Fireproof coating and preparation method thereof
By using multi-core shell flame retardant microcapsules and flame retardant in power battery coatings, the problems of low hygroscopicity and explosion-proof performance of existing coatings are solved, and higher flame retardancy and stability are achieved. In the high humidity and heat environment of modern lithium-ion batteries.
Patent Information
- Application Number
- CN202411418598.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the fire-retardant coating of power batteries has strong hygroscopicity, low viscosity, low fire-proof and explosion-proof performance, and the traditional organic expansion fire-retardant coating has poor water resistance and aging resistance, making it difficult to meet the high humidity and heat environment needs of modern lithium-ion batteries.
A new type of fire retardant coating is prepared by collaborative cooperation between multi-core shell flame retardant microcapsules and flame retardant and resin, including resin, microencapsulated flame retardant, modified fibers, hollow microspheres, filled pellet materials and solvents. The fire extinguishing agent is encapsulated by multiple layers of shells to improve high-temperature flame retardant performance and waterproof stability.
It significantly improves the flame retardant performance of the carbon layer under high temperature conditions, has fire extinguishing ability, enhances the flame retardancy, waterproofness and stability of the coating, and overcomes the problems of poor water resistance and aging resistance of traditional coatings.
Smart Images

Figure CN118909514A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy power batteries and coatings, and in particular to a fire retardant coating and a preparation method thereof. Background Art
[0002] Fire and explosion accidents caused by thermal runaway of new energy power batteries have been reported frequently, and safety issues have become one of the main reasons hindering the large-scale commercial application of lithium-ion batteries in the energy storage and power supply industries. Traditional battery protection materials are outdated or gradually being eliminated, and it is difficult to adapt to the current needs of thermal runaway fire protection. At the same time, thermal protection materials must also meet the requirements of coating thickness, temperature resistance, fire protection time, cold surface temperature, etc. Intumescent fire retardant coatings can protect the battery casing and block the rapid spread of thermal runaway explosions and fires. The organic flame retardant system PCN commonly used in intumescent fire retardant coatings is composed of ammonium polyphosphate, pentaerythritol, and melamine. It does not have active fire extinguishing capabilities and has poor water resistance. The coating is prone to cracking in high humidity and heat areas, affecting the stability of the fire retardant coating. Summary of the invention
[0003] The purpose of the present invention is to provide a fire retardant coating and a preparation method thereof, so as to solve the problems of strong hygroscopicity, low viscosity, and low fire and explosion resistance of the fire retardant coating of power batteries in the prior art.
[0004] To achieve the above object, the present invention provides the following solutions: One of the technical solutions of the present invention is a fire retardant coating, wherein the raw materials include, by weight, 0.1-30 parts of resin, 0-20 parts of microencapsulated flame retardant, 0-20 parts of modified fiber, 0-20 parts of hollow microspheres, 0.1-30 parts of filling particle material, 0.1-50 parts of flame retardant and 10-50 parts of solvent.
[0005] A second technical solution of the present invention is a method for preparing the above-mentioned fire retardant coating, which comprises uniformly mixing the raw materials according to their mass fractions to obtain the fire retardant coating.
[0006] A third technical solution of the present invention is the application of the above-mentioned fire retardant coating in lithium-ion power batteries.
[0007] The present invention discloses the following technical effects: The present invention constructs a new type of multi-core shell flame retardant microcapsule (microencapsulated flame retardant), which significantly increases the flame retardant performance of the char layer under high temperature conditions compared with a single flame retardant. At the same time, the fire retardant coating of the present invention has a certain fire extinguishing ability and exhibits better flame retardancy, water resistance and stability.
[0008] The fireproof coating of the present invention is to protect the power battery from deflagration during thermal runaway. The present invention uses a microencapsulated flame retardant with good flame retardancy, a flame retardant system (flame retardant) and a film-forming material (resin) to make the coating have the characteristics of moisture resistance and high bonding strength, overcoming the defects of traditional organic intumescent fireproof coatings such as poor water resistance and aging resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0010] Figure 1 The SEM images of ammonium polyphosphate in the present invention and the microencapsulated flame retardant prepared in Example 2 are shown in FIG. 1 , wherein (a) is ammonium polyphosphate and (b) is the microencapsulated flame retardant. DETAILED DESCRIPTION
[0011] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0012] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0013] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.
[0014] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0015] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0016] The "parts" described in the present invention, unless otherwise specified, all represent parts by mass.
