Water melt adhesive with high bonding strength, preparation method and use method of water melt adhesive and adhesive tape

Through the combination of hydrophobic monomers, hydrophilic monomers and ionic liquids, a hydromelt adhesive with high bonding strength is prepared, combined with water droplet wetting and pressing load, which solves the problem of equipment dependence and limited strength of the adhesive during the bonding process. problem, achieving efficient and convenient bonding effects.

CN118791992APending Publication Date: 2024-10-18THE CHINESE UNIV OF HONG KONG (SHENZHEN)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410776459.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing adhesives have problems with liquid leakage, self-curing, and equipment dependence during the bonding process. Moreover, the bonding strength of tape-type adhesives is limited by interface wettability and bulk strength, making it difficult to use effectively in daily life.

Method used

Using a combination of hydrophobic monomers, hydrophilic monomers, ionic liquids and initiators, water-melt adhesives with high bonding strength are prepared through photo-initiated or thermal-initiated polymerization reactions, combined with the wetting and pressing load of water droplets, to achieve equipment-free Efficient bonding.

Benefits of technology

It has achieved high bonding strength, easy to use, repeatable and recyclable water-melt adhesives and tapes. The bonding strength reaches the level of commercial hot-melt adhesives, and has good universality and ease of operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791992A_ABST
    Figure CN118791992A_ABST
Patent Text Reader

Abstract

The invention provides a water melt adhesive with high bonding strength, a preparation method and a use method thereof, and an adhesive tape, and relates to the field of materials. The water melt adhesive with high bonding strength is prepared from the following raw materials: a hydrophobic monomer, a hydrophilic monomer, ionic liquid and an initiator, the ionic liquid is intermiscible with the hydrophobic monomer and the hydrophilic monomer. The preparation method comprises the following steps: mixing raw materials to obtain precursor liquid; carrying out degassing treatment on the precursor liquid, then carrying out reaction, and then carrying out vacuum drying. The use method comprises the following steps: infiltrating a target base material with water, and then arranging the water melt adhesive with high bonding strength on the surface of the target base material to obtain a bonding assembly; a normal load is applied to the surface of the adhesive assembly. The water melt adhesive has no obvious viscosity in a dry state, and by dropwise adding water on a target base material, attaching an adhesive tape to the target base material and pressing with a small load, the lap joint shear strength of the water melt adhesive on glass can reach 2.9 MPa, which is equivalent to that of the existing commercial hot melt adhesive and is far higher than that of a common adhesive tape type adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of materials, and in particular to a water-melt adhesive with high bonding strength, a preparation method, a use method and an adhesive tape thereof. Background Art

[0002] As one of the most important synthetic polymer materials, adhesives are ubiquitous in engineering and daily life. According to the bonding strategy, adhesives can be divided into two types: glue-type and tape-type. Glue-type adhesives form strong adhesion by solidifying at the interface. Its precursor is a liquid, which is inconvenient to transport and use. It is easy to leak and self-solidify, not suitable for long-term storage and cannot be reused. Tape-type adhesives achieve adhesion by pressing. Its body is a soft solid, and its bonding strength is limited by the wettability of the interface and the strength of the body. To address this problem, the hot-pressed tape / hot-melt adhesive commonly used in industry softens or melts the solid adhesive by heating, and uses an external load to make it fit tightly to the target bonding substrate, forming strong adhesion after cooling. However, this method requires additional auxiliary equipment (such as a hot press) and is not suitable for daily life. Summary of the invention

[0003] The purpose of the present application is to provide a water-melt adhesive with high bonding strength and a preparation method, a use method and an adhesive tape thereof to solve the above-mentioned problems.

[0004] To achieve the above objectives, this application adopts the following technical solutions:

[0005] A water-melt adhesive with high bonding strength, the raw materials of which include: a hydrophobic monomer, a hydrophilic monomer, an ionic liquid and an initiator;

[0006] The ionic liquid is compatible with the hydrophobic monomer and the hydrophilic monomer.

[0007] Preferably, the raw materials meet one or more of the following conditions:

[0008] A. the hydrophobic monomer comprises a hydrophobic acrylate compound and / or a hydrophobic vinyl compound;

[0009] B. The hydrophilic monomer includes one or more of a hydrophilic acrylamide compound, a hydrophilic acrylate compound, a hydrophilic acrylic compound, and a hydrophilic vinyl compound;

[0010] C. The amount of the hydrophobic monomer used accounts for no more than 99% of the total mass of the hydrophobic monomer and the hydrophilic monomer.

