ligand chelating titanium catalyst used for polyester preparation

    CN102875786A

  • Degradable polyester synthesis catalyst as well as preparation method and application thereof

    CN114621426A