Preparation method of novel organic-inorganic hybrid self-repairing anticorrosive paint

By introducing the Schiff base/epoxy resin self-healing bottom layer and the Ti4O7/epoxy resin outer layer into the epoxy coating, the self-healing performance is used to solve the problem of reduced corrosion resistance caused by micropores and damage in the coating, achieving a better High corrosion resistance and service life, suitable for offshore wind power corrosion protection.

CN118791933APending Publication Date: 2024-10-18GUANGXI UNIV

Patent Information

Application Number
CN202410855073.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing epoxy coatings form micropores during the curing process, leading to the penetration of corrosive electrolytes, reducing the corrosion resistance and service life of the coating, and inevitable damage and cracks weaken the corrosion resistance of the coating.

Method used

Using a layered painting method, the Schiff base/epoxy resin self-healing bottom layer and the Ti4O7/epoxy resin outer layer are first painted on the tinplate. The self-healing material is prepared by imine exchange reaction to form a Schiff base/Ti4O7/EP double-layer self-healing coating, and the self-healing performance is used to improve the corrosion resistance of the coating.

Benefits of technology

It significantly improves the corrosion resistance and service life of the coating, avoids the failure of the coating due to damage, enhances the protective effect, and simplifies the coating preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791933A_ABST
    Figure CN118791933A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a novel organic-inorganic hybrid self-repairing anticorrosive coating. The method comprises the following steps: 1) polishing and washing a tinplate base material; 2) heating, condensing and refluxing terephthalaldehyde, triethylene tetramine and polyether amine D-230 under the protection of inert gas to obtain a reversible Schiff base chain segment, and then heating, stirring and mixing the reversible Schiff base chain segment, epoxy resin and methyl tetrahydrophthalic anhydride to obtain a Schiff base / epoxy resin self-repairing material; (3) uniformly brushing the self-repairing material in the step (2) on a base material by using a wire coating rod, and curing to obtain the base material coated with a Schiff base / epoxy resin self-repairing bottom layer; and 4) uniformly dispersing dopamine-modified Ti4O7 in epoxy resin, coating the base material in the step 3) with a wire coating rod, and curing to obtain the novel organic-inorganic hybrid self-repairing anticorrosive coating. The method is simple in process, and the obtained coating has self-repairing capacity and good corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal material surface treatment, and specifically is a method for preparing a novel organic-inorganic hybrid self-repairing anti-corrosion coating. Background Art

[0002] Metal corrosion is a common phenomenon that affects all areas of production and life. It leads to structural damage, material function failure, massive waste of resources and huge economic losses. For decades, various anti-corrosion methods have been used, including anti-corrosion coatings, corrosion inhibitors, alloy treatments and cathodic protection. Among them, organic coatings are the most convenient and effective technology to protect metal materials from corrosion because they are easy to apply and have significant physical shielding properties that can separate corrosive media from metal substrates and prevent the penetration of corrosive media. Epoxy coatings, in particular, are widely used in industrial applications due to their excellent mechanical properties, high bonding strength, good heat resistance and relatively low cost. However, during curing, solvent evaporation leads to the formation of micropores, which are the entrances for corrosive electrolytes to penetrate into the coating matrix, resulting in reduced hardness and anti-corrosion efficiency.

[0003] Previous studies have shown that adding nanofillers to epoxy resin can effectively fill defects such as micropores in the coating, extend the diffusion path of the corrosive medium, and significantly improve the corrosion resistance of the epoxy resin coating. However, in actual use, the coating will inevitably be damaged and cracked, which greatly weakens the corrosion resistance and service life of the coating. Inspired by the timely self-repair of natural organisms after damage and breakage, the introduction of self-healing properties in corrosion-resistant coatings can reduce corrosion caused by coating damage, greatly improve the life and stability of the coating, and reduce the maintenance cost of the coating. In recent years, with the increasing demand for long-term protection capabilities, self-healing coatings have become one of the hot research topics in the field of metal corrosion protection. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a preparation method of a novel organic-inorganic hybrid self-healing anti-corrosion coating. The preparation process of the method is simple. The coating is applied in layers, and a Schiff base / epoxy resin self-healing bottom layer and a Ti4O7 / epoxy resin outer layer are successively applied on tinplate with a wire coating rod, and finally a Schiff base / Ti4O7 / EP double-layer self-healing coating with self-healing ability and good corrosion resistance is obtained.

