Composition, inner cavity coating as well as preparation method and application of inner cavity coating
By using a combination of silicone, antibacterial agents and cross-linking assistants in the inner cavity coating, the problems of poor antibacterial performance and insufficient durability of the inner cavity coating material are solved, and high temperature, water boiling and water vapor are achieved. The improved performance extends equipment service life and improves food safety.
Patent Information
- Application Number
- CN202310387547.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-18
AI Technical Summary
The existing inner cavity coating materials cannot meet the antibacterial requirements, and have insufficient resistance to high temperatures, boiling water, and water vapor. They are easily contaminated by microorganisms during idle processes, and have weak binding force with the substrate, causing the coating to fall off and cannot be used for long periods of time. Time to resist high temperature steam erosion.
Using a composition including 10-70 parts by weight of silicone resin, 0.001-30 parts by weight of antibacterial agents and 0.5-45 parts by weight of cross-linking assistants, the inner cavity coating is formed with excellent resistance to It is resistant to high temperatures, boiling and water vapor, and effectively prevents high-temperature oxidation and corrosion of the substrate, while also having excellent antibacterial properties.
The inner cavity coating has an E. coli antibacterial rate of ≥99.99%, a Staphylococcus aureus antibacterial rate of ≥99.99%, a high temperature resistance of ≥300°C, a boiling resistance of ≥30 hours, and a water vapor resistance of ≥20 hours, extending the service life of the micro-baking equipment. , and meet consumers’ food safety needs.
Smart Images

Figure BDA0004174608700000091 
Figure BDA0004174608700000101 
Figure HDA0004174608710000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of kitchen appliance materials, and in particular relates to a composition, an inner cavity coating, and a preparation method and application thereof. Background Art
[0002] With the improvement of living standards, people have higher and higher requirements for food safety. Ensuring food safety is a basic requirement for cooking kitchen appliances and is also the focus of consumers' attention when purchasing products. Although microwave ovens, steam ovens, ovens and other microwave ovens can kill microorganisms in food through high-temperature cooking, during the idle period of microwave ovens, microorganisms may colonize in the oily areas of the inner cavity coating to form biofilms, causing potential risks. Therefore, controlling the microbial contamination of the inner cavity coating of microwave ovens during the idle period after use has become an important part of ensuring food safety. Currently, existing inner cavity coating materials cannot meet the antibacterial needs.
[0003] In addition, the bonding force between the existing inner cavity coating and the substrate is weak. After long-term use, the inner cavity coating is easy to fall off from the substrate, resulting in failure of the inner cavity coating, which makes it difficult for the existing inner cavity coating to resist the erosion of high-temperature steam for a long time. In the prior art, there is no inner cavity coating material that can simultaneously be resistant to high temperature, boiling water, and water vapor and has excellent antibacterial properties. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the purpose of the present invention is to provide a composition, an inner cavity coating and a preparation method and application thereof. The inner cavity coating formed by the composition system of the present invention not only has relatively excellent high temperature resistance, boiling resistance and water vapor resistance, but also can effectively prevent the substrate from high temperature oxidation and corrosion; at the same time, the inner cavity coating formed by the composition system also has excellent antibacterial properties.
[0005] In one aspect of the present invention, the present invention provides a composition. According to an embodiment of the present invention, the composition is used to prepare an inner cavity coating, and the composition comprises: 10-70 parts by weight of silicone resin, 0.001-30 parts by weight of antibacterial agent, 0.5-45 parts by weight of cross-linking auxiliary agent and 18-70 parts by weight of solvent.
[0006] According to the composition of the embodiment of the present invention, the inner cavity coating formed by the composition system not only has excellent high temperature resistance, boiling resistance and water vapor resistance, but also can effectively prevent high temperature oxidation and corrosion of the substrate; at the same time, the inner cavity coating formed by the composition system also has excellent antibacterial properties.
[0007] In addition, the composition according to the above embodiment of the present invention may also have the following additional technical features:
[0008] In some embodiments of the present invention, the composition comprises: 15-50 parts by weight of the silicone resin, 0.02-18 parts by weight of the antibacterial agent, 0.5-30 parts by weight of the cross-linking auxiliary agent and 30-65 parts by weight of the solvent.
[0009] In some embodiments of the present invention, the antimicrobial agent includes at least one of an inorganic antimicrobial agent, an organic antimicrobial agent, and a natural antimicrobial agent.