[0011] Preferably, the water-melt adhesive with high bonding strength satisfies one or more of the following conditions:

[0012] (1) The hydrophobic acrylic acid ester compound includes one or more of ethyl methacrylate, methyl methacrylate, isopropyl methacrylate, benzyl methacrylate, phenyl methacrylate, isobornyl methacrylate, glycidyl methacrylate, methyl acrylate, cyclohexyl acrylate, and benzyl acrylate;

[0013] (2) The hydrophobic vinyl compound includes styrene;

[0014] (3) The hydrophilic acrylamide compound includes one or more of diethyl acrylamide, dimethyl acrylamide, acrylamide, isoacrylamide, and hydroxyethyl acrylamide;

[0015] (4) the hydrophilic acrylic ester compound includes one or more of hydroxyethyl methacrylate, hydroxyethyl acrylate, and diethylaminoethyl methacrylate;

[0016] (5) The hydrophilic acrylic compound includes acrylic acid and / or methacrylic acid;

[0017] (6) The hydrophilic vinyl compound includes sodium vinyl sulfonate and / or vinyl glycol monoether.

[0018] Preferably, the water-melt adhesive with high bonding strength satisfies one or more of the following conditions:

[0019] a. The ionic liquid comprises a hydrophobic imidazole ionic liquid;

[0020] The hydrophobic imidazolium ionic liquid includes one or more of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-propyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1,3-dimethylimidazolium bis(trifluoromethylsulfonyl)imide, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium hexafluorophosphate, and 1-butyl-3-methylimidazolium tetrafluoroborate;

[0021] b. The amount of the ionic liquid is 10%-50% of the total mass of the raw material;

[0022] c. The initiator comprises a photoinitiator and / or a thermal initiator;

[0023] The photoinitiator includes one or more of 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6-trimethylbenzoyl diphenyl phosphine oxide, 2,4,6-trimethylbenzoyl phosphonic acid ethyl ester, 2-methyl-1-[4-methylthiophenyl]-2-morpholinyl-1-propanone, 2-isopropylthioxanthone, 4-dimethylamino-ethyl benzoate, benzoin dimethyl ether, methyl o-benzoylbenzoate, 4-chlorobenzophenone, 4-phenylbenzophenone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, and α-ketoglutaric acid;

[0024] The thermal initiator includes one or more of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, 1-(cyano-1-methylethylazo)formamide, 1,1'-azo(cyanocyclohexane), dibenzoyl peroxide, diisopropylbenzene peroxide, methyl ethyl ketone peroxide, di-tert-butyl peroxide, potassium persulfate, and ammonium persulfate;

[0025] d. The amount of the initiator used accounts for 0.01%-10% of the total mass of the hydrophobic monomer and the hydrophilic monomer.

[0026] The present application also provides a method for preparing the water-melt adhesive with high bonding strength, comprising:

[0027] mixing the raw materials to obtain a precursor liquid;

[0028] The precursor liquid is degassed, reacted, and then vacuum dried to obtain the water-melt adhesive with high bonding strength.

[0029] Preferably, the reaction includes one or more of a photo-initiated polymerization reaction, a thermal-initiated polymerization reaction, a blending reaction, an immersion reaction, and a solution polymerization reaction;

[0030] The preparation method meets one or more of the following conditions:

[0031] (1) The light source power density of the photopolymerization reaction is 1-1000 Mw / cm 2 , wavelength is 200-450nm, time is 0.01-24h;

[0032] (2) The temperature of the thermally initiated polymerization reaction is 40-110° C. and the time is 1-72 hours.

[0033] Preferably, the method for preparing the water-melt adhesive with high bonding strength satisfies one or more of the following conditions:

[0034] (1) The vacuum degree of the degassing treatment is 1-20 kPa, and the time is 0.1-10 min;

[0035] (2) The vacuum degree of the vacuum drying is 0.1-1000 kPa, the temperature is 10-100° C., and the time is 6-72 h;

[0036] (3) The storage conditions of the water-melt adhesive with high bonding strength are relative humidity of 0-60% and temperature of -50°C to 60°C.

[0037] The present application also provides a method for using the water-melt adhesive having high bonding strength, comprising:

[0038] Wetting the target substrate with water, and then placing the water-melt adhesive with high bonding strength on the surface of the target substrate to obtain a bonding assembly;

[0039] A normal load is applied to the surface of the bonded assembly.

[0040] Preferably, the amount of water used is 0.1-100 μL / cm 2 ;

[0041] The normal load is 1-100 kPa, and the action time is not less than 0.1 h.

[0042] The present application also provides an adhesive tape, comprising the water-melt adhesive with high bonding strength.

[0043] Compared with the prior art, the beneficial effects of this application include:

[0044] The water-melt adhesive with high bonding strength provided in the present application comprises raw materials including hydrophobic monomers, hydrophilic monomers, ionic liquids and initiators; wherein the hydrophobic monomers and hydrophilic monomers jointly adjust the water absorption rate and the degree of plasticization of the material, and the ionic liquid provides fluidity and a large amount of interaction force for the polymer network.

