Preparation method of bio-based fireproof coating material and automobile battery cover

By applying the prepared bio-based fire-proof coating material to the electric vehicle battery pack, the problems of poor insulation and fire-proof effects in the existing technology are solved, and the safety and fire-proof and heat-insulating performance of the battery are significantly improved.

CN118791964APending Publication Date: 2024-10-18SHANGHAI BENYO NEW MATERIAL & TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411140615.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The existing fire-retardant coating materials in electric vehicle battery packs have poor insulation and fire-proof effects, leading to the risk of battery fire and explosion and affecting the safety of new energy vehicles.

Method used

A method for preparing bio-based fire retardant coating materials is adopted. Insulating modified bio-based polyethers and flame retardants are stirred under specific temperature and vacuum conditions, and catalysts and isocyanates are added for reaction to form a coating with excellent insulation and fire retardant properties. Bio-based fire retardant coating materials and applied to car battery covers.

Benefits of technology

This bio-based fireproof coating material can maintain low temperature under 1200°C flame burning, significantly improve the fireproof, heat insulation and insulation performance of the battery cover, and enhance the safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791964A_ABST
    Figure CN118791964A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a preparation method of a bio-based fireproof coating material and an automobile battery cover, and the preparation method of the bio-based fireproof coating material comprises the following steps: respectively preparing a component A and a component B in sequence, and then mixing the component A and the component B to obtain the bio-based fireproof coating material. According to the preparation method of the bio-based fireproof coating material, the reaction conditions and time of all the raw materials are optimized and adjusted, and the matching and interaction of all the raw materials are utilized, so that the final product bio-based fireproof coating material can have more excellent flame retardance and insulation performance and also has excellent bonding performance; the composite material has excellent application prospect and excellent performance, and can effectively improve the safety performance of a battery when being applied to a shell and a cover plate of the power battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of fire-resistant coating materials, and in particular to a preparation method of a bio-based fire-resistant coating material and an automobile battery cover. Background Art

[0002] With the continuous development of my country's economy and the continuous improvement of people's living standards, cars have become a daily means of transportation for ordinary people, but most of them are fuel-powered cars, with a large amount of fuel consumption and exhaust emissions, which have an increasingly serious impact on the environment. People are increasingly aware of the importance of protecting the environment. Therefore, in order to protect the environment, the country issued a new energy vehicle industry development plan in 2012 and continued to vigorously promote new energy vehicles, which has led to the rapid development of new energy vehicles. In particular, the sales of new energy vehicles have exploded in recent years, making new energy vehicles quickly enter people's daily lives.

[0003] With the advancement of power battery technology and the increasing market recognition of new energy vehicles, the proportion of pure electric vehicles will further increase. The core technologies of new energy vehicles are mainly power battery technology, motor technology and electronic control technology, among which power batteries are one of the important core components of electric vehicles. Whether power battery technology can make breakthroughs, that is, whether power batteries with higher energy density and longer driving range can be achieved, is the key to the development prospects of electric vehicles. However, most power batteries are arranged under the floor of the vehicle body, which has a relatively harsh installation environment. During the driving process of the vehicle, the battery will have the risk of fire and explosion. In addition, the increase in energy density will further increase the risk of fire and explosion caused by thermal runaway of the power battery, resulting in casualties and property losses. Ultimately, it has affected consumers' confidence in the safety of new energy vehicles to a certain extent.

[0004] Most of the existing technologies achieve fireproofing of the battery pack of electric vehicles by applying a fireproof coating on the battery, thereby effectively reducing or even avoiding the risk of battery fire. However, most of the fireproof coatings used in the existing technologies have poor composition ratios of the constituent materials, resulting in poor insulation and fireproofing effects of the fireproof coatings. Therefore, there is an urgent need for a fireproof coating with excellent insulation and fireproofing effects. Summary of the invention

[0005] In order to overcome the technical problems existing in the prior art, the present application provides a bio-based fire-retardant coating material and a preparation method and a car battery cover, so that the battery using the bio-based fire-retardant coating material provided by the present application can have both good insulation and fire-retardant properties, thereby solving the problems raised in the above-mentioned background technology.

[0006] The present application provides a method for preparing a bio-based fire retardant coating material, comprising the following steps:

[0007] Step S1: adding the insulating modified bio-based polyether and the flame retardant into a reaction kettle and stirring them evenly, then heating the reaction kettle to 95-105° C. and stirring for 120 minutes to obtain a first product;

[0008] Step S2: evacuate the reactor until the vacuum degree is less than 0.005Mpa;

[0009] Step S3: testing the first product for moisture until the moisture content of the first product is less than 300 ppm;

[0010] Step S4: lowering the temperature of the reaction kettle to below 70° C., adding a catalyst, and stirring for another 30 minutes to obtain the A component;

[0011] Step S5: adding 0.001 part of antioxidant, 0.00001 part of polymerization inhibitor and A part of isocyanate into a reaction kettle, stirring evenly, then heating the reaction kettle to 45-55° C. and stirring for 15 minutes;

[0012] Step S6: adding the insulating modified bio-based polyol into the reactor, and then heating the reactor to 65-80° C.; keeping the temperature for 2-3 hours;

[0013] Step S7: adding a B-component isocyanate into the reactor, the isocyanate is fully reacted and converted into a polyurethane prepolymer, and the NCO content of the polyurethane prepolymer is tested at the same time. When the NCO content of the polyurethane prepolymer is a second preset value, the B component is obtained;

[0014] Step S8: mixing the component A and the component B to obtain the bio-based fire retardant coating material;

[0015] The sum of part A isocyanate and part B isocyanate is the whole part of isocyanate.

