Corrosion inhibition and viscosity reduction composition as well as preparation method and application thereof

By preparing a corrosion-inhibiting and viscosity-reducing composition containing imidazoline compounds, parabens, dimethyl carbonate and polyacrylic acid, the problem of the lack of simultaneous viscosity-reducing and corrosion-inhibiting effects in the existing technology is solved, and the invention is achieved. Effective viscosity reduction and corrosion inhibition effects in high salinity environments reduce costs and improve the efficiency of industrial applications.

CN118792033AActive Publication Date: 2024-10-18CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310381208.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-18
Estimated Expiration
2043-04-11

AI Technical Summary

Technical Problem

The existing technology lacks multifunctional crude oil additives that can simultaneously reduce viscosity and inhibit corrosion in high-salinity environments, resulting in high costs and poor effects when using corrosion inhibitors and viscosity reducers. Moreover, existing oil-soluble viscosity reducers The agent cannot meet the replacement efficiency requirements of industrial production.

Method used

Provided is a corrosion inhibitor and viscosity reducing composition, which includes imidazoline compounds, paraben compounds, dimethyl carbonate and polyacrylic acid, is combined with maleic acid and a solvent, and is prepared by heating and cooling to form a strong Soluble and dispersible compositions to achieve viscosity reduction and corrosion inhibition effects.

Benefits of technology

The composition has a significant viscosity-reducing effect on heavy oil at different temperatures, and significantly reduces the corrosion rate of N80 steel sheets in high-salinity environments, proving its effectiveness and broad application potential in the field of oilfield corrosion prevention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004172291460000021
    Figure BDA0004172291460000021
  • Figure BDA0004172291460000022
    Figure BDA0004172291460000022
  • Figure BDA0004172291460000051
    Figure BDA0004172291460000051
Patent Text Reader

Abstract

The invention provides a corrosion-inhibiting and viscosity-reducing composition as well as a preparation method and application thereof. The corrosion-inhibiting and viscosity-reducing composition provided by the invention comprises an imidazoline compound, a p-hydroxybenzoate compound, dimethyl carbonate and polyacrylic acid, and further comprises maleic acid and a solvent, so that the corrosion-inhibiting and viscosity-reducing composition is a corrosion inhibitor with a viscosity-reducing effect. The corrosion-inhibiting viscosity-reducing composition provided by the invention is simple in preparation method and easy in raw material obtaining, has viscosity-reducing and corrosion-inhibiting properties, and is suitable for popularization and application in the field of corrosion prevention of oil fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oilfield corrosion prevention, and in particular relates to a corrosion inhibition and viscosity reduction composition, a preparation method and an application thereof. Background Art

[0002] As an efficient strategic resource, oil plays a vital role in people's lives and national development. With the development of society and the advancement of science and technology, people's demand for oil continues to rise, resulting in my country's oil consumption continuing to increase in recent years, oil reserves are rapidly declining, and oil production is increasing year by year.

[0003] Crude oil, especially heavy oil, has the characteristics of high viscosity and difficulty in flowing, which seriously restricts the mining and transportation of heavy oil. This characteristic determines that the mining, transportation and refining of heavy oil must be carried out around viscosity reduction, decondensation modification or modification. The viscosity reduction method of adding viscosity reducer has the advantages of simple process and low cost, thus becoming a method with great development prospects.

[0004] Blending and diluting to reduce viscosity is a widely used heavy oil production process. This process uses distillate oil, thin crude oil or other organic solvents as diluents, which are injected into the wellbore and mixed with heavy oil to significantly reduce its viscosity and improve its fluidity to a degree that it can be produced. According to existing research, crude oil viscosity is usually below 4000mPa·s to be produced and transported. For some super-heavy oil and extra-heavy oil, such as Tahe heavy oil, the viscosity is mostly above 50000mPa·s, and a large amount of diluent needs to be added to achieve the viscosity required for normal production. The amount of diluent is an important indicator that determines the economic efficiency of heavy oil production. The development of oil-soluble viscosity reducers for the purpose of reducing the amount of diluent has been widely carried out, but most of them are limited to indoor research and field test stages. Industrial production requires that oil-soluble viscosity reducers have a high substitution efficiency, and a small amount of viscosity reducer can replace a large amount of diluent. Most of the oil-soluble viscosity reducers reported cannot meet the requirements.

