Preparation method of super-hydrophobic coating

By adjusting the addition ratio of epoxy resin/hydrophobic silica and the electrochemical method, the polyaniline superhydrophobic coating was prepared, which solved the problem of superhydrophobic surface roughness control, achieved excellent anti-corrosion, mechanical and thermal properties, and simplified process and reduces costs, making it suitable for mass production.

CN118791965AActive Publication Date: 2024-10-18NORTH PAINT & COATINGS IND RES & DESIGN INS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410805025.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-18
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

Existing superhydrophobic surface materials have complex preparation methods, high process requirements, difficulty in mass production, and low stability in use. In particular, it is difficult to achieve precise control of superhydrophobic surface roughness at the molecular scale, which limits their application potential.

Method used

By adjusting the addition ratio of epoxy resin/hydrophobic silica and combining electrochemical methods to prepare polyaniline superhydrophobic coatings, the superhydrophobic surface roughness can be precisely controlled to form a new superhydrophobic coating with excellent anti-corrosion, mechanical and heat-resistant properties. layer.

Benefits of technology

It achieves precise molecular-scale control of superhydrophobic surface roughness, improves the anti-corrosion, mechanical and thermal properties of the coating, simplifies the preparation process, reduces costs, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004904420900000041
    Figure BDA0004904420900000041
  • Figure BDA0004904420900000051
    Figure BDA0004904420900000051
Patent Text Reader

Abstract

The invention discloses a preparation method of a super-hydrophobic coating. The preparation method comprises the following steps: firstly, preparing an inner-layer cured polyaniline coating from 0.5 mol / L aniline, 0.1 mol / L phytic acid, 0.2 mol / L sulfuric acid and nickel acetate by adopting a three-electrode electrochemical working system; then, absolute ethyl alcohol, distilled water, dodecyl trimethoxy silane, hexadecyl trimethoxy silane, 3-aminopropyltriethoxysilane, epoxy resin E51 and hydrophobic silicon dioxide are adopted for preparing an outer layer curing polyaniline coating; and finally, curing at normal temperature to obtain the novel polyaniline super-hydrophobic coating with excellent corrosion resistance, mechanical property and heat resistance. The surface roughness of the super-hydrophobic coating is more accurately controlled by adjusting the adding proportion of the epoxy resin and the hydrophobic silicon dioxide, accurate control over the surface roughness of the super-hydrophobic coating on the molecular scale is achieved, and meanwhile the super-hydrophobic coating has good corrosion resistance and adhesive force. Raw materials are easy to obtain, no environment-friendly reagent exists, curing conditions are simple, and other reagents do not need to be added.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive coatings, and particularly relates to a method for preparing a super-hydrophobic coating. Background Art

[0002] Inspired by the super-hydrophobic phenomenon represented by the "lotus effect", the super-hydrophobic material preparation technology has developed rapidly over the past few decades. Due to the special wettability of the super-hydrophobic surface, water droplets are difficult to adhere to its surface, so the super-hydrophobic surface has huge application potential in waterproofing, anti-fog, anti-freezing, self-cleaning, anti-biological pollution, drug delivery, reducing fluid transport resistance, corrosion resistance, batteries and oil-water separation fields, but the current research on super-hydrophobic surface materials still has some shortcomings, such as complex preparation methods, high process requirements, batch production has difficulties and low stability in use, causing extensive attention from the scientific and industrial communities. At present, researchers have used a variety of measures to develop super-hydrophobic coatings, such as chemical etching, laser etching, template etching, anodizing, self-assembly, phase separation and sol-gel methods. A large number of improvements have been made from aspects such as preparation schemes and hydrophobic effects, in order to obtain a durable super-hydrophobic coating that is low in cost, simple to prepare and can be put into large-scale use.

[0003] Existing technologies cannot achieve precise control of superhydrophobic surface roughness at the molecular scale, which is not conducive to further improving the superhydrophobic theoretical model. Summary of the invention

[0004] The purpose of the present invention is to prepare a novel polyaniline super-hydrophobic coating having excellent anti-corrosion performance, mechanical properties and heat resistance, and to more accurately control the surface roughness of the super-hydrophobic coating by adjusting the addition ratio of epoxy resin / hydrophobic silica, so as to achieve precise control of the super-hydrophobic surface roughness at the molecular scale.