[0016] The bio-based fire retardant coating material prepared by the above steps using component A and component B as raw materials absorbs the insulation properties of the insulating modified bio-based polyol and the fire retardant properties of the flame retardant, so that it can have excellent fireproof and heat-insulating and insulation properties, and at the same time has strong adhesion properties, thereby effectively improving the comprehensive performance of the bio-based fire retardant coating material.

[0017] In some embodiments, the method for preparing the bio-based fire retardant coating material comprises the following steps:

[0018] Step S01: putting the bio-based polyol and the insulation modifier into the reactor, stirring them evenly, then heating the reactor to 95-105° C., stirring for 30 minutes, so that the insulation modifier and the bio-based polyol are fully reacted and converted into insulation-modified bio-based polyether;

[0019] Step S02: testing the hydroxyl value of the insulating modified bio-based polyether. When the hydroxyl value of the insulating modified bio-based polyether is a first preset value, the insulating modified bio-based polyether of component A is obtained.

[0020] In some embodiments, the first preset value is 20-300 mgKOH / g.

[0021] In some embodiments, the functionality of the bio-based polyol is 1 to 4, the hydroxyl value of the bio-based polyol is 20 to 300 mgKOH / g, and the weight ratio of the bio-based polyol is 50 to 95 wt %.

[0022] In some embodiments, the second preset value is 10-25 wt %.

[0023] In some embodiments, the weight portion of the insulating modified bio-based polyol is 40 to 45 parts, the weight portion of the flame retardant is 40 to 60 parts, and the weight portion of the catalyst is 0 to 1 part;

[0024] The mass ratio of the A component to the B component is 0.1-10.

[0025] By mixing component A and component B in a mass ratio of 10 / 1 to 1 / 10, the insulation performance and fire resistance of the final fire-retardant coating material can reach a balance, that is, it has good insulation performance and fire resistance at the same time. The fire-retardant coating material with better comprehensive performance can have stronger market competitiveness.

[0026] In some embodiments, the isocyanate is at least one of diphenylmethane diisocyanate and perhydrogenated diphenylmethane diisocyanate.

[0027] In some embodiments, the functionality of the insulation modified bio-based polyol is 0-4, the hydroxyl value of the insulation modified bio-based polyol is 20-300 mgKOH / g, and the weight average molecular weight of the insulation modified bio-based polyol is 300-1500 g / mol.

[0028] In some embodiments, the flame retardant is an expandable flame retardant with a particle size of 1 to 200 um.

[0029] Through many experiments, it is known that when the particle size of the flame retardant is 1-200um, the specific surface area of ​​the flame retardant is relatively larger and the porosity is also higher, so that the flame retardant can better adsorb and disperse the gaseous substances in the flame, and can also better slow down the combustion rate, thereby achieving a stronger flame retardant and fireproof effect.

[0030] In some embodiments, the present application also provides a car battery cover, which includes a bio-based fire-retardant coating material manufactured by the preparation method described in any of the above embodiments; the electrical breakdown strength of the car battery cover is greater than 5kv / mm; the temperature of the car battery cover does not exceed 300°C under the burning of a 1200°C flame.

[0031] The present invention has at least the following beneficial effects:

[0032] 1. By optimizing and adjusting the proportion of each component in the raw material, and utilizing the coordination and interaction between the components, the bio-based fire-retardant coating material of the present invention can have both more excellent fire-retardant performance and good insulation performance, and also has excellent bonding performance, and thus has excellent application prospects and excellent performance. It can be applied to power battery housings and cover plates, and can effectively improve the safety performance of the battery;

[0033] 2. By using specific specifications of insulation-modified bio-based polyols and flame retardants, the insulation and flame retardant properties of the bio-based fire-retardant coating material are improved, thereby ensuring that it has good comprehensive performance in many aspects. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a temperature curve diagram of the flame retardant test results of the bio-based fire retardant coating materials prepared in Examples 1-3 and Comparative Example 4 of the present application. DETAILED DESCRIPTION

[0035] The following specific embodiments illustrate the implementation of the present application, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Although the description of the present application will be introduced in conjunction with some embodiments, this does not mean that the features of this application are limited to the implementation. On the contrary, the purpose of introducing the application in conjunction with the implementation is to cover other options or modifications that may be extended based on the claims of the present application. In order to provide a deep understanding of the present application, the following description will include many specific details. The present application can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present application, some specific details will be omitted in the description. It should be noted that the embodiments in the present application and the features in the embodiments can be combined with each other without conflict.

