Carbon fiber composite material for new energy automobile battery pack tray

By using carbon fiber composite materials on the new energy vehicle battery pack tray, combining polyphenylene sulfide, carbon fiber and silicon carbide powder, and through hot pressing curing treatment, the stability and weight problems of the tray material in high temperature and corrosive environments are solved. It achieves high strength, low density and chemical resistance, meeting the lightweight needs of new energy vehicles.

CN118791872APending Publication Date: 2024-10-18Guangdong Yuhao New Materials Technology Research Institute
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411140792.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing new energy vehicle battery pack tray materials are prone to corrosion in high-temperature and corrosive environments. Anti-corrosion coatings are costly and have poor stability. The fixing technology relies on human adjustment. They are also heavy and have no thermal insulation function, which cannot meet the demand for lightweighting. .

Method used

Using carbon fiber composite materials, water-soluble phenolic resin is immersed in the mesh fiber layer, combined with polyphenylene sulfide, carbon fiber short fibers and silicon carbide powder to form a flame-retardant, thermally conductive, heat-resistant and tough material, suitable for injection molding processing, and Improve mechanical properties through hot press curing and cyclic densification treatment.

Benefits of technology

Realized the excellent performance of carbon fiber composite materials on new energy vehicle battery pack trays, including high strength, low density, chemical resistance and low warpage, suitable for high temperature and corrosive environments, and suitable for injection molding processing, improving the battery pack The stability and lightweight properties of the pallet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791872A_ABST
    Figure CN118791872A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon fiber composite material for a new energy automobile battery pack tray, and belongs to the technical field of carbon fiber composite materials. The material provided by the invention is suitable for a frame material for a battery of a new energy automobile, and particularly meets the requirements of a battery pack tray; according to the preparation method, the water-soluble phenolic resin solution is immersed into the reticular fiber layer, so that wool-like short carbon fibers are completely infiltrated, a good carbon fiber and resin bonding interface is formed, the heterogeneous bonding strength and density uniformity are improved, and the mechanical property of a finished product is improved; by using the polyphenylene sulfide, the short carbon fibers and the silicon carbide powder, the material has the characteristics of flame retardance, heat conduction, heat resistance, strong toughness, high strength, good chemical resistance and low warping degree, and is suitable for injection molding processing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of carbon fiber composite materials, and specifically refers to a carbon fiber composite material for a battery pack tray of a new energy vehicle. Background Art

[0002] The automobile industry is developing rapidly, but energy issues are becoming increasingly urgent, and the environmental problems caused by automobiles are also attracting much attention. Developing the new energy automobile industry is an effective way to alleviate the energy crisis, reduce greenhouse gas emissions, and reduce environmental pollution. At present, new energy vehicles have become an important direction for the transformation of the automobile industry. Unlike traditional vehicles, new energy vehicles use batteries as power to drive the vehicle. They are restricted by the weight of power batteries, the range of power batteries, and the high pressure of automobile energy conservation and emission reduction policies. As an indispensable part of the power battery production process, especially under the trend of domestic power battery production basically realizing automation and intelligence, pallets play a very critical role in improving production capacity, quality, and one-time pass rate. As an important component used in electric vehicles to support and fix the battery pack, the battery pack pallet has higher requirements for precision, high temperature, corrosion and other performance. Since the pallet is susceptible to corrosion in a humid and corrosive medium environment, a layer of anti-corrosion coating needs to be applied on the surface to isolate it from the external environment. However, the anti-corrosion coating has the problems of high raw material cost, complex process and poor coating stability, which is not conducive to the long-term use of the pallet. At the same time, the battery pack fixing technology in the prior art is limited to the mobile frame clamping and limiting the two ends of the battery pack, which requires manual adjustment and control, and has poor stability when encountering external impact.