[0005] A method for preparing a super-hydrophobic coating comprises the following steps:

[0006] (1) Preparation of phytic acid-doped aniline tempered film matrix for inner layer curing

[0007] An electrolyte is prepared in a 25 mL beaker using a three-electrode electrochemical workstation working system, wherein the electrolyte contains 0.5 mol / L aniline, 0.1 mol / L phytic acid and 0.2 mol / L sulfuric acid, and nickel acetate is added to the electrolyte; a cyclic voltammetry (CV) method is used with a potential range of -0.2 V to 1.1 V and a scanning rate of 20 mV / s for 20 to 30 cycles; after the polymerization is completed, anhydrous ethanol is used to rinse the surface oligomers of the polyaniline, and the temperature of the blast oven is adjusted to 60 to 65° C. and dried for 10 to 12 hours to obtain an inner layer of cured polyaniline coating;

[0008] (2) Preparation of epoxy resin / hydrophobic silica film for outer layer curing

[0009] In a 100 ml three-necked flask, anhydrous ethanol, distilled water, dodecyltrimethoxysilane, hexadecyltrimethoxysilane and 3-aminopropyltriethoxysilane are added respectively, heated and stirred at 60-70° C. to fully dissolve, and heated in an oil bath for reaction for 4-6 hours at a reaction temperature of 60-70° C.; after the reaction is completed, epoxy resin E51 is added, and after reacting for 1-2 hours, hydrophobic silica is added, and then sprayed on the inner layer cured polyaniline coating prepared in (1) to obtain an outer layer cured polyaniline coating;

[0010] (3) Preparation of a novel polyaniline superhydrophobic coating with excellent anti-corrosion, mechanical and thermal properties

[0011] The outer layer cured polyaniline coating prepared in (2) was cured at room temperature for 12 hours to obtain a novel polyaniline super-hydrophobic coating with excellent anti-corrosion, mechanical and thermal properties.

[0012] Specific formula and process of the method:

[0013] Raw material name Specification Mass fraction / % Anhydrous ethanol Analytical grade 69.2~76.7 Distilled water Chemically pure 3.8~4.2 Hexadecyltrimethoxysilane Analytical grade 6.1~6.5 3-Aminopropyltriethoxysilane Analytical grade 1.2~2.3 Dodecyltrimethoxysilane Analytical grade 2.0~3.3 Nickel acetate Analytical grade 2.7~3.0 Epoxy resin E51 Analytical grade 1.7~2.3 Hydrophobic Silica Chemically pure 4.8~9.6

[0014] The three-electrode electrochemical workstation working system adopts a counter electrode of platinum wire, a reference electrode of calomel electrode, and a working electrode of a pre-treated metal sheet, and the working electrode is a SS304 stainless steel sheet polished with sandpaper.

[0015] The mass ratio of the epoxy resin E51 to the hydrophobic silica is 3:1 to 4:1; by adjusting the addition ratio of the epoxy resin / hydrophobic silica, the surface roughness of the super-hydrophobic coating can be more accurately controlled, thereby achieving precise control of the super-hydrophobic surface roughness at the molecular scale.

[0016] Beneficial Effects

[0017] (1) In the method provided by the present invention, polyaniline can form a metal passivation layer, trigger the metal / polyaniline interlayer electric field effect and construct a hydrophobic adsorption layer. Its synthesized reactant has low toxicity, scratch resistance and pitting resistance, and can also induce the passivation behavior between the coating and the metal oxide layer, which can protect the metal from further corrosion. In addition, the electrochemical CV method is used to prepare a novel polyaniline super-hydrophobic coating, by adjusting the ratio of epoxy resin / hydrophobic silica, and hydrophobic modification is carried out to silicon dioxide nanoparticles, the interface between silicon dioxide nanoparticles and epoxy resin is improved, and the surface roughness of the super-hydrophobic coating can be more accurately controlled.

[0018] (2) In the method provided by the present invention, based on the chelation of phytic acid and metal particles, phytic acid can chelate with divalent and higher valence metal ions (such as Cu2+, Zn2+, Fe2+, Fe3+, Al3+, Ca2+, Mg2+, etc.) in a wide pH range to form a stable complex, and can also form a dense chemical conversion film on the surface of metals such as steel, aluminum alloy, magnesium alloy, and copper by chelating with metal surface atoms, thereby slowing down the diffusion rate of corrosive media such as oxygen, Cl-, and H+ to the surface of the metal substrate, and finally playing a role in inhibiting metal corrosion. Moreover, the phytic acid chemical conversion film, because it contains abundant hydroxyl and phosphate groups, can effectively chemically crosslink with the organic coating of the metal coating, improve the adhesion between the metal surface and the outer coating, thereby forming a dense chemical conversion film, so that the new polyaniline super hydrophobic coating has good corrosion resistance and adhesion at the same time.