[0017] The first aspect of the present invention provides a fire retardant coating, wherein the raw materials include, by weight, 0.1-30 parts of resin, 0-20 parts of microencapsulated flame retardant, 0-20 parts of modified fiber, 0-20 parts of hollow microspheres, 0.1-30 parts of filling particulate material, 0.1-50 parts of flame retardant and 10-50 parts of solvent.
[0018] In some embodiments of the present invention, the raw materials of the fire retardant coating include, by weight, 10-20 parts of resin, 0-20 parts of microencapsulated flame retardant, 0-20 parts of modified fiber, 0-20 parts of hollow microspheres, 5-10 parts of filling particulate material, 5-15 parts of flame retardant and 30-35 parts of solvent.
[0019] In some embodiments of the present invention, the raw materials of the fire retardant coating include, by mass, 18-25 parts of resin, 5-8 parts of microencapsulated flame retardant, 1-3 parts of modified fiber, 1-3 parts of hollow microspheres, 5-9 parts of filling particulate material, 8-10 parts of flame retardant and 30-35 parts of solvent.
[0020] In the present invention, the resin is a film-forming material. If the addition ratio is too low, the film cannot be formed or the hardness of the coating decreases and it is easy to crack. The filling particles play a role of skeleton and filling. If the addition ratio is too low, the mechanical properties of the coating decrease. If the solvent addition ratio exceeds the parameter range recorded above, it will cause the coating to be too thick or too thin, affecting the coating effect.
[0021] In some embodiments of the present invention, the resin is at least one of epoxy resin, solvent-free epoxy resin, unsaturated resin, modified amino resin, polyamide resin, acrylic resin, polyurethane, urea-formaldehyde resin, and alkyd resin.
[0022] In some embodiments of the present invention, the method for preparing the microencapsulated flame retardant comprises the following steps: After adding melamine and formaldehyde solution into water and mixing, adding NaHCO3 solution to adjust the pH to 9-10, then adding tetraethyl orthosilicate and perfluorohexanone to carry out heating reaction in a water bath, and freeze-drying to obtain microcapsule wall; Add chitosan or sulfate lignin to ethyl acetate or aminosilsesquioxane to dissolve, then add 10-50 parts of flame retardant, 0-5 parts of silane coupling agent and 30-50 parts of microcapsule wall to react, and dry the reaction product to constant weight to obtain the microencapsulated flame retardant; The flame retardant is the same as the above-mentioned flame retardant.
[0023] The temperature of the water bath heating reaction is 80°C and the time is 2h; the temperature of the reaction is 80°C and the time is 2h.
[0024] The molar ratio of the chitosan (or kraft lignin) to the ethyl acetate (or aminosilsesquioxane) is 0.3-1:15-19.
[0025] The mass ratio of the chitosan (or sulfate lignin) to the flame retardant is 1:(4-40).
[0026] In some specific embodiments of the present invention, the method for preparing the microencapsulated flame retardant comprises the following steps: Melamine and formaldehyde solution (concentration of formaldehyde solution is 36%) were mixed into deionized water (mass ratio of melamine and deionized water is 3:20) in a molar ratio of melamine to formaldehyde of 1:3, and stirred for 10 min using a magnetic stirrer. After stirring, NaHCO3 solution was added dropwise to adjust the pH to the range of 9-10. Then, tetraethyl orthosilicate and perfluorohexanone (mass ratio of tetraethyl orthosilicate to perfluorohexanone is 5:3; mass ratio of tetraethyl orthosilicate to melamine is 1:1) were added, and the mixture was placed in a water bath at a constant temperature of 80°C and stirred for 2 h. The microcapsule wall was obtained after freeze-drying.
[0027] Chitosan or sulfate lignin with a molar ratio of 0.3-1:15-19 is added to ethyl acetate or aminosilsesquioxane, and stirred until completely dissolved, and 10-50 parts of a flame retardant, 0-5 parts of a silane coupling agent, and 30-50 parts of the microcapsule wall are added; stirring is carried out in a water bath at a constant temperature of 80°C for 2 h, and then the reactant is filtered, washed with deionized water and ethanol and filtered again, cooled at room temperature and filtered, and the powder is poured into a petri dish and dried in an oven at 50°C for 24 hours to constant weight, and finally a microencapsulated flame retardant is obtained.