[0045] The water-melt adhesive with high bonding strength provided in the present application is simple to prepare, can achieve strong adhesion by applying only a small amount of water, and can be recycled and reused. This application names it as "water-melt adhesive and water-melt adhesive tape" for the first time. The water-melt adhesive and adhesive tape have no obvious stickiness in a dry state. By dropping a small amount of water on the target substrate and attaching the tape thereto, and pressing it with a small load for a certain period of time, its lap shear strength on the glass can reach 2.9MPa, which is equivalent to the existing commercial hot melt adhesive and much higher than the general tape adhesive (<500kPa). In addition, the water-melt adhesive and adhesive tape can achieve repeated bonding and can be recycled by common organic solvents. The basic principle is: water droplets plasticize the polymer network on the surface of the tape near the layer. Due to the lack of covalent cross-linking constraints, this part of the polymer network temporarily turns into "glue-like", which is very easy to wet the target substrate; water droplets penetrate into the material and disperse evenly. Since the water-melt adhesive tape has good overall hydrophobicity, the water absorption rate after reaching equilibrium is low (<2wt%), so the tape can maintain extremely high body strength.

[0046] The tape does not require additional equipment during the bonding process, and only a few water drops and external force are needed to form strong adhesion, which is suitable for life scenes. The design combines the advantages of glue-type adhesives and tape-type adhesives, showing high bonding strength, and having the characteristics of easy use, easy storage, repeatability and recyclability. At the same time, the material proposed in this application is prepared by a photoinitiator (or thermal initiator) method, which is convenient, fast and easy to operate. The selected system is mainly composed of hydrophobic monomers, hydrophilic monomers and ionic liquids, and has good universality. The method can be extended to different monomers and ionic liquids with the same function, and excellent adhesion performance can be shown by adjusting the appropriate feed ratio. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0048] Figure 1 Schematic diagram of the method of using the water-melt adhesive tape provided in this application;

[0049] Figure 2 The bonding strength of the water-melt adhesive tape provided in Example 1 on different substrates;

[0050] Figure 3 The correlation between the bonding strength of the water-melt adhesive tape provided in Example 1 and the load action time;

[0051] Figure 4 The correlation between the bonding strength and load size of the water-melt adhesive tape provided in Example 1;

[0052] Figure 5 Bond strength of water-melt tapes prepared for different formulations;

[0053] Figure 6 Schematic diagram of different tape wetting methods before gluing;

[0054] Figure 7 The bonding strength of water-melt adhesive tape under different wetting methods;

[0055] Figure 8 The bonding strength of water-melt adhesive tape at different monomer feed ratios;

[0056] Fig. 9 Variation of the surface stiffness of the water-melt adhesive tape with the time of applying water drops;

[0057] Fig.10 The change of visible light transmittance after the water-melt adhesive tape is applied on the rough surface;

[0058] Fig.11 Differential scanning calorimetry (DSC) graph of water-melt adhesive tape before and after adhesive application. DETAILED DESCRIPTION

[0059] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows:

[0060] A water-melt adhesive with high bonding strength, the raw materials of which include: a hydrophobic monomer, a hydrophilic monomer, an ionic liquid and an initiator;

[0061] The ionic liquid is compatible with the hydrophobic monomer and the hydrophilic monomer.

[0062] In an optional embodiment, the raw material satisfies one or more of the following conditions:

[0063] A. the hydrophobic monomer comprises a hydrophobic acrylate compound and / or a hydrophobic vinyl compound;

[0064] B. The hydrophilic monomer includes one or more of a hydrophilic acrylamide compound, a hydrophilic acrylate compound, a hydrophilic acrylic compound, and a hydrophilic vinyl compound;

[0065] C. The amount of the hydrophobic monomer used accounts for no more than 99% of the total mass of the hydrophobic monomer and the hydrophilic monomer.

[0066] Optionally, the ratio of the amount of the hydrophobic monomer to the total mass of the hydrophobic monomer and the hydrophilic monomer can be 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 99% or any value not greater than 99%, preferably 60%.

[0067] In an optional embodiment, the water-melt adhesive with high bonding strength satisfies one or more of the following conditions:

[0068] (1) The hydrophobic acrylic acid ester compound includes one or more of ethyl methacrylate, methyl methacrylate, isopropyl methacrylate, benzyl methacrylate, phenyl methacrylate, isobornyl methacrylate, glycidyl methacrylate, methyl acrylate, cyclohexyl acrylate, and benzyl acrylate;

[0069] (2) The hydrophobic vinyl compound includes styrene;

[0070] (3) The hydrophilic acrylamide compound includes one or more of diethyl acrylamide, dimethyl acrylamide, acrylamide, isoacrylamide, and hydroxyethyl acrylamide;

[0071] (4) the hydrophilic acrylic ester compound includes one or more of hydroxyethyl methacrylate, hydroxyethyl acrylate, and diethylaminoethyl methacrylate;

[0072] (5) The hydrophilic acrylic compound includes acrylic acid and / or methacrylic acid;

[0073] (6) The hydrophilic vinyl compound includes sodium vinyl sulfonate and / or vinyl glycol monoether.