[0005] The present invention solves the above technical problems with the following technical solutions: The present invention provides a method for preparing a novel organic-inorganic hybrid self-repairing anti-corrosion coating, comprising the following steps: 1) Substrate pretreatment: Tinplate is selected as the substrate, and the surface of the tinplate is polished and washed to obtain a continuous, smooth and relatively rough substrate surface; 2) Preparation of Schiff base / epoxy resin self-healing material: terephthalaldehyde, triethylenetetramine and polyetheramine D-230 are heated and condensed under inert gas protection to obtain a reversible Schiff base segment, wherein terephthalaldehyde, triethylenetetramine and polyetheramine D-230 are configured in a molar ratio of 10:3:17. Subsequently, the reversible Schiff base segment, epoxy resin and methyltetrahydrophthalic anhydride are heated and stirred to obtain a Schiff base / epoxy resin self-healing material; 3) Preparation of Schiff base / epoxy resin self-healing bottom layer: The self-healing material of step 2) is evenly applied on the tinplate substrate using a wire coating rod, and then heat-cured in sections in an oven. The operation of the section heat-curing is: first, treat at 80 °C for 2 h, then treat at 90 °C for 12 h, and finally obtain a tinplate substrate with a Schiff base / epoxy resin self-healing bottom layer formed on the surface; 4) Preparation of Ti4O7 / epoxy resin outer coating: The dopamine-modified Ti4O7 was uniformly dispersed in the epoxy resin by ultrasound, and the Ti4O7 / epoxy resin coating was coated on the tinplate substrate in step 3) using a wire coating rod, and then placed in an oven and heated to 80 °C for curing for 1 h to obtain a Schiff base / Ti4O7 / EP double-layer self-healing coating for offshore wind power corrosion protection.

[0006] In the invention, in step 1) and step 4), the Schiff base / Ti4O7 / EP double-layer self-healing coating contains a Schiff base / epoxy resin self-healing bottom layer and a Ti4O7 / epoxy resin outer layer coating. In the preparation of the Schiff base / epoxy resin self-healing bottom layer, the molar ratio of terephthalaldehyde, triethylenetetramine and polyetheramine D-230 is 10:3:17; in the Ti4O7 / epoxy resin outer layer coating, the mass ratio of dopamine-modified Ti4O7 and epoxy resin is 1:50.

[0007] In step 2) of the present invention, the inert gas is high-purity argon.

[0008] In step 1) of the present invention, the size of the tinplate substrate is 150 mm×70 mm×0.28 mm.

[0009] In step 1) of the present invention, the grinding in the substrate pretreatment is performed using 600-mesh and 1000-mesh sandpapers in sequence.

[0010] The method of the present invention is to sequentially apply a Schiff base / epoxy resin self-repairing bottom layer and a Ti4O7 / epoxy resin outer layer on the tinplate surface to finally obtain a Schiff base / Ti4O7 / EP double-layer self-repairing coating. The method of the present invention has the following beneficial effects: 1) The present invention obtains a Schiff base segment with self-repairing properties through an imine exchange reaction of terephthalaldehyde, triethylenetetramine and polyetheramine D-230, which effectively solves the problem of coating failure due to damage.

[0011] 2) The present invention adopts a layered coating method when preparing the Schiff base / Ti4O7 / EP double-layer self-healing coating. The Schiff base / epoxy resin self-healing bottom layer and the Ti4O7 / epoxy resin outer layer are successively coated on the tinplate using a wire coating rod. The layered coating can improve the hydrophobicity of the coating, thereby improving the corrosion resistance of the coating.

[0012] 3) In the method of the present invention, a Schiff base segment with self-healing properties is prepared by an imine exchange reaction of terephthalaldehyde, triethylenetetramine and polyetheramine D-230. The Schiff base self-healing response conditions are simple, and no thermal or optical excitation is required. The recombination of the imine bond can be achieved in the presence of water. Moreover, the Schiff base can form a metal coordination bond with the metal, and hydrogen bonds can also be formed between the Schiff bases, which provides a basis for the construction of double network self-healing materials.

[0013] 4) The method of the present invention improves the overall protective effect of the coating and avoids the problem of coating failure caused by coating damage to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 This is a surface scanning electron microscope image of the artificially damaged Schiff base / Ti4O7 / EP double-layer self-healing coating in Example 1 of the present invention, which achieves bottom layer healing under water stimulation.

