Manufacturing process of working roll of roughing mill
By optimizing the chemical composition and process flow, adding Ni and ferroniobium alloy, an efficient bainite + tempered sorbite + carbide structure is formed, which solves the problems of poor thermal fatigue resistance and short rolling life of the roughing mill work rolls. Achieved higher wear resistance and thermal cracking resistance, extending roll life.
Patent Information
- Application Number
- CN202411273855.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-10-18
AI Technical Summary
The existing roughing mill work rolls have problems with poor heat fatigue resistance and short rolling life during the rolling process. Especially due to insufficient addition of heat-resistant alloy Ni, the rolls are prone to hot cracks and wear at high temperatures.
By optimizing the chemical composition, increasing the Ni content, and adding Mg, rare earth yttrium and ferroniobium alloy, the pearlite ductile iron blank is prepared by integral casting, and is subjected to high-temperature annealing and quenching heat treatment to form bainite + tempered sorbite + carbide. The organizational structure improves thermal fatigue resistance and wear resistance.
It significantly improves the rolling life of the roughing mill work rolls, extending the service life to twice that of similar products in the same industry. It also reduces the amount of grinding and production costs, and improves the wear resistance and hot cracking resistance of the rolls.
Smart Images

Figure CN118792572A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rolling and relates to a manufacturing process of a working roll of a rough rolling mill. Background Art
[0002] After being heated in a heating furnace, the conventional hot rolling mill slab is generally rolled into an intermediate slab with a certain thickness by a rough rolling mill, and then rolled into a plate coil with a thickness that meets customer requirements by a finishing mill. When the slab is rolled in the rough rolling mill, it is generally rolled several times to ensure that the intermediate slab has a certain temperature and plate shape, creating good conditions for the subsequent finishing mill to continue rolling.
[0003] In recent years, with the development of high-speed and continuous rolling of wire rod mills at home and abroad, and the continuous improvement of rolled materials, steel mills have higher and higher requirements for the applicability of rolls. Roughing mills have the characteristics of high rolling temperature, low rolling speed and large reduction. Especially in recent years, the rolled materials have been long in length and the roughing rolls have been heated for a long time. Therefore, the rolls are not only required to have good wear resistance and high strength, but also better heat crack resistance and rolling life.
[0004] Chinese patent CN 201911392869.4 discloses a working roll for a rough rolling mill stand for wire rods and a manufacturing method thereof, wherein the chemical composition and weight percentage of each component are: C 2.9~3.6%, Si 1.2~2.0%, Mn 0.3~0.8%, Cr 0.2~1.0%, Ni 1.0~2.0%, Mo 0.2~0.5%, P≤0.15, S≤0.3, and the rest are Fe and unavoidable impurities. The manufacturing method is to cast the pearlite ductile iron blank by integral casting, and then quench and heat treat it to obtain a rough rolling mill stand with a structure of bainite + tempered troostite + carbide. The patent not only reduces the hardness difference between the inside and outside of the working layer, but also improves the wear resistance and reduces the probability of thermal cracks at the bottom of the roll groove. However, the addition amount of heat-resistant alloy Ni in the patent is low, and the thermal fatigue resistance is poor, which reduces the rolling life of the rough rolling mill working roll. Summary of the invention
[0005] In order to solve the technical problems in the background technology, the purpose of the present invention is to provide a manufacturing process for the working rolls of a rough rolling mill. Through formula optimization, pearlite ductile iron blanks are prepared by integral casting, and after high-temperature annealing, rough machining and quenching heat treatment are performed to improve the grain size and thermal fatigue resistance of the pearlite ductile iron blank, thereby improving the rolling life of the working rolls of the rough rolling mill.
[0006] In order to achieve the above object, the present invention provides a manufacturing process for a roughing mill working roll, comprising: S1, integrally casting to prepare a pearlite ductile iron blank, and performing hot unpacking high temperature annealing treatment to obtain an annealed pearlite ductile iron blank; S2. The pearlite ductile iron blank after annealing is subjected to rough machining and quenching heat treatment to obtain a roughing mill working roll. The chemical composition of the roughing mill working roll and the weight percentage of each component are as follows: C 3.4%~3.7%; Si 1.5%~2.1%; Mn 0.4%~1.0%; Cr0.35%~1.0%; Ni 2.01%~2.5%; Mo 0.35%~0.6%; P≤0.05%; S≤0.03%; Mg ≥ 0.04%; Y≥0.02%; The rest is Fe and unavoidable impurities; Wherein, ferroniobium alloy is added during smelting, and the amount of ferroniobium alloy added is 0.1% to 0.4% of the total weight of the raw materials.