[0028] Compared with a single flame retardant such as ammonium polyphosphate, the microencapsulated flame retardant exhibits better flame retardancy and fire safety. The present invention disperses the fire extinguishing agent (perfluorohexanone) into the microencapsulated flame retardant through multi-layer core-shell encapsulation. The microcapsules rupture at high temperatures to release the fire extinguishing agent (i.e., perfluorohexanone) to alleviate the impact of thermal disasters. The present invention selects a multi-layer shell layer to improve the water resistance, flame retardancy, foaming, temperature resistance, aging resistance, and thermal stability of the flame retardant.
[0029] In some embodiments of the present invention, the modified fiber is at least one of modified aluminum silicate fiber, glass fiber, quartz fiber, mullite fiber, alumina fiber or basalt fiber.
[0030] In the present invention, the modified fiber can improve the crack resistance of the coating.
[0031] The preparation method of the modified fiber (taking alumina fiber as an example) comprises the following steps: adding alumina fiber to a mixture of KH560 solvent and anhydrous ethanol (the volume ratio of KH560 solvent to anhydrous ethanol is 1: (30-50)), and then stirring at 60°C for 6 hours. Subsequently, HQ flame retardant (ODOPB Chinese name 10-(2,5-dihydroxyphenyl)-9,10-dihydro-9-oxa-10-phosphophananthrene-10-oxide), triethylamine (catalyst) and dimethylformamide are added, inert gas is introduced, heated at 120-130°C for 12 hours, washed and dried to obtain organically modified alumina fiber (i.e., modified fiber).
[0032] The mass ratio of alumina fiber to HQ flame retardant, triethylamine and dimethylformamide is 10:8:1:1 In some embodiments of the present invention, the hollow microspheres are at least one of ceramic microspheres, glass microspheres, fly ash microspheres, zirconium oxide microspheres, and silicon oxide microspheres.
[0033] In a specific embodiment of the present invention, the hollow microspheres are at least one of etched ceramic microspheres, glass microspheres, fly ash microspheres, zirconium oxide microspheres, and silicon oxide microspheres.
[0034] The etching method is as follows (taking ceramic microspheres as an example): placing the ceramic microspheres in a 5%wt hydrochloric acid solution, keeping the constant temperature at 20°C, stirring for 2 hours and then standing for 24 hours, washing and drying to obtain etched hollow microspheres.
[0035] In some embodiments of the present invention, the filling particle material is at least one of glass powder, graphite powder, pearl powder, shell powder, mica powder, alumina powder, magnesium oxide powder, nano titanium oxide powder, nano magnesium hydroxide powder, montmorillonite, kaolin, bentonite, expandable graphite, cellulose, and aerogel powder.
[0036] In some embodiments of the present invention, the flame retardant is at least one of pentaerythritol phosphate (PEPA), expandable graphite (EG), melamine, pentaerythritol, dipentaerythritol, tripentaerythritol, zinc borate, cobalt aluminate, starch, glucose, melamine polyphosphate, dihydrogen aluminum phosphate, diammonium hydrogen phosphate, ammonium polyphosphate, ammonium pyrophosphate, melamine orthophosphate, polyethylene glycol, polyphosphoric acid, guanidine phosphate, and guanyl urea phosphate.
[0037] In some embodiments of the present invention, the solvent is at least one of modified emulsion, waterborne polyurethane, formaldehyde, ethanol, tetraethyl orthosilicate, ethyl acetate, silicone-acrylic emulsion, pure acrylic emulsion, styrene-acrylic emulsion, high-purity water, and deionized water.
[0038] In some embodiments of the present invention, the raw material further includes a foaming agent and a foam stabilizer.
[0039] The foaming agent is at least one of sodium dodecyl sulfate, ammonia formaldehyde, rosin, yellow dextrin, gelatin or water glue, etc.; the foam stabilizer is alum and / or aluminum sulfate.
[0040] When adding the foaming agent, add the foaming agent into the solvent, the speed of the foaming machine is about 200r / min, the stirring time is 30min, and then add the resin and other raw materials to disperse evenly.
[0041] In the present invention, a foaming agent is added to form a reticular porous three-dimensional polymer in the coating material, and the coating material has a sound-absorbing function, thereby becoming a flame-retardant and heat-insulating material for a battery pack of a new energy vehicle.
[0042] The second aspect of the present invention provides a method for preparing the above-mentioned fire retardant coating, which comprises uniformly mixing various raw materials according to their mass fractions to obtain the fire retardant coating.