[0036] It should be noted that in this specification, similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings.

[0037] The present application provides a method for preparing a bio-based fire-retardant coating material, which is used to manufacture the bio-based fire-retardant coating material in any of the above embodiments, and is characterized in that it includes the following steps: Step S1: Add the insulating modified bio-based polyether and the flame retardant into a reactor, stir evenly, then heat the reactor to 95-105°C, and stir for 120 minutes to obtain a first product; Step S2: Evacuate the reactor until the vacuum degree is <0.005Mpa; Step S3: Test the moisture content of the first product until the moisture content of the first product is <300ppm; Step S4: Reduce the temperature of the reactor to below 70°C, add a catalyst, and stir for another 30 minutes to obtain component A; Step S5: Add 0.001 parts of an antioxidant and an inhibitor; Step S6: Add 0.001 parts of an antioxidant and an inhibitor; Step S7: Add 0.001 parts of an antioxidant and an inhibitor; Step S8: Add 0.001 parts of an antioxidant and an inhibitor; Step S9: Add 0.001 parts of an antioxidant and an inhibitor; Step S10: Add 0.001 parts of an antioxidant and an inhibitor; Step S11: Add 0.001 parts of an antioxidant and an inhibitor; Step S12: Add 0.001 parts of an antioxidant and an inhibitor; Step S13: Add 0.001 parts of an antioxidant and an inhibitor; Step S14: Add 0.001 parts of an antioxidant and an inhibitor; Step S15: Add 0.001 parts of an antioxidant and an inhibitor; Step S16: Add 0.001 parts of an antioxidant and an inhibitor; Step S17: Add 0.001 parts of an antioxidant and an inhibitor; Step S18: Add 0.001 parts of an antioxidant and an inhibitor; Step S19: Add 0.001 parts of an antioxidant and an inhibitor; Step S20: Add 0.001 parts of an antioxidant and an inhibitor 0.00001 parts and A parts of partial isocyanate are put into the reactor, stirred evenly, then the reactor is heated to 45-55°C and stirred for 15 minutes; step S6: insulating modified bio-based polyol is put into the reactor, then the reactor is heated to 65-80°C; keep warm for 2-3 hours; step S7: the remaining isocyanate of B parts is put into the reactor, the isocyanate is fully reacted and converted into polyurethane prepolymer, and the NCO content of the polyurethane prepolymer is tested at the same time. When the NCO content of the polyurethane prepolymer is a second preset value, the B component is obtained; step S8: mixing the A component and the B component to obtain the bio-based fire retardant coating material; wherein the sum of the A part of the isocyanate and the B part of the remaining isocyanate is the whole part of the isocyanate.

[0038] Specifically, the raw materials are fully reacted by heating and stirring to obtain the first product, the vacuum degree in the test reactor and the moisture in the first product are tested, and the vacuum degree in the test reactor and the moisture in the first product are controlled by controlling the high-temperature reaction time in time to ensure that the vacuum degree is less than 0.005Mpa and the final moisture of the first product is less than 300ppm, and then the catalyst is added after cooling, and then fully stirred to obtain the A component material, which provides a guarantee for the subsequent preparation of high-quality bio-based fire retardant coating materials. In addition, the preparation of the B component material is mainly as follows: first, prepare a sufficient amount of isocyanate, and divide it into A part and B part, and mix the A part isocyanate and the barrier The flame retardant and antioxidant are put into the reactor and stirred evenly. Then the reactor is heated to 45-55°C and stirred for 15 minutes to mix the isocyanate, flame retardant and antioxidant in the reactor and react fully. Then the insulating modified bio-based polyol is put into the reactor and the reactor is heated to 65-80°C. The reaction is kept warm for 2-3 hours. Part B of isocyanate is put into the reactor and mixed with the materials in the reactor. Then the isocyanate is fully reacted and converted into a polyurethane prepolymer. The NCO content of the polyurethane prepolymer is tested. When the NCO content of the polyurethane prepolymer is the preset value, a bio-based fire retardant coating material with excellent heat resistance and insulation properties is obtained. By adding isocyanate into the reactor in batches for reaction, the isocyanate can be fully and evenly distributed in the bio-based fire-retardant coating material, thereby effectively ensuring the uniformity of the thermal insulation and insulation properties of the bio-based fire-retardant coating material. The insulating modified bio-based polyol in the raw material has good insulation properties. The flame retardant can be mainly composed of zinc borate and cobalt aluminate. A certain proportion of insulating modified bio-based polyol, flame retardant and catalyst are mixed to prepare the raw material of component A. The raw material of component B is mainly isocyanate, wherein the insulating modified bio-based polyol, flame retardant, isocyanate and catalyst can be more than one. Under certain conditions, the reaction can form a high molecular polymer of polyurethane prepolymer. The polyurethane prepolymer has the characteristic of improving the adhesion strength of the material, especially can produce good adhesion with materials such as metals. In addition, when the polyurethane prepolymer is used in the coating, it can increase the effect of the coating by controlling the internal materials in the coating, and can be quickly dried in a natural environment, which has the effect of strengthening the coating effect.