[0010] In some embodiments of the present invention, the inorganic antibacterial agent includes at least one of silver ion antibacterial agent, copper ion antibacterial agent, zinc ion antibacterial agent, diammonium phosphate antibacterial agent, lithium carbonate antibacterial agent, and graphene antibacterial agent; and / or, the organic antibacterial agent includes at least one of vanillin antibacterial agent, acylanilide antibacterial agent, imidazole antibacterial agent, thiazole antibacterial agent, isothiazolone derivative antibacterial agent, quaternary ammonium salt antibacterial agent, bis-quat antibacterial agent, and phenolic antibacterial agent; and / or, the natural antibacterial agent includes at least one of chitosan, mustard, castor oil, and horseradish.
[0011] In some embodiments of the present invention, the silicone resin includes at least one of methylphenyl silicone resin, methyl silicone resin, low phenylmethyl silicone resin, epoxy-modified silicone resin, silicone polyester-modified resin, benzyl transparent silicone resin, methyl transparent silicone resin, mica bonding silicone resin, polymethyl silicone resin, amino silicone resin, fluorosilicone resin, silicone resin solution, silicone-epoxy resin, and silicone polyester resin.
[0012] In some embodiments of the present invention, the crosslinking aid includes at least one of a polycarbodiimide crosslinking aid, an acrylate crosslinking aid, an organic peroxide crosslinking aid, a polyamine crosslinking aid, a polyol crosslinking aid, a glycidyl ether crosslinking aid, a silicone crosslinking aid, a benzenesulfonic acid crosslinking aid, an aziridine crosslinking aid, an olefin monomer crosslinking aid and an inorganic crosslinking aid.
[0013] In some embodiments of the present invention, the polyamine crosslinking aid includes at least one of propylene diamine and MOCA; and / or, the polyol crosslinking aid includes at least one of polyethylene glycol, polypropylene glycol, trimethylolpropane, and trimethylolethane; and / or, the inorganic crosslinking aid includes at least one of zinc oxide, aluminum chloride, and aluminum sulfate; and / or, the silicone crosslinking aid includes at least one of tetraethyl orthosilicate, methyl orthosilicate, and trimethoxysilane; and / or, the benzenesulfonic acid crosslinking aid includes at least one of p-toluenesulfonic acid and p-toluenesulfonyl chloride; and / or, the acrylate The crosslinking aid of the type includes at least one of 1,4-butylene glycol diacrylate, ethylene glycol dimethacrylate, TAC, butyl acrylate, HEA, HPA, HEMA, HPMA and MMA; and / or, the organic peroxide crosslinking aid includes at least one of dicumyl peroxide and bis-2,4-dichlorobenzoyl peroxide; and / or, the olefin monomer crosslinking aid includes at least one of acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, hydroxypropyl methacrylate, divinylbenzene, N-hydroxymethyl acrylamide and diacetone acrylamide.
[0014] In some embodiments of the present invention, the solvent includes at least one of an alkane solvent, an ether solvent, a ketone solvent, and a benzene-derived biosolvent.
[0015] In another aspect of the present invention, the present invention provides an inner cavity coating. According to an embodiment of the present invention, the inner cavity coating is prepared using the composition described in the above embodiment. As a result, the inner cavity coating has relatively excellent high temperature resistance, boiling resistance and water vapor resistance, and can also effectively prevent the substrate from high temperature oxidation and corrosion; at the same time, the inner cavity coating also has excellent antibacterial properties.
[0016] In a third aspect of the present invention, the present invention provides a method for preparing the above-mentioned inner cavity coating. According to an embodiment of the present invention, the method comprises:
[0017] (1) mixing a silicone resin, an antibacterial agent, a cross-linking aid and a solvent to form a coating solution;
[0018] (2) The coating liquid is formed on a substrate and heat-treated to form the inner cavity coating on the substrate.
[0019] According to the method for preparing the inner cavity coating of the embodiment of the present invention, the inner cavity coating prepared by the method has relatively excellent high temperature resistance, boiling resistance and water vapor resistance, and can also effectively prevent the substrate from high temperature oxidation and corrosion; at the same time, it also has excellent antibacterial properties. The preparation method is simple in steps and easy to operate.
[0020] In addition, the method for preparing the inner cavity coating according to the above embodiment of the present invention may also have the following additional technical features:
[0021] In some embodiments of the present invention, step (1) includes: (1-1) mixing the silicone resin with the solvent to form a first mixed liquid; (1-2) mixing the first mixed liquid with the cross-linking aid to form a second mixed liquid; (1-3) mixing the second mixed liquid with the antibacterial agent to form the coating liquid.