[0003] At present, the chassis of new energy vehicles around the world all adopt the following structural types: steel structure, aluminum alloy structure or aluminum-magnesium alloy structure. Under the premise of ensuring strength, the requirements for lightweighting of the whole vehicle are constantly increasing, which cannot meet the market demand. Taking the battery pack tray with aluminum alloy structure as an example, all new energy battery packs use a combination of aluminum alloy tray CNC processing and engineering plastic injection molding battery cover. The battery pack cover is not only heavy but also does not have thermal insulation function. Carbon fiber composite materials have the advantages of low density, high specific modulus, high specific strength, high temperature resistance, corrosion resistance, and small thermal expansion coefficient. Therefore, the present invention provides a carbon fiber composite material for a new energy vehicle battery pack tray. Summary of the invention

[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a carbon fiber composite material for a new energy vehicle battery pack pallet. The material provided by the present invention is suitable for the frame material for new energy vehicle batteries, especially the requirements of the battery pack pallet; the present invention allows the water-soluble phenolic resin solution to be immersed in the mesh fiber layer, thereby completely infiltrating the hairy carbon fiber staple fibers, forming a good carbon fiber and resin bonding interface, improving the heterogeneous bonding strength and density uniformity, and improving the mechanical properties of the finished product; the present invention uses polyphenylene sulfide, carbon fiber staple fibers, and silicon carbide powder, so that it has the characteristics of flame retardancy, thermal conductivity, heat resistance, strong toughness, high strength, good chemical resistance, low warping, and is suitable for injection molding.

[0005] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows: a carbon fiber composite material for a new energy vehicle battery pack tray, the carbon fiber composite material comprising the following components in parts by weight: 50-100 parts of polyphenylene sulfide, 20-80 parts of carbon fiber staple fibers, 10-50 parts of silicon carbide powder, 1-20 parts of dispersant, 1-15 parts of water-soluble phenolic resin, and 1-20 parts of defoaming agent.

[0006] Preferably, the carbon fiber composite material comprises the following components in parts by weight: 50-80 parts of polyphenylene sulfide, 20-50 parts of carbon fiber staple fibers, 12-40 parts of silicon carbide powder, 2-10 parts of dispersant, 2-10 parts of water-soluble phenolic resin, and 3-15 parts of defoaming agent.

[0007] Preferably, the carbon fiber composite material comprises the following components in parts by weight: 50-70 parts of polyphenylene sulfide, 20-30 parts of carbon fiber staple fibers, 12-16 parts of silicon carbide powder, 2-8 parts of dispersant, 3-9 parts of water-soluble phenolic resin, and 4-10 parts of defoaming agent.

[0008] Furthermore, the silicon carbide powder can be replaced by graphite powder or carbon powder.

[0009] Furthermore, the dispersant is one or more of hydroxypropyl methylcellulose, hydroxyethyl methylcellulose, and polyethylene glycol.

[0010] Furthermore, the degassing agent is one of BYK-066N and BYK-054 degassing agents or a mixture of both.

[0011] Furthermore, the defoaming agent is a polymer defoaming agent, and the defoaming agent does not contain silicone.

[0012] The present invention also provides a method for preparing a carbon fiber composite material for a new energy vehicle battery pack tray, the preparation method comprising the following steps:

[0013] (1) dispersing polyphenylene sulfide, carbon fiber staple fibers, silicon carbide powder and a dispersant in water to form a fiber composite dispersion;

[0014] (2) providing a preset trough-shaped container with a suction hole and a filter screen formed at the bottom, and pouring the fiber composite dispersion into the inner cavity of the preset trough-shaped container, and filtering through the suction hole to form a mesh fiber layer in the preset trough-shaped container;

[0015] (3) applying a water-soluble phenolic resin to the mesh fiber layer in step (2), filtering, and drying to obtain a fiber prepreg sheet;

[0016] (4) The fiber prepreg sheets are stacked and bonded, and after hot pressing curing, carbonization and cyclic densification treatment, high-temperature purification and machining are performed to obtain the carbon fiber composite material.

[0017] Furthermore, the pressure of hot pressing curing in step (4) is 10-12 MPa.

[0018] Furthermore, the purification temperature of the high-temperature purification treatment in step (4) is 1800-2400°C.

[0019] The beneficial effects achieved by the present invention using the above structure are as follows: (1) The material provided by the present invention is suitable for frame materials for new energy vehicle batteries, especially the requirements of battery pack trays; (2) The present invention allows the water-soluble phenolic resin solution to penetrate into the mesh fiber layer, thereby completely soaking the hairy carbon fiber staple fibers, forming a good carbon fiber and resin bonding interface, improving heterogeneous bonding strength and density uniformity, and improving the mechanical properties of the finished product; (3) The present invention uses polyphenylene sulfide, carbon fiber staple fibers, and silicon carbide powder, so that it has the characteristics of flame retardancy, thermal conductivity, heat resistance, strong toughness, high strength, good chemical resistance, low warpage, and is suitable for injection molding processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Residual mass rate of carbon fiber composite materials.