[0039] It should be pointed out that, according to experimental data, when the amount of A is greater than the amount of B, the obtained B component product has the characteristics of fast reaction activity, unstable state and high reaction efficiency, and when the amount of A is less than the amount of B, the obtained B component product has the characteristics of slow reaction activity and stable state. The specific amount of A and B is usually adjusted according to the actual final demand. For example, the bio-based fire retardant coating material required for the battery cover of an automobile usually requires fast reaction activity, unstable state and high reaction efficiency, that is, it is more suitable for the amount of A to be greater than the amount of B. In addition, the antioxidant can be 4,4'-thiobis(6-tert-butyl-m-cresol), and the inhibitor can be any one of benzoyl chloride and terephthaloyl chloride.

[0040] In some embodiments, the preparation method of the insulating modified bio-based polyether includes the following steps: Step S01: Add the bio-based polyol and the insulating modifier into a reactor and stir evenly, then heat the reactor to 95-105°C, and stir for 30 minutes to allow the insulating modifier and the bio-based polyol to fully react and convert into the insulating modified bio-based polyether; Step S02: Test the hydroxyl value of the insulating modified bio-based polyether. When the hydroxyl value of the insulating modified bio-based polyether is a first preset value, the insulating modified bio-based polyether of component A is obtained.

[0041] Specifically, by stirring for 30 minutes in a high temperature environment, the insulation modifier and the bio-based polyol are fully reacted to be converted into an insulation-modified bio-based polyether, so that the bio-based polyether has good insulation properties, while having heat resistance and flame retardant properties that the polyol does not have, thereby providing a guarantee for achieving the insulation, heat resistance and flame retardant properties of the final bio-based fire retardant coating material.

[0042] In some embodiments, the first preset value is 20-300 mgKOH / g.

[0043] Specifically, through multiple experiments, it is known that when the hydroxyl value of the insulating modified bio-based polyether is preferably 20-300 mgKOH / g, its insulation strength is higher. Therefore, by multiple adjustments, the hydroxyl value of the insulating modified bio-based polyether of component A is optimized to 20-300 mgKOH / g, which can optimize the insulation performance of the bio-based fire retardant coating material applied for in this application.

[0044] In some embodiments, the functionality of the bio-based polyol is 1 to 4, the hydroxyl value of the bio-based polyol is 20 to 300 mgKOH / g, and the weight ratio of the bio-based polyol is 50 to 95 wt %.

[0045] Specifically, through many experiments, it is known that when the functionality of the bio-based polyol is preferably 1-4, the hydroxyl value of the insulation-modified bio-based polyol is 20-300 mgKOH / g, and the weight ratio of the bio-based polyol is 50-95wt%, the fire-retardant coating material prepared after the reaction can effectively improve its insulation performance without affecting its fire-retardant performance, thereby comprehensively improving the comprehensive performance of the fire-retardant coating material provided in the present application.

[0046] In some embodiments, the second preset value is 10-25 wt %.

[0047] Specifically, through many experimental results, it can be known that when the NCO content of the polyurethane prepolymer calculated based on the total amount of the prepolymer is 10-25wt%, preferably 15-23wt%, and particularly preferably 18-22wt%, the bio-based fire retardant coating material has excellent heat resistance and insulation properties.

[0048] In some embodiments, the weight portion of the insulating modified bio-based polyol is 40-45 parts, the weight portion of the flame retardant is 40-60 parts, the weight portion of the catalyst is 0-1 part, and the mass ratio of component A to component B is 0.1-10.

[0049] Specifically, when component A and component B are mixed in a mass ratio of 10 / 1 to 1 / 10, the fire-retardant coating material finally prepared has better comprehensive performance. According to multiple experimental results, it can be known that the mass ratio of component A to component B is preferably 2 / 1 to 1 / 2 for the best effect. The bio-based fire-retardant coating material provided in the present application adds a certain proportion of isocyanate to effectively improve the adhesion of the fire-retardant coating material itself. The bio-based fire-retardant coating material prepared by using component A and component B as raw materials can have excellent fireproofing, heat insulation and insulation properties, and at the same time has strong adhesion properties, effectively improving the comprehensive performance of the bio-based fire-retardant coating material.

[0050] It should be pointed out that according to experimental data, the greater the proportion of component B in the raw material, the harder the final bio-based fire retardant coating material will be. The specific ratio of component A to component B depends on actual needs.

[0051] In some embodiments, the isocyanate is at least one of diphenylmethane diisocyanate and perhydrogenated diphenylmethane diisocyanate.