[0022] In some embodiments of the present invention, the temperature of the heat treatment is 25°C-450°C.
[0023] In a fourth aspect of the present invention, the present invention provides a micro-baking device. According to an embodiment of the present invention, the micro-baking device has an inner cavity coating of the above embodiment or an inner cavity coating prepared by the method described in the above embodiment. Therefore, the micro-baking device has all the advantages of the inner cavity coating of the above embodiment. Specifically, the inner cavity of the micro-baking device has excellent high temperature resistance, boiling resistance and water vapor resistance, thereby extending the service life of the micro-baking device. At the same time, it also has excellent antibacterial properties, further meeting the needs of consumers.
[0024] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0026] Figure 1 The figure is a schematic flow chart of a method for preparing an inner cavity coating according to an embodiment of the present invention. DETAILED DESCRIPTION
[0027] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0028] In one aspect of the present invention, the present invention provides a composition. According to an embodiment of the present invention, the composition is used to prepare an inner cavity coating, and the composition includes: 10-70 parts by weight of silicone resin (e.g., 10 / 15 / 20 / 30 / 40 / 50 / 60 / 70 parts by weight), 0.001-30 parts by weight of antibacterial agent (e.g., 1 / 3 / 5 / 10 / 15 / 18 / 20 / 25 / 30 parts by weight), 0.5-45 parts by weight of cross-linking auxiliary agent (e.g., 1 / 5 / 10 / 15 / 20 / 25 / 30 / 35 / 40 / 45 parts by weight), and 18-70 parts by weight of solvent (e.g., 18 / 20 / 30 / 40 / 50 / 60 / 65 / 70 parts by weight). Therefore, the inner cavity coating formed by the composition system not only has excellent high temperature resistance, boiling resistance and water vapor resistance, but also can effectively prevent high temperature oxidation and corrosion of the substrate; at the same time, the inner cavity coating formed by the composition system also has excellent antibacterial properties.
[0029] The principle by which the inner cavity coating proposed by the present invention can achieve the above beneficial effects is described in detail below:
[0030] In the prior art, the inner cavity coating of microwave ovens, steam-bake-in-one machines, ovens and other microwave-baking products has the following disadvantages: 1) poor antibacterial performance; 2) poor high temperature resistance, yellowing and cracking after baking in a 300°C environment for 1 hour; 3) poor water boiling resistance, whitening in a short period of time (30 minutes or more) or even falling off from the substrate; 4) poor water vapor resistance, whitening in a short period of time (30 minutes or more) or even falling off from the substrate. In order to solve the above problems, the present invention provides a composition for preparing an inner cavity coating, the composition comprising 10-70 parts by weight of silicone resin, 0.001-30 parts by weight of antibacterial agent, 0.5-45 parts by weight of cross-linking auxiliary agent and 18-70 parts by weight of solvent. Silicone resin is a thermosetting polysiloxane polymer with a highly cross-linked structure, which has excellent electrical insulation, heat resistance and water resistance, and silicone resin has good adhesion to iron, aluminum, silver, tin, glass and ceramics. The inventors added a cross-linking aid and an antibacterial agent to the silicone resin to cause a cross-linking reaction in the entire system, which not only makes the inner cavity coating formed by the composition system have excellent high temperature resistance, water boiling resistance and water vapor resistance, but also effectively prevents the substrate from high temperature oxidation and corrosion; at the same time, the inner cavity coating formed by the composition system has excellent antibacterial properties. Specifically, the inner cavity coating formed by the composition system has an antibacterial rate of ≥99.99% for Escherichia coli, ≥99.99% for Staphylococcus aureus, high temperature resistance ≥300°C, water boiling resistance ≥30 hours, and water vapor resistance ≥20 hours.
[0031] The inventors found that if the content of the antibacterial agent is too low, it is impossible to effectively ensure that the inner cavity coating formed by the composition system has excellent antibacterial properties. If the content of the antibacterial agent is too high, the boiling resistance and water vapor resistance of the inner cavity coating formed by the composition system will decrease. If the content of the cross-linking auxiliary agent is too low, it will not be possible to ensure the cross-linking effect of the entire system, thereby causing the antibacterial properties, boiling resistance and water vapor resistance of the inner cavity coating formed by the composition system to decrease. If the content of the cross-linking auxiliary agent is too high, the leveling of the inner cavity coating formed by the composition system will deteriorate (for example, problems such as pinholes and orange peels will occur).