[0021] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0024] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials and test strains used in the following examples are purchased from commercial channels unless otherwise specified.

[0025] Example 1

[0026] A carbon fiber composite material for new energy vehicle battery pack tray

[0027] The carbon fiber composite material comprises the following components in parts by weight: 50 parts of polyphenylene sulfide, 20 parts of carbon fiber staple fibers, 12 parts of silicon carbide powder, 2 parts of dispersant, 3 parts of water-soluble phenolic resin, and 4 parts of defoaming agent.

[0028] Wherein, the silicon carbide powder can be replaced by graphite powder or carbon powder.

[0029] Wherein, the dispersant is one or more of hydroxypropyl methylcellulose, hydroxyethyl methylcellulose and polyethylene glycol.

[0030] The degassing agent is one of BYK-066N and BYK-054 degassing agents or a mixture of both.

[0031] Wherein, the defoaming agent is a polymer defoaming agent, and the defoaming agent does not contain silicone.

[0032] The present invention also provides a method for preparing a carbon fiber composite material for a new energy vehicle battery pack tray, the preparation method comprising the following steps:

[0033] (1) dispersing polyphenylene sulfide, carbon fiber staple fibers, silicon carbide powder and a dispersant in water to form a fiber composite dispersion;

[0034] (2) providing a preset trough-shaped container with a suction hole and a filter screen formed at the bottom, and pouring the fiber composite dispersion into the inner cavity of the preset trough-shaped container, and filtering through the suction hole to form a mesh fiber layer in the preset trough-shaped container;

[0035] (3) applying a water-soluble phenolic resin to the mesh fiber layer in step (2), filtering, and drying to obtain a fiber prepreg sheet;

[0036] (4) The fiber prepreg sheets are stacked and bonded, and after hot pressing curing, carbonization and cyclic densification treatment, high-temperature purification and machining are performed to obtain the carbon fiber composite material.

[0037] Wherein, the pressure of hot pressing curing in step (4) is 10-12 MPa.

[0038] Wherein, the purification temperature of the high-temperature purification treatment in step (4) is 1800-2400°C.

[0039] Example 2

[0040] A carbon fiber composite material for new energy vehicle battery pack tray

[0041] The carbon fiber composite material includes the following components in parts by weight: 60 parts of polyphenylene sulfide, 25 parts of carbon fiber staple fibers, 14 parts of silicon carbide powder, 6 parts of dispersant, 6 parts of water-soluble phenolic resin, and 7 parts of defoaming agent.

[0042] Wherein, the silicon carbide powder can be replaced by graphite powder or carbon powder.

[0043] Wherein, the dispersant is one or more of hydroxypropyl methylcellulose, hydroxyethyl methylcellulose and polyethylene glycol.

[0044] The degassing agent is one of BYK-066N and BYK-054 degassing agents or a mixture of both.

[0045] Wherein, the defoaming agent is a polymer defoaming agent, and the defoaming agent does not contain silicone.

[0046] The present invention also provides a method for preparing a carbon fiber composite material for a new energy vehicle battery pack tray, and the preparation method is implemented with reference to Example 1.

[0047] Example 3

[0048] A carbon fiber composite material for new energy vehicle battery pack tray

[0049] The carbon fiber composite material comprises the following components in parts by weight: 70 parts of polyphenylene sulfide, 30 parts of carbon fiber staple fibers, 16 parts of silicon carbide powder, 8 parts of dispersant, 9 parts of water-soluble phenolic resin, and 10 parts of defoaming agent.

[0050] Wherein, the silicon carbide powder can be replaced by graphite powder or carbon powder.

[0051] Wherein, the dispersant is one or more of hydroxypropyl methylcellulose, hydroxyethyl methylcellulose and polyethylene glycol.

[0052] The degassing agent is one of BYK-066N and BYK-054 degassing agents or a mixture of both.

[0053] Wherein, the defoaming agent is a polymer defoaming agent, and the defoaming agent does not contain silicone.