[0052] Specifically, the isocyanate can be diphenylmethane diisocyanate, or fully hydrogenated diphenylmethane diisocyanate, or a mixture of diphenylmethane diisocyanate and fully hydrogenated diphenylmethane diisocyanate. Both diphenylmethane diisocyanate and fully hydrogenated diphenylmethane diisocyanate have excellent thermal insulation properties and good corrosion resistance, and can be used as the main component of the coating to further improve the fireproof and heat-insulating properties and service life of the coating.

[0053] In some embodiments, the flame retardant is an expandable flame retardant having a particle size of 1 to 200 um.

[0054] Specifically, the main components of expandable flame retardants include inorganic substances, organic substances, and a small amount of catalysts and foaming agents. During the combustion process, a large amount of carbonized products can be produced to form an expanded carbonized layer, thereby more effectively isolating oxygen and flames. According to multiple experiments, when the particle size of the flame retardant is 1 to 200 um, the specific surface area of ​​the flame retardant is relatively larger and the porosity is also higher, so that the flame retardant can better adsorb and disperse the gaseous substances in the flame, and can also better slow down the combustion rate, thereby achieving a stronger flame retardant and fireproof effect.

[0055] It should be pointed out that the expandable flame retardant can be an inorganic expandable flame retardant such as sodium aluminum silicate, calcium aluminum phosphate, etc., or a nitrogen-phosphorus flame retardant, or a metal hydroxide flame retardant, which is not limited here and depends on actual needs.

[0056] In some embodiments, the functionality of the insulated modified bio-based polyol is 0-4, the hydroxyl value of the insulated modified bio-based polyol is 20-300 mgKOH / g, and the weight average molecular weight of the insulated modified bio-based polyol is 300-1500 g / mol.

[0057] Specifically, through multiple experiments, it is known that when the functionality of the insulating modified bio-based polyol is 0-4, the hydroxyl value of the insulating modified bio-based polyol is 20-300 mgKOH / g, and the weight-average molecular weight of the insulating modified bio-based polyol is 300-1500 g / mol, it has a higher insulation strength than other bio-based polyols, so that the fire-retardant coating material prepared after the reaction can effectively improve its insulation performance without affecting its fire-retardant performance, thereby comprehensively improving the comprehensive performance of the fire-retardant coating material provided in the present application.

[0058] The present application also provides a car battery cover, the surface of which is coated with the bio-based fireproof coating material in any of the above embodiments, and the electrical breakdown strength of the car battery cover is greater than 5kv / mm, see the attached Figure 1 It can be seen that the temperature of the car battery cover does not exceed 300°C under the burning of a 1200°C flame.

[0059] Specifically, the automobile battery cover applied with the bio-based fire-retardant coating material provided by the present application has excellent fireproofing, heat-insulating and insulating properties. After many experiments, it is known that the electrical breakdown strength of the automobile battery cover of the present application is greater than 5kv / mm. It can effectively ensure the structural stability of the automobile battery cover and effectively avoid the risk of electric shock caused by leakage. The specific experimental method is to burn one side of the automobile battery cover at 1200°C, and then monitor the temperature of the other side to achieve a thermal assessment experiment on the automobile battery cover. The automobile battery cover that has been used with the bio-based fire-retardant coating material of the present application has better fireproofing and heat-insulating properties. When the automobile battery cover is burned at a flame of 1200°C, the temperature of the side of the automobile battery cover away from the flame does not exceed 300°C. When the quality of the bio-based fire-retardant coating material is excellent, the temperature of the side of the car battery cover away from the flame does not exceed 270°C, or even 250°C. In addition, it can ensure that the car battery cover will not be burned through when burned at a flame of 1200°C for at least 10 minutes, and can even last for 20 minutes without being burned through. When the quality of the bio-based fire-retardant coating material is excellent, the car battery cover can remain unburned when burned at a flame of 1200°C for at least 30 minutes, which effectively reflects the excellent thermal insulation and fire retardant properties of the bio-based fire-retardant coating material.

[0060] The present invention is further explained below in conjunction with specific examples, but the examples do not limit the present invention in any form.

[0061] The insulating agent described in the following embodiments adopts an insulating agent with a brand of Asko and a model of ASK-50; the isocyanate adopts an isocyanate with a brand of Suprasec and a model of Suprasec2020, Suprasec1801, and Suprasec5005; the modified castor oil adopts a modified castor oil with a brand of Benyou and a model of BP-19; the bio-based polyol adopts a dimer acid polyester with a brand of Benyou and a model of BPD-16; the antioxidant adopts an antioxidant with a brand of Chemtura and a model of TMB-6; the defoamer adopts a defoamer with a brand of BYK and a model of BYK-088; the flame retardant adopts a flame retardant with a brand of Clariant and a model of AP422 and AP428; the remaining raw materials are conventional raw materials that can be purchased by those skilled in the art.