[0032] According to some specific embodiments of the present invention, the composition includes: 15-50 parts by weight of silicone resin, 0.02-18 parts by weight of antibacterial agent, 0.5-30 parts by weight of cross-linking aid and 30-65 parts by weight of solvent. By limiting the content of each component within the above range, the high temperature resistance, boiling resistance and water vapor resistance of the inner cavity coating formed by the composition system are further improved, and high temperature oxidation and corrosion of the substrate are further effectively prevented; at the same time, the antibacterial property of the inner cavity coating formed by the composition system is further improved.
[0033] In the embodiments of the present invention, the specific types of the above-mentioned silicone resins are not particularly limited, and those skilled in the art can flexibly select according to actual needs. As some specific examples, the silicone resin includes at least one of methylphenyl silicone resin, methyl silicone resin, epoxy-modified silicone resin, silicone polyester-modified resin, benzyl transparent silicone resin, mica bonding silicone resin, amino silicone resin, fluorosilicone resin, silicone-epoxy resin, and silicone polyester resin. It should be noted that the performance of silicone resin is also closely related to the type of organic group R on the silicone resin. When the organic group is -CH3, the thermal stability, hydrophobicity, demolding property and arc resistance of the silicone resin can be improved; when the organic group is -C6H5, the oxidative stability and thermal stability of the silicone resin can be improved; when the organic group is -CH=CH2, the curing performance of the silicone resin can be improved and the coupling property can be imparted; when the organic group is phenyl or ethyl, the miscibility of the silicone resin with organic matter can be improved; when the organic group is -NH2(CH2), the water solubility of the polymer can be improved and the coupling property can be imparted at the same time; when the organic group is a long-chain alkyl group, the hydrophobicity of the silicone resin can be improved.
[0034] In the embodiments of the present invention, the specific types of the above-mentioned antibacterial agents are not particularly limited, and those skilled in the art can flexibly select according to actual needs. As some specific examples, the antibacterial agent includes at least one of an inorganic antibacterial agent, an organic antibacterial agent, and a natural antibacterial agent. Among them, the specific types of inorganic antibacterial agents are not particularly limited. For example, inorganic antibacterial agents include at least one of silver ion antibacterial agents, copper ion antibacterial agents, zinc ion antibacterial agents, diammonium phosphate antibacterial agents, lithium carbonate antibacterial agents, and graphene antibacterial agents. The specific types of organic antibacterial agents are not particularly limited. For example, organic antibacterial agents include at least one of vanillin antibacterial agents, acylanilide antibacterial agents, imidazole antibacterial agents, thiazole antibacterial agents, isothiazolone derivative antibacterial agents, quaternary ammonium salt antibacterial agents, biguanide antibacterial agents, and phenolic antibacterial agents. The specific types of natural antibacterial agents are not particularly limited. For example, natural antibacterial agents include at least one of chitosan, mustard, castor oil, and horseradish. The above-mentioned antibacterial agents are added to the silicone resin system, so that the inner cavity coating formed by the system has excellent antibacterial properties, with an antibacterial rate of ≥99.99% against Escherichia coli and an antibacterial rate of ≥99.99% against Staphylococcus aureus.
[0035] In the embodiments of the present invention, the specific types of the above cross-linking aids are not particularly limited, and those skilled in the art can flexibly select according to actual needs. As some specific examples, the cross-linking aids include at least one of polycarbodiimide cross-linking aids, acrylate cross-linking aids, organic peroxide cross-linking aids, polyamine cross-linking aids, polyol cross-linking aids, glycidyl ether cross-linking aids, silicone cross-linking aids, benzenesulfonic acid cross-linking aids, aziridine cross-linking aids, olefin monomer cross-linking aids and inorganic cross-linking aids. Among them, the specific types of polyamine cross-linking aids are not particularly limited, for example, the polyamine cross-linking aids include at least one of propylene diamine and MOCA. The specific types of polyol cross-linking aids are not particularly limited, for example, the polyol cross-linking aids include at least one of polyethylene glycol, polypropylene glycol, trimethylol propane, and trimethylol ethane. The specific types of inorganic cross-linking aids are not particularly limited, for example, the inorganic cross-linking aids include at least one of zinc oxide, aluminum chloride and aluminum sulfate. The specific types of organosilicon crosslinking aids are not particularly limited. For example, organosilicon crosslinking aids include at least one of ethyl orthosilicate, methyl orthosilicate and trimethoxysilane. The specific types of benzenesulfonic acid crosslinking aids are not particularly limited. For example, benzenesulfonic acid crosslinking aids include at least one of p-toluenesulfonic acid and p-toluenesulfonyl chloride. The specific types of acrylate crosslinking aids are not particularly limited. For example, acrylate crosslinking aids include at least one of dibutylene glycol diacrylate, ethylene glycol dimethacrylate, TAC, butyl acrylate, HEA, HPA, HEMA, HPMA and MMA. The specific types of organic peroxide crosslinking aids are not particularly limited. For example, organic peroxide crosslinking aids include at least one of diisopropylbenzene peroxide and di-2,4-dichlorobenzoyl peroxide. The specific types of vinyl monomer crosslinking aids are not particularly limited. For example, the vinyl monomer crosslinking aids include at least one of acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, hydroxypropyl methacrylate, divinylbenzene, N-hydroxymethyl acrylamide, and diacetone acrylamide.