[0074] In an optional embodiment, the water-melt adhesive with high bonding strength satisfies one or more of the following conditions:

[0075] a. The ionic liquid comprises a hydrophobic imidazole ionic liquid;

[0076] The hydrophobic imidazolium ionic liquid includes one or more of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-propyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1,3-dimethylimidazolium bis(trifluoromethylsulfonyl)imide, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium hexafluorophosphate, and 1-butyl-3-methylimidazolium tetrafluoroborate;

[0077] b. The amount of the ionic liquid is 10%-50% of the total mass of the raw material;

[0078] Optionally, the proportion of the amount of the ionic liquid to the total mass of the raw material can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or any value between 10% and 50%, preferably 30%;

[0079] c. The initiator comprises a photoinitiator and / or a thermal initiator;

[0080] The photoinitiator includes one or more of 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6-trimethylbenzoyl diphenyl phosphine oxide, 2,4,6-trimethylbenzoyl phosphonic acid ethyl ester, 2-methyl-1-[4-methylthiophenyl]-2-morpholinyl-1-propanone, 2-isopropylthioxanthone, 4-dimethylamino-ethyl benzoate, benzoin dimethyl ether, methyl o-benzoylbenzoate, 4-chlorobenzophenone, 4-phenylbenzophenone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, and α-ketoglutaric acid;

[0081] The thermal initiator includes one or more of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, 1-(cyano-1-methylethylazo)formamide, 1,1'-azo(cyanocyclohexane), dibenzoyl peroxide, diisopropylbenzene peroxide, methyl ethyl ketone peroxide, di-tert-butyl peroxide, potassium persulfate, and ammonium persulfate;

[0082] d. The amount of the initiator used accounts for 0.01%-10% of the total mass of the hydrophobic monomer and the hydrophilic monomer.

[0083] Optionally, the amount of the initiator used may be 0.01%, 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any value between 0.01% and 10% of the total mass of the hydrophobic monomer and the hydrophilic monomer.

[0084] The present application also provides a method for preparing the water-melt adhesive with high bonding strength, comprising:

[0085] mixing the raw materials to obtain a precursor liquid;

[0086] The precursor liquid is degassed, reacted, and then vacuum dried to obtain the water-melt adhesive with high bonding strength.

[0087] In an optional embodiment, the reaction includes one or more of a photo-initiated polymerization reaction, a thermal-initiated polymerization reaction, a blending reaction, an immersion reaction, and a solution polymerization reaction;

[0088] The preparation method meets one or more of the following conditions:

[0089] (1) The light source power density of the photopolymerization reaction is 1-1000 Mw / cm 2 , wavelength is 200-450nm, time is 0.01-24h;

[0090] Optionally, the light source power density of the photo-initiated polymerization reaction can be 1Mw / cm 2 、10Mw / cm 2 、100Mw / cm 2 、500Mw / cm 2 、1000Mw / cm 2 Or 1-1000Mw / cm 2 The wavelength can be 200nm, 250nm, 300nm, 350nm, 400nm, 450nm or any value between 200-450nm, and the time can be 0.01h, 0.1h, 1h, 2h, 6h, 12h, 24h or any value between 0.01-24h;

[0091] (2) The temperature of the thermally initiated polymerization reaction is 40-110° C. and the time is 1-72 hours.

[0092] Optionally, the temperature of the thermally initiated polymerization reaction can be 40, 50, 60, 70, 80, 90, 100, 110 or 40-110° C., and the time can be 1 h, 2 h, 6 h, 12 h, 24 h, 36 h, 48 h, 60 h, 72 h or 1-72 h.

[0093] In an optional embodiment, the method for preparing the water-melt adhesive with high bonding strength satisfies one or more of the following conditions:

[0094] (1) The vacuum degree of the degassing treatment is 1-20 kPa, and the time is 0.1-10 min;

[0095] Optionally, the vacuum degree of the degassing treatment may be 1 kPa, 5 kPa, 10 kPa, 15 kPa, 20 kPa or any value between 1 and 20 kPa, and the time may be 0.1 min, 1 min, 5 min, 10 min or any value between 0.1 and 10 min;

[0096] (2) The vacuum degree of the vacuum drying is 0.1-1000 kPa, the temperature is 10-100° C., and the time is 6-72 h;

[0097] Optionally, the vacuum degree of the vacuum drying can be 0.1 kPa, 1 kPa, 10 kPa, 100 kPa, 500 kPa, 1000 kPa or any value between 0.1-1000 kPa, the temperature can be 10°C, 50°C, 100°C or any value between 10-100°C, and the time can be 6 h, 12 h, 24 h, 36 h, 48 h, 60 h, 72 h or any value between 6-72 h;

[0098] (3) The storage conditions of the water-melt adhesive with high bonding strength are relative humidity of 0-60% and temperature of -50°C to 60°C.

[0099] Optionally, the storage conditions of the water-melt adhesive with high bonding strength are relative humidity of 0%, 10%, 20%, 30%, 40%, 50%, 60% or any value between 0-60%, and the temperature can be -50℃, -40℃, -30℃, -20℃, -10℃, 0℃, 10℃, 20℃, 30℃, 40℃, 50℃, 60℃ or any value between -50℃ and 60℃.