[0005] There are currently two main approaches to solving the corrosion problem in oil fields. One is to change the material of the oil and gas well pipe column to make it corrosion-resistant or use anti-corrosion pipes for lining; the other is to use corrosion inhibitors. In actual applications, the cost of using corrosion-resistant pipes is high, and pitting and pitting problems still occur, causing the strength of corrosion-resistant pipes to be unable to meet production needs within the safe service life. Although corrosion inhibitors are widely used, corrosion inhibitors that can withstand high temperatures in high-mineralization environments are still rare.

[0006] There are many types of corrosion inhibitors and viscosity reducers currently used in industry. Using corrosion inhibitors and viscosity reducers at the same time for the purpose of corrosion prevention and viscosity reduction will lead to problems such as reduced corrosion inhibition and viscosity reduction effects and increased costs. It can be seen that developing multifunctional crude oil additives that have the functions of viscosity reduction, corrosion inhibition, and pour point reduction to further reduce costs and simplify process flow is the future development direction. Summary of the invention

[0007] The purpose of the present invention is to provide a corrosion inhibition and viscosity reduction composition and a preparation method and application thereof. The corrosion inhibition and viscosity reduction composition has strong solubility and dispersibility in crude oil, and has a viscosity reduction effect while having corrosion inhibition performance, so as to solve the above-mentioned problems existing in the prior art.

[0008] To achieve the above objectives, the first aspect of the present invention provides a corrosion inhibition and viscosity reduction composition, which comprises an imidazoline compound, a p-hydroxybenzoate compound, dimethyl carbonate and polyacrylic acid.

[0009] In a specific embodiment of the present invention, the corrosion inhibition and viscosity reduction composition further comprises maleic acid and a solvent;

[0010] Preferably, the solvent is a lower alcohol;

[0011] Preferably, the lower alcohol is ethanol.

[0012] In a specific embodiment of the present invention, based on the mass of the corrosion inhibition and viscosity reduction composition, the corrosion inhibition and viscosity reduction composition comprises:

[0013]

[0014] Preferably, the corrosion inhibition and viscosity reduction composition comprises:

[0015]

[0016] In a specific embodiment of the present invention, the imidazoline compound is selected from at least one of aminoethyl heptadecenyl imidazoline, imidazoline ester and lauryl imidazoline.

[0017] In a specific embodiment of the present invention, the imidazoline compound is lauryl imidazoline.

[0018] In a specific embodiment of the present invention, the paraben compound is selected from at least two of methyl parahydroxybenzoate, ethyl parahydroxybenzoate and propyl parahydroxybenzoate.

[0019] In a specific embodiment of the present invention, the paraben compound is a mixture of methyl paraben and ethyl paraben;

[0020] Preferably, the molar ratio of methyl parahydroxybenzoate to ethyl parahydroxybenzoate is 1:0.8.

[0021] In a specific embodiment of the present invention, the weight average molecular weight of the polyacrylic acid is 3000 to 5000;

[0022] Preferably, the weight average molecular weight of the polyacrylic acid is 5,000.

[0023] The second aspect of the present invention provides a method for preparing the corrosion inhibition and viscosity reduction composition according to the first aspect of the present invention, which comprises the following steps:

[0024] The imidazoline compound, the p-hydroxybenzoate compound, dimethyl carbonate and polyacrylic acid are mixed, heated and cooled to obtain the corrosion inhibition and viscosity reduction composition.

[0025] In a specific embodiment of the present invention, the imidazoline compound, the p-hydroxybenzoate compound, dimethyl carbonate, polyacrylic acid, maleic acid and a solvent are mixed, and then the heating is performed;

[0026] Preferably, the heating temperature is 80°C to 90°C; and / or

[0027] The cooling is cooling to room temperature (i.e. 25° C.);

[0028] Preferably, the heating temperature is 85°C.

[0029] Application of the corrosion-inhibiting and viscosity-reducing composition according to the first aspect of the present invention or the corrosion-inhibiting and viscosity-reducing composition prepared by the method according to the second aspect of the present invention in the field of oilfield corrosion protection technology, especially as a corrosion inhibitor with viscosity-reducing effect.