[0036] In the embodiments of the present invention, the specific types of the above-mentioned solvents are not particularly limited, and those skilled in the art can flexibly select according to actual needs. As some specific examples, the solvent includes at least one of an alkane solvent, an ether solvent, a ketone solvent, and a benzene-derived biological solvent. Among them, the specific types of hydrocarbon solvents are not particularly limited. For example, the alkane solvent includes at least one of n-hexane, n-octane, n-decane, chloroform, dichloromethane, dichloroethylene, and mineral oil. The specific types of ether solvents are not particularly limited. For example, the ether solvent includes at least one of ether, petroleum ether, and dibutyl ether. The specific types of ketone solvents are not particularly limited. For example, the ketone solvent includes at least one of acetone, methyl ethyl ketone, cyclohexanone, and isophorone. The specific types of benzene derivative solvents are not particularly limited. For example, the benzene derivative solvent includes at least one of toluene, m-xylene, p-xylene, o-xylene, and chlorobenzene.
[0037] In another aspect of the present invention, the present invention proposes an inner cavity coating. According to an embodiment of the present invention, the inner cavity coating is prepared using the composition of the above embodiment. As a result, the inner cavity coating has relatively excellent high temperature resistance, boiling resistance and water vapor resistance, and can also effectively prevent high temperature oxidation and corrosion of the substrate; at the same time, the inner cavity coating also has excellent antibacterial properties. Specifically, the inner cavity coating has an antibacterial rate of Escherichia coli ≥ 99.99%, an antibacterial rate of Staphylococcus aureus ≥ 99.99%, high temperature resistance ≥ 300°C, boiling resistance ≥ 30 hours, and water vapor resistance ≥ 20 hours.
[0038] In the third aspect of the present invention, the present invention provides a method for preparing the above-mentioned inner cavity coating. Figure 1 , the method comprising:
[0039] S100: Silicone resin, antimicrobial agent, cross-linking aid and solvent are mixed to form a coating solution.
[0040] According to some specific embodiments of the present invention, step S100 includes the following steps: firstly, the silicone resin and the solvent are fully mixed to form a first mixed solution; then, the cross-linking agent is fully mixed in the first mixed solution to form a second mixed solution; and finally, the antibacterial agent is fully mixed in the second mixed solution to finally form a coating solution. Thus, the components are mixed more fully, and the side reactions that may be caused by the silicone resin and the antibacterial agent first contact are avoided.
[0041] S200: forming a coating liquid on a substrate and performing a heat treatment to form an inner cavity coating on the substrate.
[0042] During the heat treatment process, a cross-linking reaction occurs in the entire system, causing the coating liquid to solidify to form an inner cavity coating. The formed inner cavity coating not only has excellent high temperature resistance, boiling resistance and water vapor resistance, but also can effectively prevent high temperature oxidation and corrosion of the substrate; at the same time, the formed inner cavity coating also has excellent antibacterial properties.
[0043] According to some specific embodiments of the present invention, the temperature of the heat treatment is 25°C-450°C, preferably 150°C-430°C; and the time of the heat treatment is 10 min-30 min.
[0044] According to the method for preparing the above-mentioned inner cavity coating of an embodiment of the present invention, the inner cavity coating prepared by the method has relatively excellent high temperature resistance, boiling resistance and water vapor resistance, and can also effectively prevent high temperature oxidation and corrosion of the substrate; at the same time, it also has excellent antibacterial properties. Specifically, the antibacterial rate of Escherichia coli of the inner cavity coating is ≥99.99%, the antibacterial rate of Staphylococcus aureus is ≥99.99%, the high temperature resistance is ≥300°C, the boiling resistance is ≥30 hours, and the water vapor resistance is ≥20 hours. The preparation method has simple steps and is easy to operate.