[0062] Example 1 Preparation of bio-based fire retardant coating materials

[0063] Raw materials by weight: insulating agent 100g, castor oil 490g, modified castor oil 150g, dimer acid polyester 80g, isocyanate (Suprasec2020) 580g, isocyanate (Suprasec1801) 113g, isocyanate (Suprasec5005) 91g, antioxidant 1g, benzoyl chloride (Chinese medicine) 0.01g;

[0064] Preparation of insulating bio-based polyol: First, 100g of insulating agent, 490g of castor oil, and 150g of modified castor oil are put into a reactor, heated to 90-105 degrees, and stirred for 30 minutes; the hydroxyl value is tested, and when the hydroxyl value reaches the theoretical value of 148mgKOH / g, the discharge process is carried out, and the preparation of the first bio-based polyol is completed.

[0065] Preparation of modified isocyanate: 580g of isocyanate (Suprasec2020), 113g of isocyanate (Suprasec1801), 1g of antioxidant, and 0.01g of benzoyl chloride are put into a reactor and heated to 45-55 degrees. Stir for 15 minutes, then add 216g of the insulating bio-based polyol prepared above, continue heating to 65-80 degrees, and react for 2-3 hours; then add 91g of isocyanate (Suprasec5005) and stir for 30 minutes; test the NCO content. When the NCO content reaches the theoretical value of 20.8, the discharging process is carried out, and the preparation of the modified isocyanate is completed.

[0066] Preparation of bio-based fire-retardant coating material: According to the raw material formula configuration, component A can be obtained, specifically: component A and the modified isocyanate prepared above are mixed at a mass ratio of 0.5-10. The bio-based fire-retardant coating material is obtained by mixing evenly, and the bio-based fire-retardant coating material obtained by mixing evenly is applied on an aluminum plate, and the coating thickness is controlled to be 1 mm. After curing, the bio-based fire-retardant coating 1 can be obtained.

[0067] Example 2 Preparation of bio-based fire retardant coating materials

[0068] Raw materials by weight: insulating agent 80g, castor oil 490g, modified castor oil 150g, dimer acid polyester 80g, isocyanate (Suprasec2020) 580g, isocyanate (Suprasec1801) 113g, isocyanate (Suprasec5005) 91g, antioxidant 1g, benzoyl chloride (Chinese medicine) 0.01g;

[0069] Preparation of insulating bio-based polyols: First, 100 g of insulating agent, 490 g of castor oil, and 150 g of modified castor oil are put into a reactor, heated to 90-105 degrees, and stirred for 30 minutes; the hydroxyl value is tested, and when the hydroxyl value reaches the theoretical value of 152 mgKOH / g, the discharge process is carried out, and the preparation of the first bio-based polyol is completed.

[0070] Preparation of modified isocyanate: 580g of isocyanate (Suprasec2020), 113g of isocyanate (Suprasec1801), 1g of antioxidant, and 0.01g of benzoyl chloride are put into a reactor and heated to 45-55 degrees. Stir for 15 minutes, then add 216g of the insulating bio-based polyol prepared above, continue heating to 65-80 degrees, and react for 2-3 hours; then add 91g of isocyanate (Suprasec5005) and stir for 30 minutes; test the NCO content. When the NCO content reaches the theoretical value of 20.8, the discharging process is carried out, and the preparation of the modified isocyanate is completed.

[0071] Preparation of bio-based fire-retardant coating material: According to the raw material formula configuration, component A can be obtained, specifically: component A and the modified isocyanate prepared above are mixed at a mass ratio of 0.5-10. The bio-based fire-retardant coating material is obtained by mixing evenly, and the bio-based fire-retardant coating material obtained by mixing evenly is applied on an aluminum plate, and the coating thickness is controlled to be 1 mm. After curing, the bio-based fire-retardant coating 2 is obtained.

[0072] Example 3 Preparation of bio-based fire retardant coating materials

[0073] Raw materials by weight: 60g insulating agent, 490g castor oil, 150g modified castor oil, 80g dimer acid polyester, 580g isocyanate (Suprasec2020), 113g isocyanate (Suprasec1801), 91g isocyanate (Suprasec5005), 1g antioxidant, 0.01g benzoyl chloride (Chinese medicine);

[0074] Preparation of insulating bio-based polyols: First, 100 g of insulating agent, 490 g of castor oil, and 150 g of modified castor oil are put into a reactor, heated to 90-105 degrees, and stirred for 30 minutes; the hydroxyl value is tested, and when the hydroxyl value reaches the theoretical value of 154 mgKOH / g, the discharge process is carried out, and the preparation of the first bio-based polyol is completed.

[0075] Preparation of modified isocyanate: 580g of isocyanate (Suprasec2020), 113g of isocyanate (Suprasec1801), 1g of antioxidant, and 0.01g of benzoyl chloride are put into a reactor and heated to 45-55 degrees. Stir for 15 minutes, then add 216g of the insulating bio-based polyol prepared above, continue heating to 65-80 degrees, and react for 2-3 hours; then add 91g of isocyanate (Suprasec5005) and stir for 30 minutes; test the NCO content. When the NCO content reaches 20.8, the discharging process is carried out, and the preparation of the modified isocyanate is completed.