[0015] Figure 2 This is the impedance spectrum of the Schiff base / Ti4O7 / EP double-layer self-healing coating sample in Example 1 of the present invention. DETAILED DESCRIPTION

[0016] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings.

[0017] The preparation method of the Schiff base / Ti4O7 / EP double-layer self-repairing coating for offshore wind power corrosion protection of the present invention has the following specific operating steps: 1) Substrate pretreatment: Use tinplate as the substrate, and pre-treat the tinplate surface by grinding, washing, etc.

[0018] The tinplate is a sheet with a size of length×width×height=150 mm×70 mm×0.28 mm.

[0019] During the polishing treatment, the substrate can be polished with 600-mesh and 1000-mesh sandpapers in sequence to obtain a continuously flat and rough substrate surface, so as to improve the bonding strength between the substrate and the coating in the subsequent curing process.

[0020] Preparation of Schiff base / epoxy resin self-healing material: Add terephthalaldehyde to a three-necked flask containing molecular sieves, add methanol (solvent), slowly add polyetheramine D-230 and tetraethylenetriamine while stirring, raise the temperature to 60 °C under condensation reflux under the protection of dry inert gas, and react with magnetic stirring for 3 h to obtain a reversible Schiff base segment, wherein terephthalaldehyde, triethylenetetramine and polyetheramine D-230 are configured in a molar ratio of 10:3:17. Subsequently, the reversible Schiff base segment, epoxy resin and methyltetrahydrophthalic anhydride are heated and stirred to obtain a Schiff base / epoxy resin self-healing material.

[0021] The present invention realizes the recombination of imine bonds under the stimulation of water through the imine exchange reaction of terephthalaldehyde, triethylenetetramine and polyetheramine D-230, thereby achieving the effect of self-repair of the coating after being damaged.

[0022] 3) Preparation of Schiff base / epoxy resin self-healing bottom layer: The Schiff base / epoxy resin self-healing material is evenly applied on the tinplate substrate using a wire coating rod, and then heat-cured in sections in an oven. The operation of the section heat-curing is: first, treat at 80 °C for 2 h, then treat at 90 °C for 12 h, and finally obtain a tinplate substrate with a Schiff base / epoxy resin self-healing bottom layer formed on the surface; After the heat curing is completed, the sample is taken out, and the tinplate surface has obtained the Schiff base / epoxy resin self-healing bottom layer.

[0023] 4) Preparation of Ti4O7 / epoxy resin outer coating: Dopamine-modified Ti4O7 was dissolved in a mixed solution of n-butanol and N-methyl-2-pyrrolidone, and the mixed solution was ultrasonicated at 45 °C for 30 min. Subsequently, epoxy resin and 2-ethyl-4-methylimidazole curing agent were added, and ethyl acetate and dibutyl phthalate were added dropwise. The mixed solution was ultrasonically stirred at 70 °C for 40 min, and then the coating was evenly coated on the tinplate substrate with Schiff base / epoxy resin self-healing bottom layer with a metal wire coating rod, and then placed in an oven and heated to 80 °C for curing for 1 h, and the Schiff base / Ti4O7 / EP double-layer self-healing coating for offshore wind power corrosion protection was obtained.

[0024] The coating system is composed of a mixture of dopamine-modified Ti4O7 and epoxy resin in a mass ratio of 1:50.

[0025] The process of dopamine-modified Ti4O7 in the reaction is as follows: First, Ti4O7 is added to a Tris buffer solution (0.01 mol / L, pH = 8.5) and continuously ultrasonicated for 45 min to obtain a uniformly dispersed Ti4O7 dispersant. After that, dopamine hydrochloride is added to the above dispersant, and then the mixed solution is vigorously stirred at 30 °C for 24 h. After the reaction is completed, the mixed solution is centrifuged at 8000 rpm for 5 min, and the precipitate is taken. The precipitate is repeatedly washed several times with deionized water and anhydrous ethanol to remove impurities. Finally, the solid product is vacuum dried in an oven at 65 °C for 12 h to obtain dopamine-modified Ti4O7 powder.