[0030] Beneficial effects of the present invention:

[0031] In view of the lack of corrosion inhibitors with viscosity reduction function in the prior art, and the high cost of using common corrosion inhibitors and viscosity reducers for the purpose of viscosity reduction and corrosion inhibition, and the problem that the viscosity reduction and corrosion inhibition effects are deteriorated, the present invention provides a corrosion inhibition and viscosity reduction composition and a preparation method and application thereof. The corrosion inhibition and viscosity reduction composition provided by the present invention first includes an imidazoline compound, a paraben compound, dimethyl carbonate, polyacrylic acid, and secondly also includes maleic acid and a solvent, and is a corrosion inhibitor with both viscosity reduction effect. The corrosion inhibition and viscosity reduction composition provided by the present invention has strong solubility and dispersibility in crude oil, and the imidazoline compounds, paraben compounds, polyacrylic acid and dimethyl carbonate synergize in viscosity reduction and corrosion inhibition performance, and simultaneously achieve good viscosity reduction effect and corrosion inhibition performance: at 80°C, 50°C and 20°C, when the amount of the corrosion inhibition and viscosity reduction composition added is 0.3wt% of the mass of the heavy oil (viscosity at 50°C is 16800mP.s), the viscosity reduction rate of the heavy oil is 29% to 35%, 46% to 48%, and 60% to 62%, respectively; at crude oil (viscosity at 30°C is 57mP.s) and heavy oil (viscosity at 30°C is 57mP.s), the viscosity reduction rate of the heavy oil is 29% to 35%, 46% to 48%, and 60% to 62%, respectively. In a corrosive medium obtained by mixing 1:1:0.7 with injection water having a mineralization degree of 210,000 mg / L (viscosity at 50°C is 16800 mP.s), when the amount of the corrosion-inhibiting and viscosity-reducing composition added is 0.3wt%, the corrosion rate of the N80 steel sheet in the corrosive medium containing the corrosion-inhibiting and viscosity-reducing composition is 0.034 to 0.046 mm / a, and the corrosion inhibition rate of the corrosion-inhibiting and viscosity-reducing composition provided by the present invention on the N80 steel sheet is 73.41% to 80.35%; compared with the corrosive medium without the corrosion-inhibiting and viscosity-reducing composition, the corrosion degree of the N80 steel sheet in the corrosive medium containing the corrosion-inhibiting and viscosity-reducing composition is significantly reduced. The preparation method of the corrosion-inhibiting and viscosity-reducing composition is simple, and the raw materials are easily available. It can be widely promoted and applied in the field of oilfield anti-corrosion technology as a corrosion inhibitor with viscosity reduction effect. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with examples, but the examples of the present invention are only exemplary descriptions, and the implementation methods do not constitute limitations of the present invention under any circumstances.

[0033] Preparation of corrosion inhibition and viscosity reduction composition

[0034] The polyacrylic acid used in Examples 1 to 3 has a weight average molecular weight of 5000 and was purchased from Shanghai Haohong Biopharmaceutical Technology Co., Ltd.;

[0035] The lauryl imidazoline used in Examples 1 to 3 was purchased from Shandong Qixinyuan New Material Technology Co., Ltd.

[0036] Example 1

[0037] 10 g of lauryl imidazoline, 2 g of a mixture of methyl p-hydroxybenzoate and ethyl p-hydroxybenzoate (wherein the molar ratio of methyl p-hydroxybenzoate to ethyl p-hydroxybenzoate is 1:0.8), 1 g of dimethyl carbonate, 1 g of polyacrylic acid, 4 g of maleic acid and 20 g of ethanol were mixed, heated to 85° C., and cooled to room temperature (25° C.) while stirring to obtain a corrosion inhibition and viscosity reduction composition, which is a corrosion inhibitor having a viscosity reduction effect.