[0100] The present application also provides a method for using the water-melt adhesive having high bonding strength, comprising:

[0101] Wetting the target substrate with water, and then placing the water-melt adhesive with high bonding strength on the surface of the target substrate to obtain a bonding assembly;

[0102] A normal load is applied to the surface of the bonded assembly.

[0103] In an optional embodiment, the amount of water used is 0.1-100 μL / cm 2 ;

[0104] The normal load is 1-100 kPa, and the action time is not less than 0.1 h.

[0105] Optionally, the amount of water used can be 0.1 μL / cm 2 , 1μL / cm 2 , 10μL / cm 2 , 50μL / cm 2 , 100μL / cm 2 Or 0.1-100μL / cm 2any value between; the normal load can be 1 kPa, 10 kPa, 50 kPa, 100 kPa or any value between 1 and 100 kPa, and the action time can be 0.1 h, 0.5 h, 1 h, 5 h, 10 h, 20 h, 30 h, 40 h, 50 h, 60 h, 70 h, 80 h, 90 h, 100 h or any value not less than 0.1 h.

[0106] The present application also provides an adhesive tape, comprising the water-melt adhesive with high bonding strength.

[0107] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0108] Example 1

[0109] This embodiment provides a water-melt adhesive tape with high bonding strength, and the preparation method thereof is as follows:

[0110] Mix 4.2g of ethyl methacrylate (hydrophobic monomer, EMA), 2.8g of diethylacrylamide (hydrophilic monomer, DEAm), 3.0g of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide salt (ionic liquid, [EMI][TFSI]) and 70mg of 1-hydroxy-cyclohexylphenyl ketone (photoinitiator 184), stir thoroughly until homogeneous, and form a precursor liquid. Place the evenly mixed precursor liquid in a vacuum box with a vacuum degree of 100kPa and degas for 30s. Inject the degassed precursor liquid into the assembled glass sheet-silicone pad-glass sheet sandwich cavity (the glass sheet is coated with a release film). Place the mold injected with the precursor liquid in a UV crosslinking box with a power density of 50mW / cm 2 After the reaction is completed, the glass mold is disassembled, the sample is taken out and placed in a vacuum drying oven for vacuum degassing at room temperature for 24 hours (vacuum degree 100 kPa) to remove residual volatile monomers to obtain a water-melt adhesive tape with high bonding strength, which is stored in a desiccator at room temperature for later use.

[0111] Example 2

[0112] This embodiment provides a water-melt adhesive tape with high bonding strength, and the preparation method thereof is as follows:

[0113] Mix 3.6g of methyl methacrylate (hydrophobic monomer, MMA), 2.4g of diethyl acrylamide (hydrophilic monomer, DEAm), 4.0g of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide salt (ionic liquid, [EMI][TFSI]) and 60mg of 1-hydroxy-cyclohexylphenyl ketone (photoinitiator 184), stir thoroughly until homogeneous, and form a precursor liquid. Place the mixed precursor liquid in a vacuum box with a vacuum degree of 100kPa and degas for 30s. Inject the degassed precursor liquid into the assembled glass sheet-silicone pad-glass sheet sandwich cavity (the glass sheet is coated with a release film). Place the mold injected with the precursor liquid in a UV crosslinking box with a power density of 50mW / cm 2 After the reaction is completed, the glass mold is disassembled, the sample is taken out and placed in a vacuum drying oven for vacuum degassing at room temperature for 24 hours (vacuum degree 100 kPa) to remove residual volatile monomers, and a water-melt adhesive tape with high bonding strength is obtained, which is stored in a desiccator at room temperature for later use.

[0114] Example 3

[0115] This embodiment provides a water-melt adhesive tape with high bonding strength, and the preparation method thereof is as follows:

[0116] Mix 4.0g of ethyl methacrylate (hydrophobic monomer, EMA), 2.7g of hydroxyethyl methacrylate (hydrophilic monomer, HEMA), 3.3g of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide salt (ionic liquid, [EMI][TFSI]) and 70mg of 1-hydroxy-cyclohexylphenyl ketone (photoinitiator 184), stir thoroughly until homogeneous, and form a precursor liquid. Place the mixed precursor liquid in a vacuum box with a vacuum degree of 100kPa and degas for 30s. Inject the degassed precursor liquid into the assembled glass sheet-silicone pad-glass sheet sandwich cavity (the glass sheet is coated with a release film). Place the mold injected with the precursor liquid in a UV crosslinking box with a power density of 50mW / cm 2 After the reaction is completed, the glass mold is disassembled, the sample is taken out and placed in a vacuum drying oven for vacuum degassing at room temperature for 24 hours (vacuum degree 100 kPa) to remove residual volatile monomers, and a water-melt adhesive tape with high bonding strength is obtained, which is stored in a desiccator at room temperature for later use.