[0076] Preparation of bio-based fire-retardant coating material: According to the raw material formula configuration, component A can be obtained, specifically: component A and the modified isocyanate prepared above are mixed at a mass ratio of 0.5-10. The bio-based fire-retardant coating material is obtained by mixing evenly, and the bio-based fire-retardant coating material obtained by mixing evenly is applied on an aluminum plate, and the coating thickness is controlled to be 1 mm. After curing, the bio-based fire-retardant coating 3 is obtained.

[0077] Comparative Example 4 Preparation of Bio-based Fire Retardant Coating Materials

[0078] The raw materials are composed by weight: 490 g of castor oil; 150 g of modified castor oil, 80 g of dimer acid polyester, 580 g of isocyanate (Suprasec 2020), 113 g of isocyanate (Suprasec 1801), 91 g of isocyanate (Suprasec 5005), 1 g of antioxidant, and 0.01 g of benzoyl chloride (Chinese medicine).

[0079] Preparation of insulating bio-based polyols: First, 490 g of castor oil and 150 g of modified castor oil were put into a reactor, heated to 90-105 degrees, and stirred for 30 minutes; the hydroxyl value was tested, and when the hydroxyl value reached the theoretical value of 160 mgKOH / g, the material was discharged, and the preparation of the first bio-based polyol was completed.

[0080] Preparation of modified isocyanate: 580g of isocyanate (Suprasec2020), 113g of isocyanate (Suprasec1801), 1g of antioxidant, and 0.01g of benzoyl chloride are put into a reactor and heated to 45-55 degrees. Stir for 15 minutes, then add 216g of the insulating bio-based polyol prepared above, continue heating to 65-80 degrees, and react for 2-3 hours; then add 91g of isocyanate (Suprasec5005) and stir for 30 minutes; test the NCO content. When the NCO content reaches 20.8, the discharging process is carried out, and the preparation of the modified isocyanate is completed.

[0081] Preparation of bio-based fire-retardant coating material: According to the raw material formula configuration, component A can be obtained, specifically: component A and the modified isocyanate prepared above are mixed at a mass ratio of 0.5-10. The bio-based fire-retardant coating material is obtained by mixing evenly, and the bio-based fire-retardant coating material obtained by mixing evenly is applied on an aluminum plate, and the coating thickness is controlled to be 1 mm. After curing, the bio-based fire-retardant coating 4 is obtained.

[0082] The coating formulas of component A in the above-mentioned Example 1, Example 2, Example 3 and Comparative Example 4 are all formulated according to the following proportions: 45% biopolyol, 1.0% defoamer, 12.5% ​​expanded graphite, 12.5% ​​aluminum hydroxide, 12.5% ​​flame retardant 1, 12.5% ​​flame retardant 2 and 4% 3A molecular sieve, and finally four different fire retardant coatings are obtained.

[0083] The flame retardant properties of the fire retardant coatings of Example 1, Example 2, Example 3, Comparative Example 4 and a blank control example were tested in turn. The specific flame retardant properties testing steps were as follows: the sample was coated on an aluminum plate, the coating thickness was controlled to be 1 mm, and then the side of the aluminum plate coated with the coating was burned with a flame of 1200°C, and then the temperature of the side without the coating was tested with an infrared thermometer and the temperature data was recorded. The results are shown in FIG. Figure 1 shown.

[0084] Depend on Figure 1 It is known that the fire-retardant coating material prepared in the present application has excellent flame retardant properties and can play a good fire-proofing effect.

[0085] The mechanical properties of the fire retardant coatings obtained in Example 1, Example 2, Example 3 and Comparative Example 4 were tested. The specific mechanical properties test experiments included breakdown strength test, tensile strength test, elongation at break test and hardness test. The specific steps of the breakdown strength test were as follows: first, the fire retardant coating sample was made into a thickness of 1 mm, and then the fire retardant coating sample was placed in a breakdown strength tester, and the voltage was adjusted until the current broke down the fire retardant coating sample. The voltage intensity recorded at the time of breakdown was the breakdown strength. The specific steps of the tensile strength test were as follows: first, the fire retardant coating sample was made into a thickness of 1 mm, and then the fire retardant coating sample was cut into tensile strips, and then a tensile test was performed with a universal machine until the tensile strip broke. The force value displayed on the universal machine was recorded, and then the tensile strength was obtained through calculation. The specific steps of the elongation at break test were as follows: first, the fire retardant coating sample was made into a thickness of 1 mm, and then the sample was cut into tensile strips, and then a tensile test was performed with a universal machine until the strip broke. Record the stretching distance displayed on the Wanli machine, and then calculate and obtain the elongation at break; the specific steps of the hardness test are to first make the fire retardant coating sample into a thickness of 10mm. Then use the Shore A hardness tester to test the surface hardness of the fire retardant coating sample. Record the reading of the Shore A hardness tester. The results of the above tests are shown in Table 1.