[0045] In a fourth aspect of the present invention, the present invention provides a micro-baking device. According to an embodiment of the present invention, the micro-baking device has an inner cavity coating of the above embodiment or an inner cavity coating prepared by the method of the above embodiment. Therefore, the micro-baking device has all the advantages of the inner cavity coating of the above embodiment. Specifically, the inner cavity of the micro-baking device has excellent high temperature resistance, boiling resistance and water vapor resistance, thereby extending the service life of the micro-baking device. At the same time, it also has excellent antibacterial properties, further meeting the needs of consumers.
[0046] Specifically, the microwave oven device may be a microwave oven, a steam-bake-in-one machine, an oven or other types of microwave oven kitchen appliances.
[0047] The embodiments of the present invention are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.
[0048] Example 1
[0049] At room temperature, 47 parts by weight of toluene solvent was added to 32 parts by weight of methylphenyl silicone resin, and the mixture was stirred for 30 minutes to obtain a first solution.
[0050] 15 parts by weight of a cross-linking aid dicumyl peroxide was added to the first solution and stirred evenly to obtain a second solution.
[0051] 10 parts by weight of the silver ion antibacterial agent are added to the second solution, and mixed evenly to obtain a coating solution.
[0052] The coating liquid was evenly sprayed on the surface of the substrate and heat-treated at 200°C for 20 minutes to obtain the antibacterial coating.
[0053] Example 2
[0054] The weight portion of the antibacterial agent in this embodiment is 1 part, and the antibacterial agent used is diammonium phosphate antibacterial agent. Other contents are the same as those in Example 1.
[0055] Example 3
[0056] The weight proportion of the antibacterial agent in this embodiment is 5 parts, and the antibacterial agent used is lithium carbonate antibacterial agent. Other contents are the same as those in Example 1.
[0057] Example 4
[0058] The weight proportion of the antibacterial agent in this embodiment is 15 parts, the antibacterial agent used is a graphene antibacterial agent, and the other contents are the same as those in Embodiment 1.
[0059] Example 5
[0060] The weight proportion of the antibacterial agent in this embodiment is 20 parts, the antibacterial agent used is vanillin, and the other contents are the same as those in Embodiment 1.
[0061] Example 6
[0062] The weight proportion of the crosslinking aid in this embodiment is 3 parts, and the other contents are the same as those in Embodiment 1.
[0063] Example 7
[0064] The weight proportion of the crosslinking aid in this embodiment is 10 parts, and the other contents are the same as those in Embodiment 1.
[0065] Example 8
[0066] The weight proportion of the crosslinking aid in this embodiment is 20 parts, and the other contents are the same as those in Embodiment 1.
[0067] Example 9
[0068] The weight proportion of the crosslinking aid in this embodiment is 30 parts, and the other contents are the same as those in Embodiment 1.
[0069] Example 10
[0070] The silicone resin used in this embodiment is methyl silicone resin, the weight portion of which is 10 parts, the cross-linking auxiliary agent used is propylene diamine, the weight portion of the solvent is 20 parts, the antibacterial agent used is aminophenylimidazole, and the heat treatment is performed at 150°C for 30 minutes. Other contents are the same as in Example 1.
[0071] Embodiment 11
[0072] The silicone resin used in this embodiment is fluorosilicone resin, which has a weight portion of 20 parts, the weight portion of the solvent is 30 parts, the cross-linking auxiliary agent used is polyethylene glycol, the antibacterial agent used is isothiazolinone, and the heat treatment is performed at 430°C for 10 minutes. Other contents are the same as in Example 1.
[0073] Example 12
[0074] The silicone resin used in this embodiment is fluorosilicone resin, and its weight proportion is 40 parts. The weight proportion of the solvent is 40 parts. The cross-linking auxiliary agent used is polyethylene glycol. The antibacterial agent used is a quaternary ammonium salt antibacterial agent. Other contents are the same as those in Example 1.
[0075] Embodiment 13
[0076] The silicone resin used in this embodiment is an organosilicon-epoxy resin, which has a weight portion of 65 parts, the weight portion of the solvent is 70 parts, the cross-linking aid used is 1,4-butylene glycol diacrylate, the antibacterial agent used is chitosan, and the other contents are the same as those in Example 1.