[0117] Example 4

[0118] This embodiment provides a water-melt adhesive tape with high bonding strength, and the preparation method thereof is as follows:

[0119] Mix 4.2g of ethyl methacrylate (hydrophobic monomer, EMA), 2.8g of diethyl acrylamide (hydrophilic monomer, DEAm), 3.0g of 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide salt (ionic liquid, [BMI][TFSI]) and 70mg of 1-hydroxy-cyclohexylphenyl ketone (photoinitiator 184), stir thoroughly until homogeneous, and form a precursor liquid. Place the uniformly mixed precursor liquid in a vacuum box with a vacuum degree of 100kPa and degas for 30s. Inject the degassed precursor liquid into the assembled glass sheet-silicone pad-glass sheet sandwich cavity (the glass sheet is coated with a release film). Place the mold injected with the precursor liquid in a UV crosslinking box with a power density of 50mW / cm 2 After the reaction is completed, the glass mold is disassembled, the sample is taken out and placed in a vacuum drying oven for vacuum degassing at room temperature for 24 hours (vacuum degree 100 kPa) to remove residual volatile monomers, and a water-melt adhesive tape with high bonding strength is obtained, which is stored in a desiccator at room temperature for later use.

[0120] Example 5

[0121] This embodiment provides a water-melt adhesive tape with high bonding strength, and the preparation method thereof is as follows:

[0122] 4.2g of ethyl methacrylate (hydrophobic monomer, EMA), 2.8g of diethyl acrylamide (hydrophilic monomer, DEAm), 3.0g of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide salt (ionic liquid, [EMI][TFSI]) and 70mg of azobisisobutyronitrile (thermal initiator) were mixed and stirred until homogeneous to form a precursor liquid. The uniformly mixed precursor liquid was placed in a vacuum box with a vacuum degree of 100kPa and degassed for 30s. The degassed precursor liquid was injected into the assembled glass sheet-silicone pad-glass sheet sandwich cavity (the glass sheet was coated with a release film). The mold injected with the precursor liquid was placed in a temperature control box with a constant temperature of 60°C and cross-linked for 12h. After the reaction was completed, the glass mold was disassembled, the sample was taken out and placed in a vacuum drying oven, vacuum degassed at room temperature for 24h (vacuum degree 100kPa) to remove residual volatile monomers, and a water-melt adhesive tape with high bonding strength was obtained, which was stored in a desiccator at room temperature for later use.

[0123] Example 6

[0124] This embodiment provides a water-melt adhesive tape with high bonding strength, and the preparation method thereof is as follows:

[0125] Mix 4.2g of ethyl methacrylate (hydrophobic monomer, EMA), 2.8g of diethylacrylamide (hydrophilic monomer, DEAm), 70mg of azobisisobutyronitrile (thermal initiator) and 15mL of tetrahydrofuran (solvent), stir thoroughly until homogeneous, and form a precursor liquid. Bubble nitrogen into the uniformly mixed precursor liquid for 30 minutes to remove dissolved oxygen in the precursor liquid. Place the precursor liquid in a glass flask, heat it to 60°C in an oil bath, and react for 12 hours. Add 60mL of n-hexane (poor solvent) to the reacted solution to obtain a suspension. Centrifuge the suspension for 15 minutes in a centrifuge (speed 5000rpm), and remove the supernatant. The precipitate was mixed with 3.0 g of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide salt (ionic liquid, [EMI][TFSI]), injected into an open glass mold (the glass sheet was coated with a release film), and vacuum degassed in a vacuum drying oven at room temperature for 24 h (vacuum degree 100 kPa) to remove residual solvent and volatile monomers. The glass mold was disassembled to obtain a water-melt adhesive tape with high bonding strength, which was stored in a desiccator at room temperature for future use.

[0126] Comparative Example 1

[0127] Mix 7.0g of ethyl methacrylate (hydrophobic monomer, EMA), 3.0g of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide salt (ionic liquid, [EMI][TFSI]) and 70mg of 1-hydroxy-cyclohexylphenyl ketone (photoinitiator 184), stir thoroughly until homogeneous, and form a precursor liquid. Place the uniformly mixed precursor liquid in a vacuum box with a vacuum degree of 100kPa and degas for 30s. Inject the degassed precursor liquid into the assembled glass sheet-silicone pad-glass sheet sandwich cavity (the glass sheet is coated with a release film). Place the mold injected with the precursor liquid in a UV crosslinking box with a power density of 50mW / cm 2 After the reaction is completed, the glass mold is disassembled, the sample is taken out and placed in a vacuum drying oven for vacuum degassing at room temperature for 24 hours (vacuum degree 100 kPa) to remove the residual volatile monomers, and the tape is obtained and stored in a desiccator at room temperature for later use.

[0128] Comparative Example 2

[0129] 7.0g diethyl acrylamide (hydrophilic monomer, DEAm), 3.0g 1-ethyl-3-methylimidazolium bis trifluoromethylsulfonyl imide salt (ionic liquid, [EMI][TFSI]) and 70mg 1-hydroxy-cyclohexyl phenyl ketone (photoinitiator 184) were mixed and stirred until homogeneous to form a precursor liquid. The uniformly mixed precursor liquid was placed in a vacuum box with a vacuum degree of 100kPa and degassed for 30s. The degassed precursor liquid was injected into the assembled glass sheet-silicone pad-glass sheet sandwich cavity (the glass sheet was coated with a release film). The mold injected with the precursor liquid was placed in a UV crosslinking box with a power density of 50mW / cm2 and crosslinked for 60min. After the reaction was completed, the glass mold was disassembled, the sample was taken out and placed in a vacuum drying oven, and vacuum degassed for 24h (vacuum degree 100kPa) at room temperature to remove residual volatile monomers to obtain a tape, which was stored in a dryer at room temperature for use.