[0038] Example 2

[0039] 12 g of lauryl imidazoline, 4 g of a mixture of methyl p-hydroxybenzoate and ethyl p-hydroxybenzoate (wherein the molar ratio of methyl p-hydroxybenzoate to ethyl p-hydroxybenzoate is 1:0.8), 3 g of dimethyl carbonate, 3 g of polyacrylic acid, 6 g of maleic acid and 25 g of ethanol were mixed, heated to 85° C., and cooled to room temperature (25° C.) while stirring to obtain a corrosion inhibition and viscosity reduction composition, which is a corrosion inhibitor having a viscosity reduction effect.

[0040] Example 3

[0041] 15 g of lauryl imidazoline, 6 g of a mixture of methyl p-hydroxybenzoate and ethyl p-hydroxybenzoate (wherein the molar ratio of methyl p-hydroxybenzoate to ethyl p-hydroxybenzoate is 1:0.8), 3 g of dimethyl carbonate, 5 g of polyacrylic acid, 8 g of maleic acid and 30 g of ethanol were mixed, heated to 85° C., and cooled to room temperature (25° C.) while stirring to obtain a corrosion inhibition and viscosity reduction composition, which is a corrosion inhibitor having a viscosity reduction effect.

[0042] Experimental evaluation

[0043] 1. Evaluation of the viscosity reduction performance of the corrosion inhibition and viscosity reduction composition at room temperature

[0044] The viscosity of crude oil and heavy oil and the salinity of injected water used in this experiment are as follows:

[0045] Crude oil: viscosity is 57mPa.s at 30°C;

[0046] Heavy oil: viscosity is 16800mPa.s at 50°C;

[0047] Injection water: oilfield produced water with a mineralization of 210,000 mg / L.

[0048] The viscosity reducing performance of the corrosion inhibition and viscosity reducing compositions prepared in Examples 1 to 3 at room temperature was evaluated by the following specific method:

[0049] i. Preparation of the test solution: crude oil, heavy oil and injection water are mixed evenly to obtain the test solution (wherein the mass ratio of crude oil, heavy oil and injection water is 1:1:0.7), and the test solution is used as a blank control;

[0050] ii. mixing the corrosion-inhibiting and viscosity-reducing composition with the liquid to be tested, wherein the mass of the corrosion-inhibiting and viscosity-reducing composition is 0.3 wt % of the mass of the liquid to be tested, to obtain the liquid to be tested treated with the corrosion-inhibiting and viscosity-reducing composition;

[0051] ⅲ At room temperature (i.e., 25°C), the viscosity of the blank control group test liquid and the test liquid of the experimental group treated with the corrosion inhibition and viscosity reduction composition was measured using the RND-1 petroleum product kinematic viscosity tester produced by Jilin Ruigu Scientific Instrument Co., Ltd. and recorded, and the viscosity reduction rate was further calculated. The results are shown in Table 1.

[0052] Table 1. Evaluation of viscosity reduction effect of corrosion inhibition and viscosity reduction composition

[0053] Serial number Viscosity(mP.s) Viscosity reduction rate (%) Blank control 28420 / Example 1 11640 59.04 Example 2 10230 64.00 Example 3 10540 62.91

[0054] As can be seen from Table 1, the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 have a viscosity reduction rate of 59% to 64% at room temperature for the test liquid obtained by mixing crude oil, heavy oil and injection water in a mass ratio of 1:1:0.7, indicating that the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 have an obvious viscosity reduction effect on the test liquid. Among them, the corrosion inhibition and viscosity reduction composition prepared in Example 2 has the best viscosity reduction performance, and its viscosity reduction rate for the test liquid at room temperature is 64%.

[0055] 2. Evaluation of viscosity reduction performance of corrosion inhibition and viscosity reduction composition at 20℃, 50℃ and 80℃

[0056] The viscosity of the heavy oil used in this experiment is as follows:

[0057] Heavy oil: Viscosity is 16800mPa.s at 50°C.