[0043] In some embodiments of the present invention, the resin and the solvent may be mixed uniformly first, and then the microencapsulated flame retardant, the modified fiber, the hollow microspheres, the filling particle material and the flame retardant may be added and mixed uniformly to obtain the fire retardant coating.
[0044] A third aspect of the present invention provides an application of the above-mentioned fire retardant coating in a lithium-ion power battery.
[0045] Unless otherwise specified, the raw materials and reagents used in the examples of the present invention can be obtained through commercial sources.
[0046] The microcapsule wall used in the embodiment of the present invention is prepared by the following steps: Melamine and formaldehyde solution (concentration of formaldehyde solution is 36%) were mixed into deionized water (mass ratio of melamine and deionized water is 3:20) in a molar ratio of melamine to formaldehyde of 1:3, and stirred thoroughly for 10 min using a magnetic stirrer. After stirring, NaHCO3 solution was added dropwise to adjust the pH to the range of 9-10; then tetraethyl orthosilicate and perfluorohexanone (mass ratio of tetraethyl orthosilicate to perfluorohexanone is 5:3; mass ratio of tetraethyl orthosilicate to melamine is 1:1), placed in a water bath at a constant temperature of 80°C and stirred continuously for 2 h, and the microcapsule wall was obtained after freeze-drying.
[0047] The preparation method of the modified mullite fiber used in the embodiment of the present invention comprises the following steps: Alumina fiber was added to a mixture of KH560 solvent and anhydrous ethanol (the volume ratio of KH560 solvent to anhydrous ethanol was 1:40), and then stirred at 60°C for 6 hours. Subsequently, HQ flame retardant, triethylamine and dimethylformamide were added and mixed (the mass ratio of alumina fiber to HQ flame retardant, triethylamine and dimethylformamide was 10:8:1:1), inert gas was introduced, heated at 120-130°C for 12 hours, washed and dried to obtain modified mullite fiber.
[0048] The preparation method of the modified glass fiber used in the embodiment of the present invention comprises the following steps: The glass fiber was added to a mixture of KH560 solvent and anhydrous ethanol (the volume ratio of KH560 solvent to anhydrous ethanol was 1:30-50), and then stirred at 60°C for 6 hours. Subsequently, HQ flame retardant, triethylamine and dimethylformamide were added and mixed (the mass ratio of glass fiber to HQ flame retardant, triethylamine and dimethylformamide was 10:8:1:1), inert gas was introduced, and the mixture was heated at 120-130°C for 12 hours, washed and dried to obtain modified glass fiber.
[0049] The molecular weight of the ammonium polyphosphate used in the examples of the present invention is 149.086.
[0050] The aerogel powder used in the embodiments of the present invention is commercially available, and is specifically silicon dioxide aerogel.
[0051] The silane coupling agent used in the embodiment of the present invention is commercially available, namely KH560.
[0052] The hollow glass beads, hollow ceramic microspheres and hollow fly ash microspheres used in the embodiments of the present invention are all etched hollow glass beads, hollow ceramic microspheres and hollow fly ash microspheres; the raw hollow glass beads, hollow ceramic microspheres and hollow fly ash microspheres before etching are purchased, and the particle sizes are 15-135 μm, 1-200 μm and 5-500 μm, respectively.
[0053] The molecular weight of the epoxy resin used in the embodiment of the present invention is 375.86.