[0019] (3) In the method provided by the present invention, the raw materials are easily available and there are no environmentally unfriendly reagents. The curing conditions are simple and no other reagents need to be added. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Embodiment 1:

[0022] (1) Preparation of phytic acid-doped aniline tempered film matrix for inner layer curing

[0023] A three-electrode electrochemical workstation working system was used, with a platinum wire as the counter electrode, a calomel electrode as the reference electrode, and a sandpaper-polished SS304 stainless steel sheet as the working electrode. In a 25mL beaker, the electrolyte was 0.5mol / L aniline, 0.1mol / L phytic acid, and 0.2mol / L sulfuric acid, and 0.85g nickel acetate was added to the beaker of 25ml electrolyte. Cyclic voltammetry (CV) was performed within -0.2V-1.1V, and 20 cycles were scanned at a rate of 20mV / s. After the polymerization was completed, the surface oligomers of polyaniline were rinsed clean with anhydrous ethanol, and the temperature of the blast oven was adjusted to 60℃ for drying for 12 hours to obtain an inner layer of cured polyaniline coating.

[0024] (2) Preparation of epoxy resin / hydrophobic silica film for outer layer curing

[0025] In a 100 ml three-necked flask, 25 ml of ethanol, 1 ml of distilled water, 0.65 g of dodecyltrimethoxysilane, 1.95 g of hexadecyltrimethoxysilane and 0.45 g of 3-aminopropyltriethoxysilane were added respectively, heated and stirred at 60° C. to fully dissolve, and heated in an oil bath for 4 h at a reaction temperature of 60° C. After the reaction, 0.65 g of epoxy resin E51 was added, and 1.40 g of hydrophobic silica was added after 1 h, and the inner layer of cured polyaniline coating prepared in (1) was coated by spraying to obtain an outer layer of cured polyaniline coating.

[0026] (3) Preparation of a novel polyaniline superhydrophobic coating with excellent anti-corrosion, mechanical and thermal properties

[0027] The outer layer cured polyaniline coating prepared in (2) was cured at room temperature for 12 hours to obtain a novel polyaniline super-hydrophobic coating with excellent anti-corrosion, mechanical and thermal properties.

[0028] The test performance is as follows:

[0029]

[0030] Embodiment 2:

[0031] (1) Preparation of phytic acid-doped aniline tempered film matrix for inner layer curing

[0032] A three-electrode electrochemical workstation working system was used, with a platinum wire as the counter electrode, a calomel electrode as the reference electrode, and a sandpaper-polished SS304 stainless steel sheet as the working electrode. In a 25mL beaker, the electrolyte was 0.5mol / L aniline, 0.1mol / L phytic acid, and 0.2mol / L sulfuric acid, and 0.98g nickel acetate was added to the beaker of 25ml electrolyte. Cyclic voltammetry (CV) was performed within -0.2V-1.1V, and 20 cycles were scanned at a rate of 20mV / s. After the polymerization was completed, the surface oligomers of polyaniline were rinsed clean with anhydrous ethanol, and the temperature of the forced air oven was adjusted to 60℃ for drying for 12 hours to obtain an inner layer of cured polyaniline coating.

[0033] (2) Preparation of epoxy resin / hydrophobic silica film for outer layer curing

[0034] In a 100 ml three-necked flask, 25 ml of ethanol, 1 ml of distilled water, 0.88 g of dodecyltrimethoxysilane, 2.15 g of hexadecyltrimethoxysilane and 0.55 g of 3-aminopropyltriethoxysilane were added respectively, heated and stirred at 60° C. to fully dissolve, and heated in an oil bath for 4 h at a reaction temperature of 60° C. After the reaction, 0.85 epoxy resin E51 was added, and 2.25 g of hydrophobic silica was added after 1 h, and the inner layer of cured polyaniline coating prepared in (1) was coated by spraying to obtain an outer layer of cured polyaniline coating.