[0058] The viscosity reducing performance of the corrosion inhibition and viscosity reducing compositions prepared in Examples 1 to 3 on heavy oil at 80° C., 50° C. and 20° C. was measured. The specific steps are as follows:

[0059] a. Take the heavy oil with viscosity of 16800mPa.s at 50℃ as blank control;

[0060] b. The corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 were mixed with heavy oil, respectively, the mass of the corrosion inhibition and viscosity reduction composition being 0.3wt% of the mass of the heavy oil, to obtain heavy oil treated with different corrosion inhibition and viscosity reduction compositions;

[0061] c. The viscosity values ​​of the blank control group (i.e., heavy oil) and the experimental group (i.e., heavy oil treated with the corrosion inhibition and viscosity reduction composition prepared in Examples 1 to 3) at 80°C, 50°C and 20°C were measured using the RND-1 petroleum product kinematic viscosity tester produced by Jilin Ruigu Scientific Instrument Co., Ltd. The specific results are shown in Table 2.

[0062] Table 2. Viscosity reduction performance of the corrosion inhibition and viscosity reduction composition on heavy oil at 80°C, 50°C and 20°C

[0063]

[0064] By comparing the blank control data in Table 2 with the data of Examples 1 to 3, it can be seen that the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 have a certain degree of viscosity reduction effect on heavy oil in the temperature range of 20°C to 80°C, among which the viscosity reduction effect at 20°C is the best: the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 have a viscosity reduction rate of 60.09% to 62.12% for heavy oil at 20°C; the corrosion inhibition and viscosity reduction composition prepared in Example 2 has a viscosity reduction rate of 62.12% for heavy oil at 20°C.

[0065] 3. Evaluation of corrosion inhibition performance of corrosion inhibition and viscosity reduction composition

[0066] The viscosity of crude oil and heavy oil and the salinity of injected water used in this experiment are as follows:

[0067] Crude oil: viscosity is 57mPa.s at 30°C;

[0068] Heavy oil: viscosity is 16800mPa.s at 50°C;

[0069] Injection water: oilfield produced water with a mineralization of 210,000 mg / L.

[0070] According to the standard SY / T 5273--2000 "Evaluation Method for Corrosion Inhibitor Performance for Oilfield Produced Water" "3 Normal Pressure Static Corrosion Rate and Inhibition Rate Determination Method" the corrosion inhibition performance of the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 was evaluated, and the specific steps are as follows:

[0071] A. Preparation of corrosive medium: crude oil, heavy oil and injection water were mixed uniformly in a mass ratio of 1:1:0.7 to obtain a corrosive medium as a blank control group;

[0072] B. Preparing a corrosive medium containing a corrosion-inhibiting and viscosity-reducing composition: The corrosion-inhibiting and viscosity-reducing compositions prepared in Examples 1 to 3 were mixed with the corrosive medium prepared in step A, respectively, with the mass of the corrosion-inhibiting and viscosity-reducing composition being 0.3 wt % of the mass of the corrosive medium, to obtain three groups of corrosive media containing different corrosion-inhibiting and viscosity-reducing compositions as experimental groups;

[0073] C. Coupon treatment: Use N80 steel sheet, first wipe it with filter paper, then put it into a container filled with petroleum ether with a boiling range of 60 to 90°C, remove the grease on the surface of the N80 steel sheet with absorbent cotton, and then soak it in anhydrous ethanol for 5 minutes for further degreasing and dehydration. Take out the N80 steel sheet and place it on the filter paper, blow it dry with cold air, then wrap the test piece with filter paper, store it in a desiccator, and measure the size and weigh the initial mass after leaving it for 1 hour, accurate to 0.1mg;

[0074] D. Three N80 steel sheets were immersed in a blank control group without the corrosion inhibition and viscosity reduction composition and in each experimental group containing different corrosion inhibition and viscosity reduction compositions, and then taken out after standing at room temperature (25° C.) for 168 hours to obtain corroded N80 steel sheets;