[0130] Comparative Example 3

[0131] Mix 4.2g of ethyl methacrylate (hydrophobic monomer, EMA), 2.8g of diethyl acrylamide (hydrophilic monomer, DEAm) and 70mg of 1-hydroxy-cyclohexyl phenyl ketone (photoinitiator 184), stir thoroughly until homogeneous, and form a precursor liquid. Place the uniformly mixed precursor liquid in a vacuum box with a vacuum degree of 100kPa and degas for 30s. Inject the degassed precursor liquid into the assembled glass sheet-silicone pad-glass sheet sandwich cavity (the glass sheet is coated with a release film). Place the mold injected with the precursor liquid in a UV crosslinking box with a power density of 50mW / cm 2 After the reaction was completed, the glass mold was disassembled, the sample was taken out and placed in a vacuum drying oven for vacuum degassing at room temperature for 24 hours (vacuum degree 100 kPa) to remove the residual volatile monomers, and a transparent hard plastic sheet was obtained, which could not be used as a tape.

[0132] The bonding performance of the water-melt adhesive tape with high bonding strength is characterized by the lap shear test. The test content includes the bonding strength of the hot melt adhesive tape on different substrates, the relationship between the bonding strength and the load size and the action time, and the effect of different feed ratios on the bonding strength (see the attached figure).

[0133] Figure 1 This is a schematic diagram of how to use water-melt adhesive tape. Specifically:

[0134] (1) Wet the target substrate with a small amount of purified water / tap water;

[0135] (2) Spread the hot melt tape evenly on the moistened substrate surface and press to drain excess water;

[0136] (3) applying a normal load to the bonding surface for a certain period of time until the water-melt adhesive tape is firmly bonded to the substrate;

[0137] (4) During the lap shear test, both sides of the hot melt tape are bonded to the substrate according to the above steps.

[0138] Figure 2 The bonding strength of the material in Example 1 on different substrates shows that the material exhibits high bonding strength (1.5 MPa to 3 MPa) on commonly used plastic, ceramic, glass and metal substrates.

[0139] Figure 3 The bonding strength of the material in Example 1 under a load of 50 kPa for different action times is shown. The results show that the bonding strength of the material rapidly increases to 80% of the maximum value in the first 6 hours and basically reaches equilibrium after 48 hours.

[0140] Figure 4 The bonding strength of the material in Example 1 under different load sizes for 3 hours and 48 hours. The results show that increasing the load can accelerate the increase in bonding strength, and the load size has no significant effect on the bonding strength after equilibrium.

[0141] Figure 5 The bonding performance of the materials in Examples 1-4 on a wet PET (polyethylene terephthalate) substrate after a load of 50 kPa for 48 hours, all of which showed high bonding strength (>1 MPa).

[0142] Figure 6 The method of wetting the tape before gluing includes but is not limited to dipping, spraying, wetting with a humidifier, soaking and the like.

[0143] Figure 7 It is the bonding strength of water-melt adhesive tape obtained after various wetting methods.

[0144] Figure 8 The bonding strength of the water-melt adhesive tapes prepared with different monomer feed ratios (f, mass ratio of hydrophobic monomer to total monomers), wherein f=1 and f=0 correspond to comparative example 1 and comparative example 2, respectively.

[0145] Fig. 9 The surface stiffness changes with time after a water layer is applied to the surface of the water-melt adhesive tape obtained in Example 1. The results show that the surface stiffness decreases rapidly within 1 hour, and the plasticization effect of the surface layer of the material is obvious.

[0146] Fig.10 The figure shows the change in visible light transmittance after the water-melt adhesive tape obtained in Example 1 was applied to a rough surface. The results show that the transmittance increased significantly 3 hours after application, proving that the material has a strong interfacial wetting ability after plasticization.

[0147] Fig.11This is the DSC graph of the water-melt adhesive tape obtained in Example 1 before and after gluing. The results show that the glass transition temperature has only a slight change, and is still 11.9°C after gluing (slightly higher than room temperature, which is a more ideal glass transition temperature of the adhesive), proving that the tape still has a high body strength after reaching equilibrium.

[0148] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A water-melt adhesive with high bonding strength, characterized in that: The raw materials include: hydrophobic monomer, hydrophilic monomer, ionic liquid and initiator; The ionic liquid is compatible with the hydrophobic monomer and the hydrophilic monomer.