[0026] The method of the present invention obtains a reversible Schiff base segment through an imine exchange reaction of terephthalaldehyde, triethylenetetramine and polyetheramine D-230. Subsequently, the reversible Schiff base segment, epoxy resin and methyltetrahydrophthalic anhydride are heated, stirred and mixed to obtain a Schiff base / epoxy resin self-healing material. It is applied on a tinplate substrate to obtain a Schiff base / epoxy resin self-healing bottom layer. Dopamine-modified Ti4O7 is uniformly dispersed in the epoxy resin by ultrasound, and then the Ti4O7 / epoxy resin coating is applied on the tinplate substrate with the Schiff base / epoxy resin self-healing bottom layer with a wire coating rod, and then a Schiff base / Ti4O7 / EP double-layer self-healing coating with self-healing ability and good corrosion resistance is finally obtained by heating and curing, which provides a new preparation method for preparing an anti-corrosion coating with self-healing performance, and the method is simple to operate.

[0027] Example 1 Commercially available tinplate was used as the experimental substrate. The size of the tinplate in the experiment was length × width × height = 150 mm × 70 mm × 0.28 mm. The element content of the tinplate is shown in Table 1. First, the tinplate was polished with 600 mesh and 1000 mesh sandpaper in turn, and a continuous flat and rough substrate surface was obtained after rinsing with deionized water and ethanol. Subsequently, the Schiff base / epoxy resin self-healing material was prepared. Terephthalaldehyde was added to a three-necked flask containing molecular sieves, methanol (solvent) was added, and polyetheramine D-230 and tetraethylenetriamine were slowly added while stirring. Under the protection of dry argon, the temperature was raised to 60 ° C under condensation reflux, and the magnetic stirring reaction was carried out for 3 h to obtain a reversible Schiff base segment, in which terephthalaldehyde, triethylenetetramine and polyetheramine D-230 were configured in a molar ratio of 10:3:17. Subsequently, the reversible Schiff base segment, epoxy resin and methyltetrahydrophthalic anhydride were heated and stirred to obtain the Schiff base / epoxy resin self-healing material. Subsequently, the Schiff base / epoxy resin self-healing material was evenly coated on the tinplate substrate using a wire coating rod, and then thermally cured in sections in an oven. The operation of the thermal curing section was: first treated at 80 °C for 2 h, then treated at 90 °C for 12 h, and finally a tinplate substrate with a Schiff base / epoxy resin self-healing bottom layer formed on the surface was obtained. Ti4O7 was added to a Tris buffer solution (0.01 mol / L, pH = 8.5) and continuously ultrasonically treated for 45 min to obtain a uniformly dispersed Ti4O7 dispersant. After that, dopamine hydrochloride was added to the above dispersant, and the mixed solution was vigorously stirred at 30 °C for 24 h. After the reaction was completed, the mixed solution was centrifuged at 8000 rpm for 5 min to obtain the precipitate. The precipitate was repeatedly washed several times with deionized water and anhydrous ethanol to remove impurities. Finally, the solid product was vacuum dried in an oven at 65 °C for 12 h to obtain dopamine-modified Ti4O7 powder. The dopamine-modified Ti4O7 was dissolved in a mixed solution of n-butanol and N-methyl-2-pyrrolidone, and then the mixed solution was ultrasonicated at 45 °C for 30 min. Subsequently, epoxy resin and 2-ethyl-4-methylimidazole curing agent were added, and ethyl acetate and dibutyl phthalate were added dropwise. Among them, the mass ratio of dopamine-modified Ti4O7 to epoxy resin was 1:50. The mixed solution was ultrasonically stirred at 70 °C for 40 min, and then the coating was evenly coated on the tinplate substrate with Schiff base / epoxy resin self-healing bottom layer with a metal wire coating rod, and then placed in an oven and heated to 80 °C for curing for 1 h, and the Schiff base / Ti4O7 / EP double-layer self-healing coating for offshore wind power corrosion protection was obtained.

[0028] In order to show the self-healing effect of the prepared Schiff base / Ti4O7 / EP double-layer self-healing coating, a sample with the Schiff base / Ti4O7 / EP double-layer self-healing coating was scratched with a scalpel, and its surface morphology was observed using a scanning electron microscope. The results are as follows: Figure 1 As shown, repair healing of the bottom coating can be observed on the tinplate surface. Figure 2 The electrochemical impedance spectrum of the Schiff base / Ti4O7 / EP double-layer self-healing coating sample after long-term immersion in 3.5 wt.% NaCl solution is shown.