[0054] The present invention also provides a method for preparing a carbon fiber composite material for a new energy vehicle battery pack tray, and the preparation method is implemented with reference to Example 1.

[0055] Experimental Example 1

[0056] Thermal stability test of carbon fiber composite material for new energy vehicle battery pack tray

[0057] The carbon fiber composite materials prepared in Example 1, Example 2 and Example 3 were crushed to obtain powder samples (100 mesh). 5-6 mg of the sample was placed in a crucible for thermogravimetric analysis (TG209F3). Test conditions: N2 atmosphere, gas flow rate 40 mL / min, heating rate 20°C / min, heating range 35-800°C.

[0058] like Figure 1 As shown, when the temperature is 600° C., the mass residual rates of the carbon fiber composite materials of Example 1, Example 2 and Example 3 are all at a relatively high level, among which the mass residual rate of Example 3 is the highest.

[0059] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0060] The present invention and its embodiments are described above, and such description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design a structure and embodiment similar to the technical solution without creativity, which should belong to the protection scope of the present invention.

Claims

1. A carbon fiber composite material for a new energy vehicle battery pack tray, characterized in that: The carbon fiber composite material comprises the following components in parts by weight: 50-100 parts of polyphenylene sulfide, 20-80 parts of carbon fiber staple fibers, 10-50 parts of silicon carbide powder, 1-20 parts of a dispersant, 1-15 parts of a water-soluble phenolic resin, and 1-20 parts of a defoaming agent.

2. The carbon fiber composite material for a new energy vehicle battery pack tray according to claim 1, characterized in that: The carbon fiber composite material comprises the following components in parts by weight: 50-80 parts of polyphenylene sulfide, 20-50 parts of carbon fiber staple fibers, 12-40 parts of silicon carbide powder, 2-10 parts of a dispersant, 2-10 parts of a water-soluble phenolic resin, and 3-15 parts of a defoaming agent.

3. The carbon fiber composite material for a new energy vehicle battery pack tray according to claim 2, characterized in that: The carbon fiber composite material comprises the following components in parts by weight: 50-70 parts of polyphenylene sulfide, 20-30 parts of carbon fiber staple fibers, 12-16 parts of silicon carbide powder, 2-8 parts of dispersant, 3-9 parts of water-soluble phenolic resin, and 4-10 parts of defoaming agent.

4. The carbon fiber composite material for a new energy vehicle battery pack tray according to claim 3, characterized in that: The silicon carbide powder may be replaced by graphite powder or carbon powder.

5. The carbon fiber composite material for a new energy vehicle battery pack tray according to claim 4, characterized in that: The dispersant is one or more of hydroxypropyl methylcellulose, hydroxyethyl methylcellulose and polyethylene glycol.

6. The carbon fiber composite material for a new energy vehicle battery pack tray according to claim 5, characterized in that: The degassing agent is one of BYK-066N and BYK-054 degassing agents or a mixture of both.

7. The carbon fiber composite material for a new energy vehicle battery pack tray according to claim 6, characterized in that: The defoaming agent is a polymer defoaming agent and does not contain silicone.

8. A method for preparing a carbon fiber composite material for a new energy vehicle battery pack tray according to claim 7, characterized in that: The preparation method comprises the following steps: (1) dispersing polyphenylene sulfide, carbon fiber staple fibers, silicon carbide powder and a dispersant in water to form a fiber composite dispersion; (2) providing a preset trough-shaped container with a suction hole and a filter screen formed at the bottom, and pouring the fiber composite dispersion into the inner cavity of the preset trough-shaped container, and filtering through the suction hole to form a mesh fiber layer in the preset trough-shaped container; (3) applying a water-soluble phenolic resin to the mesh fiber layer in step (2), filtering, and drying to obtain a fiber prepreg sheet; (4) The fiber prepreg sheets are stacked and bonded, and after hot pressing curing, carbonization and cyclic densification treatment, high-temperature purification and machining are performed to obtain the carbon fiber composite material.

9. The method for preparing a carbon fiber composite material for a new energy vehicle battery pack tray according to claim 8, characterized in that: The pressure of the hot pressing curing in step (4) is 10-12 MPa.

10. The method for preparing a carbon fiber composite material for a new energy vehicle battery pack tray according to claim 9, characterized in that: The purification temperature of the high-temperature purification treatment in step (4) is 1800-2400°C.