[0035] (3) Preparation of a novel polyaniline superhydrophobic coating with excellent anti-corrosion, mechanical and thermal properties

[0036] The outer layer cured polyaniline coating prepared in (2) was cured at room temperature for 12 hours to obtain a novel polyaniline super-hydrophobic coating with excellent anti-corrosion, mechanical and thermal properties.

[0037] The test performance is as follows:

[0038]

[0039] The present disclosure has been described by the above-mentioned relevant embodiments, but the above-mentioned embodiments are only examples for implementing the present disclosure. It must be pointed out that the disclosed embodiments do not limit the scope of the present disclosure. On the contrary, changes and modifications made without departing from the spirit and scope of the present disclosure are all within the scope of patent protection of the present disclosure.

Claims

1. A method for preparing a super hydrophobic coating, characterized in that: The following steps are involved: (1) Preparation of inner layer cured polyaniline coating: An electrolyte is prepared in a 25 mL beaker using a three-electrode electrochemical workstation working system, wherein the electrolyte contains 0.5 mol / L aniline, 0.1 mol / L phytic acid and 0.2 mol / L sulfuric acid, and 0.8 g to 1.0 g nickel acetate is added; a cyclic voltammetry method is used with a potential range of -0.2 V to 1.1 V and a scanning rate of 20 mV / s for 20 to 30 cycles; after the polymerization is completed, anhydrous ethanol is used to rinse the surface oligomers of the polyaniline, and the temperature of the blast oven is adjusted to 60 to 65° C. and dried for 10 to 12 hours to obtain an inner layer of cured polyaniline coating; (2) Preparation of outer cured polyaniline coating In a 100 ml three-necked flask, anhydrous ethanol, distilled water, dodecyltrimethoxysilane, hexadecyltrimethoxysilane and 3-aminopropyltriethoxysilane are added respectively, heated and stirred at 60-70° C. to fully dissolve, and heated in an oil bath for reaction for 4-6 hours at a reaction temperature of 60-70° C.; after the reaction is completed, epoxy resin E51 is added, and after reacting for 1-2 hours, hydrophobic silica is added, and then sprayed on the inner layer cured polyaniline coating prepared in (1) to obtain an outer layer cured polyaniline coating; (3) Preparation of polyaniline superhydrophobic coating The outer layer of the cured polyaniline coating prepared in (2) is cured to obtain a super hydrophobic coating; Calculated by mass percentage, the following ingredients include 69.2-76.7% anhydrous ethanol, 3.8-4.2% distilled water, 6.1-6.5% hexadecyltrimethoxysilane, 1.2-2.3% 3-aminopropyltriethoxysilane, 2.0-3.3% dodecyltrimethoxysilane, 2.7-3.0% nickel acetate, 1.7-2.3% epoxy resin E51, and 4.8-9.6% hydrophobic silica.

2. The method for preparing a super hydrophobic coating according to claim 1, wherein: The three-electrode electrochemical workstation working system adopts a counter electrode that is a platinum wire, a reference electrode that is a calomel electrode, and a working electrode that is a pre-treated metal sheet.

3. The preparation method of super hydrophobic coating according to claim 1, characterized in that: The mass ratio of the epoxy resin E51 to the hydrophobic silica is 3:1 to 4:

1.

4. The method for preparing a super hydrophobic coating according to claim 2, wherein: The working electrode is a SS304 stainless steel sheet polished with sandpaper.

5. The method for preparing a super hydrophobic coating according to claim 1, wherein: The distilled water, hexadecyltrimethoxysilane, 3-aminopropyltriethoxysilane, dodecyltrimethoxysilane, nickel acetate, and epoxy resin E51 are of chemical purity; and the anhydrous ethanol and hydrophobic silica are of analytical purity.

6. The method for preparing a super hydrophobic coating according to claim 1, wherein: The curing condition of step (3) is curing at room temperature for 12 hours.

Citation Information

Patent Citations

  • Method for preparing functional cotton fabric by divalent nickel ion complex phytic acid

    CN105603734A

  • Phytic acid-doped polyaniline / polyphenylene sulfone coating composition and preparation method thereof

    CN110684462A

  • Preparation method and application of conductive polysiloxane-polyaniline anticorrosive coating

    CN112625484A

  • Epoxy nano composite material modified based on layered nickel silicate coated polyaniline composite nanofibers and preparation method thereof

    CN112831155A

  • Phytic acid doped carbon nitride-polyaniline nano composite material and preparation method thereof as well as intumescent fire retardant coating and preparation method thereof

    CN114409897A