2. The water-melt adhesive with high bonding strength according to claim 1, characterized in that: The raw materials meet one or more of the following conditions: A. the hydrophobic monomer comprises a hydrophobic acrylate compound and / or a hydrophobic vinyl compound; B. The hydrophilic monomer includes one or more of a hydrophilic acrylamide compound, a hydrophilic acrylate compound, a hydrophilic acrylic compound, and a hydrophilic vinyl compound; C. The amount of the hydrophobic monomer used accounts for no more than 99% of the total mass of the hydrophobic monomer and the hydrophilic monomer.

3. The water-melt adhesive with high bonding strength according to claim 2, characterized in that: One or more of the following conditions are met: (1) The hydrophobic acrylic acid ester compound includes one or more of ethyl methacrylate, methyl methacrylate, isopropyl methacrylate, benzyl methacrylate, phenyl methacrylate, isobornyl methacrylate, glycidyl methacrylate, methyl acrylate, cyclohexyl acrylate, and benzyl acrylate; (2) The hydrophobic vinyl compound includes styrene; (3) The hydrophilic acrylamide compound includes one or more of diethyl acrylamide, dimethyl acrylamide, acrylamide, isoacrylamide, and hydroxyethyl acrylamide; (4) the hydrophilic acrylic ester compound includes one or more of hydroxyethyl methacrylate, hydroxyethyl acrylate, and diethylaminoethyl methacrylate; (5) The hydrophilic acrylic compound includes acrylic acid and / or methacrylic acid; (6) The hydrophilic vinyl compound includes sodium vinyl sulfonate and / or vinyl glycol monoether.

4. The water-melt adhesive with high bonding strength according to any one of claims 1 to 3, characterized in that: One or more of the following conditions are met: a. The ionic liquid comprises a hydrophobic imidazole ionic liquid; The hydrophobic imidazolium ionic liquid includes one or more of 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-propyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1,3-dimethylimidazolium bis(trifluoromethylsulfonyl)imide, 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-butyl-3-methylimidazolium hexafluorophosphate, and 1-butyl-3-methylimidazolium tetrafluoroborate; b. The amount of the ionic liquid is 10%-50% of the total mass of the raw material; c. The initiator comprises a photoinitiator and / or a thermal initiator; The photoinitiator includes one or more of 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6-trimethylbenzoyl diphenyl phosphine oxide, 2,4,6-trimethylbenzoyl phosphonic acid ethyl ester, 2-methyl-1-[4-methylthiophenyl]-2-morpholinyl-1-propanone, 2-isopropylthioxanthone, 4-dimethylamino-ethyl benzoate, benzoin dimethyl ether, methyl o-benzoylbenzoate, 4-chlorobenzophenone, 4-phenylbenzophenone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, and α-ketoglutaric acid; The thermal initiator includes one or more of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, 1-(cyano-1-methylethylazo)formamide, 1,1'-azo(cyanocyclohexane), dibenzoyl peroxide, diisopropylbenzene peroxide, methyl ethyl ketone peroxide, di-tert-butyl peroxide, potassium persulfate, and ammonium persulfate; d. The amount of the initiator used accounts for 0.01%-10% of the total mass of the hydrophobic monomer and the hydrophilic monomer.

5. A method for preparing a water-melt adhesive with high bonding strength according to any one of claims 1 to 4, characterized in that: include: mixing the raw materials to obtain a precursor liquid; The precursor liquid is degassed, reacted, and then vacuum dried to obtain the water-melt adhesive with high bonding strength.

6. The method for preparing a water-melt adhesive with high bonding strength according to claim 5, characterized in that: The reaction includes one or more of a photo-initiated polymerization reaction, a thermal-initiated polymerization reaction, a blending reaction, an immersion reaction, and a solution polymerization reaction; The preparation method meets one or more of the following conditions: (1) The light source power density of the photopolymerization reaction is 1-1000 Mw / cm 2 , wavelength is 200-450nm, time is 0.01-24h; (2) The temperature of the thermally initiated polymerization reaction is 40-110° C. and the time is 1-72 hours.

7. The method for preparing a water-melt adhesive with high bonding strength according to claim 5 or 6, characterized in that: One or more of the following conditions are met: (1) The vacuum degree of the degassing treatment is 1-20 kPa, and the time is 0.1-10 min; (2) The vacuum degree of the vacuum drying is 0.1-1000 kPa, the temperature is 10-100° C., and the time is 6-72 h; (3) The storage conditions of the water-melt adhesive with high bonding strength are relative humidity of 0-60% and temperature of -50°C to 60°C.

8. A method for using the water-melt adhesive with high bonding strength as claimed in any one of claims 1 to 4, characterized in that: include: Wetting the target substrate with water, and then placing the water-melt adhesive with high bonding strength on the surface of the target substrate to obtain a bonding assembly; A normal load is applied to the surface of the bonded assembly.

9. The method for using the water-melt adhesive with high bonding strength according to claim 8, characterized in that: The amount of water used is 0.1-100 μL / cm 2 ; The normal load is 1-100 kPa, and the action time is not less than 0.1 h.

10. An adhesive tape, characterized in that: The invention comprises the water-melt adhesive with high bonding strength as described in any one of claims 1 to 4.