[0077] Comparative Example 1
[0078] No antibacterial agent was added in this comparative example, and other contents were the same as those in Example 1.
[0079] Comparative Example 2
[0080] The weight proportion of the antibacterial agent added in this comparative example is 35 parts, and the other contents are the same as those in Example 1.
[0081] The antibacterial properties, boiling resistance, steam resistance, and temperature resistance of the antibacterial coatings prepared in Examples 1-13 and Comparative Examples 1-2 were tested respectively, and the specific testing methods are as follows:
[0082] Antibacterial performance: The antibacterial coatings prepared in Examples 1-13 and Comparative Examples 1-2 were tested in accordance with the standard "GB 21551.2-2010 Special requirements for antibacterial materials with antibacterial, sterilizing and purification functions for household and similar electrical appliances".
[0083] Water boiling resistance: The coating liquids prepared in Examples 1-13 and Comparative Examples 1-2 were sprayed on the same substrate, and the samples were placed in water boiling vessels after curing. After continuous boiling for 40 hours, if the coating did not fall off and the color difference ⊿E before and after boiling was in the range of 0 to 0.25, the water boiling resistance was excellent; if the coating did not fall off and the color difference ⊿E before and after boiling was in the range of 0.25 to 0.5, the water boiling resistance was good; if the coating did not fall off and the color difference ⊿E before and after boiling was in the range of 0.5 to 1.0, the water boiling resistance was qualified; if the coating fell off, or the coating did not fall off and the color difference ⊿E before and after boiling was in the range of 1.0 to 1.5, the water boiling resistance was unqualified.
[0084] Water vapor resistance: The coating liquids prepared in Examples 1-13 and Comparative Examples 1-2 were sprayed on the same substrate respectively. After curing, the samples were placed in steam vessels and subjected to continuous water vapor for 20 hours. If the coating did not fall off and the color difference ⊿E before and after steaming was in the range of 0 to 0.25, the steam resistance was excellent; if the coating did not fall off and the color difference ⊿E before and after steaming was in the range of 0.25 to 0.5, the steam resistance was good; if the coating did not fall off and the color difference ⊿E before and after steaming was in the range of 0.5 to 1.0, the steam resistance was qualified; if the coating fell off, or the coating did not fall off and the color difference ⊿E before and after steaming was in the range of 1.0 to 1.5, the steam resistance was unqualified.
[0085] Heat resistance: Spray the coating liquids prepared in Examples 1-13 and Comparative Examples 1-2 on the same substrate, respectively. After curing, place the samples in a high-temperature oven, set the temperature to 300°C, keep warm for 6 hours, take out and cool to room temperature, and observe whether there is cracking or discoloration. If the coating has no cracks and the color difference ⊿E before and after the high-temperature test is within the range of 0 to 0.25, the heat resistance is excellent; if the coating has no cracks and the color difference ⊿E before and after the high-temperature test is within the range of 0.25 to 0.5, the heat resistance is good; if the coating has no cracks and the color difference ⊿E before and after the high-temperature test is within the range of 0.5 to 1.0, the heat resistance is qualified; if the coating cracks, or if the coating has no cracks and the color difference ⊿E before and after the high-temperature test is within the range of 1.0 to 1.5, the heat resistance is unqualified.
[0086] The test results are shown in Table 1.
[0087] Table 1
[0088]
[0089]
[0090] As can be seen from Table 1, Examples 1-13 all have excellent antibacterial properties, boiling resistance, steam resistance, and temperature resistance.
[0091] It can also be seen from Table 1 that, compared with Example 1, the antibacterial performance of Comparative Example 1 is poor.
[0092] It can also be seen from Table 1 that, compared with Example 1, the boiling resistance and steam resistance of Comparative Example 2 are relatively poor.
[0093] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0094] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A composition for preparing an inner cavity coating, characterized in that: The composition comprises: 10-70 parts by weight of silicone resin, 0.001-30 parts by weight of antibacterial agent, 0.5-45 parts by weight of cross-linking auxiliary agent and 18-70 parts by weight of solvent.
2. The composition according to claim 1, characterized in that The composition comprises: 15-50 parts by weight of the silicone resin, 0.02-18 parts by weight of the antibacterial agent, 0.5-30 parts by weight of the cross-linking auxiliary agent and 30-65 parts by weight of the solvent.