[0075] E. Cleaning of the N80 steel sheet after corrosion: Wipe the corroded N80 steel sheet dry with filter paper, put it into a vessel of petroleum ether with a boiling range of 60 to 90°C, remove the oil stains on the surface of the N80 steel sheet with absorbent cotton, and then soak it in anhydrous ethanol for 5 minutes for further degreasing and dehydration; then soak the corroded N80 steel sheet in an acid cleaning solution (mixed with 100mL concentrated hydrochloric acid and 5g hexamethylenetetramine, diluted with water to 1000mL) for 5 minutes, and at the same time, use tweezers to hold a small amount of absorbent cotton to gently wipe the corrosion products on the surface of the N80 steel sheet, then take out the N80 steel sheet, rinse the residual acid on the surface with tap water, and immediately immerse it in a sodium hydroxide aqueous solution with a mass concentration of 60g / L, soak for 30s, then rinse with tap water, and then soak it in anhydrous ethanol for 5 minutes, and wash and dehydrate twice. Finally, the corroded N80 steel sheet after the above cleaning treatment is placed on the filter paper, blown dry with cold air, and then wrapped with filter paper and stored in a desiccator. After 1 hour, the mass of the corroded N80 steel sheet is weighed, with an accuracy of 0.1 mg.

[0076] F. The uniform corrosion rate of each N80 steel sheet is calculated by formula (1), and then the arithmetic mean of the uniform corrosion rates of the three N80 steel sheets in the same group is taken as the measurement result of the group.

[0077]

[0078] Among them, r corr is the uniform corrosion rate, in mm / a;

[0079] m is the initial mass of the N80 steel sheet, in g;

[0080] m t is the mass of the corroded N80 steel sheet, in g;

[0081] S1 is the area of ​​N80 steel sheet, in cm 2 ;

[0082] t is the experimental time, in h;

[0083] ρ is the density of N80 steel sheet material, in g / cm 3 .

[0084] G. The corrosion inhibition rate of each N80 steel sheet is further calculated by formula (2), and then the arithmetic mean of the corrosion inhibition rates corresponding to the three N80 steel sheets in the same group is taken as the measurement result of the group.

[0085]

[0086] Wherein, η is the corrosion inhibition rate, in %;

[0087] Δm0 is the mass loss of N80 steel sheet in the blank control group, in g;

[0088] Δm1 is the mass loss of N80 steel sheet in the experimental group, in g.

[0089] The results are shown in Table 3.

[0090] Table 3. Evaluation of corrosion inhibition performance of corrosion inhibition and viscosity reduction composition

[0091] Serial number Uniform corrosion rate (mm / a) Corrosion inhibition rate (%) Blank control 0.173 / Example 1 0.042 75.72 Example 2 0.034 80.35 Example 3 0.046 73.41

[0092] From the data in Table 3, it can be seen that the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 have good corrosion inhibition effects: the corrosion inhibition and viscosity reduction composition prepared in Example 1 has a corrosion inhibition rate of 75.72% for N80 steel sheet, the corrosion inhibition rate of the corrosion inhibition and viscosity reduction composition prepared in Example 2 is 80.35% for N80 steel sheet, and the corrosion inhibition performance is the best, and the corrosion inhibition rate of the corrosion inhibition and viscosity reduction composition prepared in Example 3 is 73.41% for N80 steel sheet. It shows that the corrosion inhibition and viscosity reduction composition has a significant corrosion inhibition effect.

[0093] The data in Table 1 and Table 2 reflecting the viscosity reduction performance of the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 obtained from the comprehensive experiments 1 to 3 and the experimental data in Table 3 reflecting the corrosion inhibition performance of the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 can be known: at room temperature, the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 have a viscosity reduction rate of 59.04%, 64% and 62.91% for the test liquid obtained by mixing crude oil, heavy oil and injection water in a mass ratio of 1:1:0.7, respectively; at 20°C, the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 have a viscosity reduction rate of 59.04%, 64% and 62.91% for the test liquid obtained by mixing crude oil, heavy oil and injection water in a mass ratio of 1:1:0.7, respectively; at 20°C, the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 have a viscosity reduction rate of 25660 mPa s at 20°C. .s) are 60.09%, 62.12% and 61.11% respectively; at 50°C, the viscosity reduction rates of the corrosion inhibition and viscosity reducing compositions prepared in Examples 1 to 3 for heavy oil (viscosity of 16800mPa.s at 50°C) are 46.9%, 49.82% and 48.10% respectively; at 80°C, the viscosity reduction rates of the corrosion inhibition and viscosity reducing compositions prepared in Examples 1 to 3 for heavy oil (viscosity of 8340mPa.s at 80°C) are 29.74%, 34.89% and 32.13% respectively, indicating that the corrosion inhibition and viscosity reducing compositions prepared in Examples 1 to 3 have viscosity reducing properties. At room temperature, the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 have corrosion inhibition rates of 75.72%, 80.35% and 73.41% for N80 steel sheets in a corrosive medium obtained by mixing crude oil, heavy oil and injection water in a mass ratio of 1:1:0.7, respectively, indicating that the corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 have corrosion inhibition performance. Combining the above two points, it is further proved that the imidazoline compounds, paraben compounds, polyacrylic acid and dimethyl carbonate have synergistic effects in terms of viscosity reduction and corrosion inhibition performance. The corrosion inhibition and viscosity reduction compositions prepared in Examples 1 to 3 have both corrosion inhibition performance and viscosity reduction effect, and are corrosion inhibitors with viscosity reduction function.