[0086] Table 1 Tensile properties test results

[0087] Test items Example 1 Example 2 Example 3 Comparative Example 4 Breakdown strength (Kv / mm) 6.5 5.4 4.5 2.9 Tensile strength(Mpa) 3.1 2.8 2.9 3.1 Elongation at break (%) 77 77 82 76 Hardness(Shore A) 85 85 85 85

[0088] It can be seen from Table 1 that the fire-retardant coating material prepared in the present application has excellent tensile properties, wherein the breakdown strength of the fire-retardant coating material prepared in the present application is significantly improved relative to the comparative example.

[0089] Obviously, those skilled in the art can make various changes and modifications to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and modifications of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and modifications.

Claims

1. A method for preparing a bio-based fire-retardant coating material, characterized in that: The following steps are involved: Step S1: adding the insulating modified bio-based polyether and the flame retardant into a reaction kettle and stirring them evenly, then heating the reaction kettle to 95-105° C. and stirring for 120 minutes to obtain a first product; Step S2: evacuate the reactor until the vacuum degree is less than 0.005Mpa; Step S3: testing the first product for moisture until the moisture content of the first product is less than 300 ppm; Step S4: lowering the temperature of the reaction kettle to below 70° C., adding a catalyst, and stirring for another 30 minutes to obtain the A component; Step S5: adding 0.001 part of antioxidant, 0.00001 part of polymerization inhibitor and A part of isocyanate into a reaction kettle, stirring evenly, then heating the reaction kettle to 45-55° C. and stirring for 15 minutes; Step S6: adding the insulating modified bio-based polyol into the reactor, and then heating the reactor to 65-80° C.; keeping the temperature for 2-3 hours; Step S7: adding a B-component isocyanate into the reactor, the isocyanate is fully reacted and converted into a polyurethane prepolymer, and the NCO content of the polyurethane prepolymer is tested at the same time. When the NCO content of the polyurethane prepolymer is a second preset value, the B component is obtained; Step S8: mixing the component A and the component B to obtain the bio-based fire retardant coating material; The sum of part A isocyanate and part B isocyanate is the whole part of isocyanate.

2. The method for preparing a bio-based fire retardant coating material according to claim 1, characterized in that: The preparation method of the insulating modified bio-based polyether comprises the following steps: Step S01: putting the bio-based polyol and the insulation modifier into the reactor, stirring them evenly, then heating the reactor to 95-105° C., stirring for 30 minutes, so that the insulation modifier and the bio-based polyol are fully reacted and converted into insulation-modified bio-based polyether; Step S02: testing the hydroxyl value of the insulating modified bio-based polyether. When the hydroxyl value of the insulating modified bio-based polyether is a first preset value, the insulating modified bio-based polyether of component A is obtained.

3. The method for preparing a bio-based fire retardant coating material according to claim 2, characterized in that: The first preset value is 20-300 mgKOH / g.

4. The method for preparing a bio-based fire retardant coating material according to claim 3, characterized in that: The functionality of the bio-based polyol is 1 to 4, the hydroxyl value of the bio-based polyol is 20 to 300 mgKOH / g, and the weight ratio of the bio-based polyol is 50 to 95 wt %.

5. The method for preparing a bio-based fire retardant coating material according to any one of claims 1 to 4, characterized in that: The second preset value is 10-25 wt %.

6. The method for preparing a bio-based fire retardant coating material according to claim 5, characterized in that: The weight portion of the insulating modified bio-based polyol is 40 to 45 parts, the weight portion of the flame retardant is 40 to 60 parts, and the weight portion of the catalyst is 0 to 1 part; The mass ratio of the A component to the B component is 0.1-10.

7. The method for preparing a bio-based fire-retardant coating material according to claim 6, characterized in that: The isocyanate is at least one of diphenylmethane diisocyanate and perhydrogenated diphenylmethane diisocyanate.

8. The method for preparing a bio-based fire-retardant coating material according to claim 7, characterized in that: The flame retardant is an expandable flame retardant with a particle size of 1 to 200 um.

9. The method for preparing a bio-based fire-retardant coating material according to claim 8, characterized in that: The functionality of the insulation modified bio-based polyol is 0-4, the hydroxyl value of the insulation modified bio-based polyol is 20-300 mgKOH / g, and the weight average molecular weight of the insulation modified bio-based polyol is 300-1500 g / mol.

10. An automobile battery cover, characterized in that: The surface of the automobile battery cover is coated with a bio-based fire-retardant coating material prepared by the preparation method described in any one of claims 1 to 9; The electrical breakdown strength of the automobile battery cover is greater than 5kv / mm; The temperature of the automobile battery cover does not exceed 300° C. under the burning of a 1200° C. flame.

Citation Information

Cited By

  • High-temperature-resistant composite integrated forming process for new energy automobile battery pack upper cover

    CN122975917A