3. The composition according to claim 1 or 2, characterized in that The antibacterial agent includes at least one of an inorganic antibacterial agent, an organic antibacterial agent, and a natural antibacterial agent.
4. The composition according to claim 3, characterized in that The inorganic antibacterial agent includes at least one of a silver ion antibacterial agent, a copper ion antibacterial agent, a zinc ion antibacterial agent, a diammonium phosphate antibacterial agent, a lithium carbonate antibacterial agent, and a graphene antibacterial agent; And / or, the organic antibacterial agent includes at least one of vanillin antibacterial agents, acylanilide antibacterial agents, imidazole antibacterial agents, thiazole antibacterial agents, isothiazolone derivative antibacterial agents, quaternary ammonium salt antibacterial agents, bis-quat antibacterial agents, and phenolic antibacterial agents; And / or, the natural antibacterial agent includes at least one of chitosan, mustard, castor oil and wasabi.
5. The composition according to claim 1 or 2, characterized in that The silicone resin includes at least one of methylphenyl silicone resin, methyl silicone resin, epoxy-modified silicone resin, silicone polyester-modified resin, benzyl transparent silicone resin, mica bonding silicone resin, amino silicone resin, fluorosilicone resin, silicone-epoxy resin, and silicone polyester resin.
6. The composition according to claim 1 or 2, characterized in that The crosslinking aid includes at least one of a polycarbodiimide crosslinking aid, an acrylate crosslinking aid, an organic peroxide crosslinking aid, a polyamine crosslinking aid, a polyol crosslinking aid, a glycidyl ether crosslinking aid, a silicone crosslinking aid, a benzenesulfonic acid crosslinking aid, an aziridine crosslinking aid, an olefin monomer crosslinking aid and an inorganic crosslinking aid.
7. The composition according to claim 6, characterized in that The polyamine cross-linking aid includes at least one of propylene diamine and MOCA; And / or, the polyol cross-linking aid includes at least one of polyethylene glycol, polypropylene glycol, trimethylolpropane and trimethylolethane; And / or, the inorganic cross-linking aid includes at least one of zinc oxide, aluminum chloride and aluminum sulfate; And / or, the organosilicon cross-linking aid includes at least one of ethyl orthosilicate, methyl orthosilicate and trimethoxysilane; And / or, the benzenesulfonic acid cross-linking aid includes at least one of p-toluenesulfonic acid and p-toluenesulfonyl chloride; and / or, the acrylate crosslinking aid comprises at least one of 1,4-butylene glycol diacrylate, ethylene glycol dimethacrylate, TAC, butyl acrylate, HEA, HPA, HEMA, HPMA and MMA; And / or, the organic peroxide cross-linking aid includes at least one of dicumyl peroxide and bis-2,4-dichlorobenzoyl peroxide; And / or, the vinyl monomer crosslinking aid includes at least one of acrylic acid, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, hydroxypropyl methacrylate, divinylbenzene, N-hydroxymethyl acrylamide, and diacetone acrylamide.
8. The composition according to claim 1 or 2, characterized in that The solvent includes at least one of an alkane solvent, an ether solvent, a ketone solvent and a benzene-derived biosolvent.
9. An inner cavity coating, characterized in that: The composition is prepared by using the composition described in any one of claims 1 to 8.
10. A method for preparing the inner cavity coating according to claim 9, characterized in that: include: (1) mixing a silicone resin, an antibacterial agent, a cross-linking aid and a solvent to form a coating solution; (2) The coating liquid is formed on a substrate and heat-treated to form the inner cavity coating on the substrate.
11. The method according to claim 10, characterized in that Step (1) comprises: (1-1) mixing the silicone resin and the solvent to form a first mixed liquid; (1-2) mixing the first mixed solution with the cross-linking auxiliary agent to form a second mixed solution; (1-3) The second mixed liquid is mixed with the antibacterial agent to form the coating liquid.
12. The method according to claim 10, characterized in that The temperature of the heat treatment is 25°C-450°C.
13. A microwave oven, characterized in that: A cavity coating according to claim 9 or an cavity coating prepared by the method according to any one of claims 10 to 12.
Citation Information
Patent Citations
Antibacterial coating, spraying method thereof and boiling equipment
CN107987653A
Temperature-resistant coating for coiled material household appliances and preparation method thereof
CN109536016A
Self-cleaning paint composition, paint, coating of paint and kitchen electric appliances
CN110373107A
Antimicrobial coating composition and article coated with the same coating composition
JP1994207127A