[0054] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention. Example 1
[0055] Add 0.8 parts of chitosan to 15 parts of ethyl acetate, stir until completely dissolved, add 7.8 parts of pentaerythritol phosphate (PEPA), 5.5 parts of expandable graphite, 1.5 parts of silane coupling agent, and 30 parts of microcapsule wall. Stir in a water bath at a constant temperature of 80°C for 2 hours, cool to room temperature and filter, and dry in an oven at 50°C for 24 hours to obtain a microencapsulated flame retardant. 5 parts of the above-mentioned microencapsulated flame retardant, 20 parts of epoxy resin, 10 parts of styrene acrylic emulsion and 20 parts of high-purity water are placed in a stainless steel dispersion tank and fully stirred at a speed of 1200 r / s for 30 min, and then 4 parts of ammonium polyphosphate, 2 parts of melamine, 3 parts of pentaerythritol, 2 parts of modified mullite fiber, 1.3 parts of hollow glass beads, 1.2 parts of nano titanium oxide powder, 2 parts of nano magnesium hydroxide powder, 2.5 parts of expandable graphite, 1.5 parts of cellulose, and 1.2 parts of aerogel powder are added to the dispersion tank, and the mixture is dispersed at a speed of 1500 r / s for 30 min to obtain an intumescent fire retardant coating. Example 2
[0056] Add 0.5 parts of chitosan to 13 parts of ethyl acetate, stir until completely dissolved, add 15 parts of ammonium polyphosphate, 0.9 parts of silane coupling agent, and 20 parts of microcapsule wall. Stir in a water bath at a constant temperature of 80°C for 2 hours, cool to room temperature, filter, and dry in an oven at 50°C for 24 hours to obtain a microencapsulated flame retardant. 6 parts of the above-mentioned microencapsulated flame retardant, 20 parts of epoxy resin, 8 parts of waterborne polyurethane and 25 parts of high-purity water are placed in a stainless steel dispersion tank and fully stirred at a speed of 1200 r / s for 30 min, and then 4 parts of ammonium polyphosphate, 2 parts of melamine, 2 parts of dipentaerythritol, 1.5 parts of modified glass fiber, 1.1 parts of hollow ceramic microspheres, 1.2 parts of nano titanium oxide powder, 2 parts of nano magnesium hydroxide powder, 2.5 parts of expandable graphite, 1.5 parts of cellulose, and 1.2 parts of aerogel powder are added to the dispersion tank, and the mixture is dispersed at a speed of 1200 r / s for 40 min to obtain an intumescent fire retardant coating.
[0057] The SEM image of the microencapsulated flame retardant in this embodiment is as follows: Figure 1 As shown in (b); Figure 1 (a) is the SEM image of flame retardant ammonium polyphosphate; Figure 1 It can be seen that ammonium polyphosphate has an irregular cubic structure under an electron microscope, and the coated microencapsulated flame retardant has an ellipsoid structure. It can be seen that the particle size of the coated microencapsulated flame retardant is significantly larger than the flame retardant ammonium polyphosphate. In addition, the surface of the ammonium polyphosphate particles is rough and some surfaces have cracks. Compared with the particles of the microencapsulated flame retardant, the ellipsoid surface is smooth and has no obvious defects. This morphological change further reveals that the flame retardant particles are well covered. Example 3
[0058] Add 2 parts of kraft lignin to 8 parts of aminosilsesquioxane, stir until completely dissolved, add 9 parts of zinc borate, 5 parts of cobalt aluminate, 0.5 parts of silane coupling agent, and 20 parts of microcapsule wall. Stir in a water bath at a constant temperature of 80°C for 24 hours, cool at room temperature and filter, and dry in an oven at 50°C for 24 hours to obtain a microencapsulated flame retardant. 7 parts of the above-mentioned microencapsulated flame retardant, 20 parts of epoxy resin, 10 parts of pure acrylic emulsion and 25 parts of high-purity water are placed in a stainless steel dispersion tank and fully stirred at a speed of 1200 r / s for 30 min, and then 4 parts of ammonium polyphosphate, 3 parts of melamine orthophosphate, 2 parts of pentaerythritol, 1 part of modified alumina fiber, 1.7 parts of hollow fly ash microbeads, 1 part of nano titanium oxide powder, 2 parts of nano magnesium hydroxide powder, 2 parts of expandable graphite, 1.5 parts of cellulose, and 1.5 parts of aerogel powder are added to the dispersion tank, and the mixture is dispersed at a speed of 1200 r / s for 40 min to obtain an intumescent fire retardant coating. Comparative Example 1
[0059] The only difference from Example 3 is that the addition of microcapsule wall is omitted; the remaining steps and parameters are the same as those of Example 1. Comparative Example 2
[0060] The only difference from Example 3 is that the modified alumina fiber is replaced by unmodified alumina fiber.
[0061] The fire retardant coatings prepared in the embodiments and comparative examples were tested for performance according to the national standard CB 12441-2018, and the results are shown in Table 1.
[0062] Table 1 Fire retardant coating performance test results , The results in Table 2 show that the fire-retardant coating prepared in the embodiment of the present invention has good adhesion and durability, and can be used as a flame-retardant and thermal-insulating coating for lithium-ion power battery compartments, solving the problems in the prior art that the foaming layer of the thin flame-retardant and thermal-insulating coating is easy to fall off and has poor durability.