[0094] Although the present invention has been described with reference to specific embodiments, it will be appreciated by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention. In addition, the subject matter, spirit and scope of the present invention may be varied to accommodate specific situations, materials, material combinations and methods. All of these changes are included within the scope of the claims of the present invention.

Claims

1. A corrosion inhibition and viscosity reduction composition, comprising an imidazoline compound, a p-hydroxybenzoate compound, dimethyl carbonate and polyacrylic acid.

2. The corrosion inhibition and viscosity reduction composition according to claim 1, characterized in that: The corrosion inhibition and viscosity reduction composition further comprises maleic acid and a solvent; Preferably, the solvent is a lower alcohol.

3. The corrosion inhibition and viscosity reduction composition according to claim 2, characterized in that: Based on the quality of the corrosion inhibition and viscosity reduction composition, the corrosion inhibition and viscosity reduction composition comprises: Preferably, the corrosion inhibition and viscosity reduction composition comprises:

4. The corrosion inhibition and viscosity reduction composition according to any one of claims 1 to 3, characterized in that: The imidazoline compound is selected from at least one of aminoethyl heptadecenyl imidazoline, imidazoline ester and lauryl imidazoline.

5. The corrosion inhibition and viscosity reduction composition according to claim 4, characterized in that: The imidazoline compound is lauryl imidazoline.

6. The corrosion inhibition and viscosity reduction composition according to any one of claims 1 to 5, characterized in that: The paraben compound is selected from at least two of methyl paraben, ethyl paraben and propyl paraben.

7. The corrosion inhibition and viscosity reduction composition according to claim 6, characterized in that: The parahydroxybenzoic acid ester compound is a mixture of methyl parahydroxybenzoate and ethyl parahydroxybenzoate; Preferably, the molar ratio of methyl parahydroxybenzoate to ethyl parahydroxybenzoate is 1:0.

8.

8. The corrosion inhibition and viscosity reduction composition according to any one of claims 1 to 7, characterized in that: The weight average molecular weight of the polyacrylic acid is 3000 to 5000; Preferably, the weight average molecular weight of the polyacrylic acid is 5,000.

9. A method for preparing the corrosion inhibition and viscosity reduction composition according to any one of claims 1 to 8, comprising the following steps: The imidazoline compound, the p-hydroxybenzoate compound, dimethyl carbonate and polyacrylic acid are mixed, heated and cooled to obtain the corrosion inhibition and viscosity reduction composition.

10. The method according to claim 9, characterized in that The imidazoline compound, the p-hydroxybenzoate compound, dimethyl carbonate, polyacrylic acid, maleic acid and a solvent are mixed, and then heated; Preferably, the heating temperature is 80°C to 90°C.

11. Use of the corrosion-inhibiting and viscosity-reducing composition according to any one of claims 1 to 8 or any one of the corrosion-inhibiting and viscosity-reducing compositions prepared by the method according to claim 9 or 10 in the field of oilfield corrosion protection technology, especially as a corrosion inhibitor with viscosity-reducing effect.

Citation Information

Patent Citations

  • Water-soluble macromolecular corrosion inhibitor with viscosity reduction effect and preparation method of water-soluble macromolecular corrosion inhibitor

    CN107541199A

  • Neutral plug removal treating agent and preparation method thereof

    CN108102624A

  • Viscosity reducing corrosion inhibitor for viscous oil mining, gathering and transportation and preparation method thereof