[0029] Table 1 element C Mn P S Fe Content (wt.%) 0.032 0.208 1.442 0.962 Bal. Through the method of the present invention, the imine exchange reaction of terephthalaldehyde, triethylenetetramine and polyetheramine D-230 can be used on the surface of tinplate to achieve self-repair of the damaged coating under the stimulation of water, providing an additional option for the preparation method of offshore wind power corrosion protection coating, and the coating preparation method is simple and has good protection effect.

Claims

1. A method for preparing a novel organic-inorganic hybrid self-repairing anti-corrosion coating. It is characterized by: The steps include: 1) Substrate pretreatment: Tinplate is selected as the substrate, and the surface of the tinplate is polished and washed to obtain a continuous, smooth and rough substrate surface; 2) Preparation of Schiff base / epoxy resin self-healing material: terephthalaldehyde, triethylenetetramine and polyetheramine D-230 are heated and condensed under inert gas protection to obtain a reversible Schiff base segment, wherein terephthalaldehyde, triethylenetetramine and polyetheramine D-230 are configured in a molar ratio of 10:3:

17. Subsequently, the reversible Schiff base segment, epoxy resin and methyltetrahydrophthalic anhydride are heated and stirred to obtain a Schiff base / epoxy resin self-healing material; 3) Preparation of Schiff base / epoxy resin self-healing bottom layer: The self-healing material of step 2) is evenly applied on the tinplate substrate using a wire coating rod, and then heat-cured in sections in an oven. The operation of the section heat-curing is: first, treat at 80 °C for 2 h, then treat at 90 °C for 12 h, and finally obtain a tinplate substrate with a Schiff base / epoxy resin self-healing bottom layer formed on the surface; 4) Preparation of Ti4O7 / epoxy resin outer coating: The dopamine-modified Ti4O7 was uniformly dispersed in the epoxy resin by ultrasound, and the Ti4O7 / epoxy resin coating was coated on the tinplate substrate in step 3) using a wire coating rod, and then placed in an oven and heated to 80 °C for curing for 1 h to obtain a Schiff base / Ti4O7 / EP double-layer self-healing coating for offshore wind power corrosion protection.

2. The method for preparing a novel organic-inorganic hybrid self-repairing anti-corrosion coating according to claim 1, characterized in that: In step 1) and step 4), the Schiff base / Ti4O7 / EP double-layer self-healing coating contains a Schiff base / epoxy resin self-healing bottom layer and a Ti4O7 / epoxy resin outer layer coating. In the preparation of the Schiff base / epoxy resin self-healing bottom layer, the molar ratio of terephthalaldehyde, triethylenetetramine and polyetheramine D-230 is 10:3:17; in the Ti4O7 / epoxy resin outer layer coating, the mass ratio of dopamine-modified Ti4O7 and epoxy resin is 1:

50.

3. The method for preparing a novel organic-inorganic hybrid self-repairing anti-corrosion coating according to claim 1, characterized in that: In step 2), the inert gas is high-purity argon.

4. The method for preparing a novel organic-inorganic hybrid self-repairing anti-corrosion coating according to claim 1, characterized in that: In step 1), the size of the tinplate substrate is 150 mm×70 mm×0.28 mm.

5. The method for preparing a novel organic-inorganic hybrid self-repairing anti-corrosion coating according to claim 1, characterized in that: In step 1), the polishing in the substrate pretreatment is performed using 600-mesh and 1000-mesh sandpapers respectively.

Citation Information

Patent Citations

  • Self-repairing composite coating, application of self-repairing composite coating, anticorrosion material and preparation method of anticorrosion material

    CN110142190A

  • Self-repairable epoxy resin material as well as preparation method and application thereof

    CN111286009A

  • Anti-corrosion structure and preparation method thereof

    CN116589905A

Cited By

  • Preparation method of reversible dual-network epoxy resin adhesive

    CN119529717A

  • Preparation method of corrosion-resistant conductive composite coating for electrode

    CN121343450A

  • A method for the preparation of a corrosion-resistant, electrically conductive composite coating for electrodes

    CN121343450B

  • Corrosion-resistant epoxy ester resin with high adhesion for anticorrosive paint and preparation method thereof

    CN122278308B