[0063] The present invention obtains a high-strength fire-retardant coating material by arranging multiple layers of flame retardant microcapsules (multi-core shell flame retardant microcapsules). The multiple layers of flame retardant microcapsules can absorb a large amount of heat, thereby improving the adhesion and durability of the coating.
[0064] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A fire retardant coating, characterized in that: Calculated by weight, the raw materials include 0.1-30 parts of resin, 0-20 parts of microencapsulated flame retardant, 0-20 parts of modified fiber, 0-20 parts of hollow microspheres, 0.1-30 parts of filling particle material, 0.1-50 parts of flame retardant and 10-50 parts of solvent.
2. The fire retardant coating according to claim 1, characterized in that: The resin is at least one of epoxy resin, solvent-free epoxy resin, unsaturated resin, modified amino resin, polyamide resin, acrylic resin, polyurethane, urea-formaldehyde resin and alkyd resin.
3. The fire retardant coating according to claim 1, characterized in that: The preparation method of the microencapsulated flame retardant comprises the following steps: After adding melamine and formaldehyde solution into water and mixing, adding NaHCO3 solution to adjust the pH to 9-10, then adding tetraethyl orthosilicate and perfluorohexanone to carry out heating reaction in a water bath, and freeze-drying to obtain microcapsule wall; Add chitosan or sulfate lignin to ethyl acetate or aminosilsesquioxane to dissolve, then add 10-50 parts of flame retardant, 0-5 parts of silane coupling agent and 30-50 parts of microcapsule wall to react, and dry the reaction product to constant weight to obtain the microencapsulated flame retardant; The flame retardant is the same as the flame retardant in claim 1.
4. The fire retardant coating according to claim 1, characterized in that: The modified fiber is at least one of modified aluminum silicate fiber, glass fiber, quartz fiber, mullite fiber, alumina fiber or basalt fiber.
5. The fire retardant coating according to claim 1, characterized in that: The hollow microspheres are at least one of ceramic microspheres, glass microspheres, fly ash microspheres, zirconium oxide microspheres, and silicon oxide microspheres.
6. The fire retardant coating according to claim 1, characterized in that: The filling particle material is at least one of glass powder, graphite powder, pearl powder, shell powder, mica powder, alumina powder, magnesium oxide powder, nano titanium oxide powder, nano magnesium hydroxide powder, montmorillonite, kaolin, bentonite, expandable graphite, cellulose, and aerogel powder.
7. The fire retardant coating according to claim 1, characterized in that: The flame retardant is at least one of pentaerythritol phosphate, expandable graphite, melamine, pentaerythritol, dipentaerythritol, tripentaerythritol, zinc borate, cobalt aluminate, starch, glucose, melamine polyphosphate, aluminum dihydrogen phosphate, diammonium hydrogen phosphate, ammonium polyphosphate, ammonium pyrophosphate, melamine orthophosphate, polyethylene glycol, polyphosphoric acid, guanidine phosphate, and guanyl urea phosphate.
8. The fire retardant coating according to claim 1, characterized in that: The solvent is at least one of modified emulsion, waterborne polyurethane, formaldehyde, ethanol, tetraethyl orthosilicate, ethyl acetate, silicone-acrylic emulsion, pure acrylic emulsion, styrene-acrylic emulsion, high-purity water, and deionized water.
9. A method for preparing a fire retardant coating according to any one of claims 1 to 8, characterized in that: The raw materials are mixed uniformly according to their mass fractions to obtain the fire retardant coating.
10. Use of the fire retardant coating as claimed in claim 9 in lithium-ion power batteries.
Citation Information
Patent Citations
Expansible fire retardant having double-layer core-shell structure, and preparation method and application thereof
CN102408897A
Phosphaphenanthrene compound 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) grafted and modified sepiolite fibers and preparation method thereof
CN103980736A
Environment-friendly fireproof coating and preparation method thereof
CN114736554A
Composite fireproof coating and preparation method thereof
CN116396656A
Fireproof coating and preparation method thereof
CN116589903A
Cited By
High-reflection environment-friendly self-cleaning coating for tunnel and preparation method thereof
CN119350960A
Water-based fireproof coating and preparation process thereof
CN121379278A
High-shielding-property flame-retardant fire-resistant control cable and preparation method thereof
CN121662500A
Flame-retardant heat-insulating coating for battery compartment and preparation method of flame-retardant heat-insulating coating
CN121736623A
Fireproof and heat-insulating nano ceramic coating for lithium battery and preparation method of fireproof and heat-insulating nano ceramic coating
CN121950144A