[0007] In a preferred embodiment, the ferroniobium alloy is one or more of FeNb50, FeNb60, FeNb65, and FeNb70.
[0008] In the present invention, by adding Mg and rare earth yttrium, the crystal structure can be refined, the density of the structure can be improved, and the decay of large-section ductile iron can be prevented; by adding 0.1% to 0.4% of ferroniobium alloy, the matrix structure is refined to break the network carbides in the eutectic structure and form small blocks or granules, fatigue cracks are prevented from penetrating along the network carbides during steel rolling, the depth of the fatigue layer is reduced, and the amount of grinding is reduced; by increasing the amount of Ni added, the thermal fatigue resistance of the alloy is improved.
[0009] In a preferred embodiment, in step S1, the integral casting is used to prepare the pearlite ductile iron blank, specifically: 1.1) Modeling: composite sand box is used, metal sand box is used for roller body, and 2~3mm high aluminum powder casting coating is sprayed on the metal sand box of upper roller neck and lower roller neck; 1.2) Melting: Smelting is carried out in a medium frequency furnace. The materials of the roller body, upper roller neck and lower roller neck are all ductile iron. The smelting temperature is 1500~1550℃. Inoculant and spheroidizing agent are added into the molten iron before it is taken out of the furnace to perform inoculation and spheroidization treatment on the molten iron; 1.3) Pouring: bottom pouring; 1.4) Unpacking: Cool to 800~950℃ and unpack. Quickly transfer to an insulation material box for high temperature annealing. When the pearlite ductile iron blank cools to 500~700℃, remove it for air cooling. After cooling to room temperature, perform rough processing.
[0010] Furthermore, in step 1.2), the inoculant added to the molten iron is 75 ferrosilicon and long-acting silicon-barium, and the added amount is 0.4%~1.0% of the total amount of the molten iron; the spheroidizer is heavy rare earth magnesium alloy, and the added amount is 0.6%~0.8% of the total amount of the molten iron.
[0011] In a preferred embodiment, in step S2, the quenching heat treatment is specifically: 2.1) High temperature quenching: The semi-finished working roll after rough processing is heated to 850~950℃ in an air furnace for high temperature quenching; The high-temperature quenching and holding time is determined according to the formula t=L÷25mm / h, where t represents the high-temperature quenching and holding time in h, and L represents the depth of the hardened layer of the semi-finished working roll in mm; 2.2) Cooling: After the semi-finished work rolls are taken out of the furnace at high temperature, they are first cooled by water spray for 5 to 60 minutes. After the water is stopped and the heat is returned for 10 to 300 seconds, water spray treatment is carried out again. After the cycle is returned to heat, the final cooling temperature is 300 to 420°C; 2.3) Medium temperature tempering: The cooled semi-finished working roll is placed in an air furnace, heated to the tempering temperature and kept warm for a predetermined time. The tempering temperature is 350~420℃, and the tempering holding time is 4~5 times the high temperature quenching holding time. Then the temperature is lowered to the set temperature and taken out of the furnace.
[0012] Furthermore, in step 2.2), the water pressure is 0.4-0.6 MPa and the water flow rate is 6.0 m 3 / h~8.0m 3 / h, intermittent water spraying time is 35~40 minutes in total, and cooling time in air is 30~60 minutes.
[0013] Furthermore, in step 2.3), after the temperature is raised to the tempering temperature and kept for a predetermined time, the temperature is lowered to 80-160°C at a rate of 10-20°C / min and the product is taken out of the furnace.
[0014] Compared with the prior art, the present invention has at least the following advantages: The present invention rationally designs the chemical composition of the roller. By adding Mg and rare earth yttrium, the crystal structure can be refined, the density of the structure can be improved, and the decay of large-section ductile iron can be prevented; 0.1% to 0.4% of ferroniobium alloy is added to refine the matrix structure so that the network carbides in the eutectic structure are broken and small blocks or granularized, ensuring that the eutectic network carbides are broken and dispersed, preventing fatigue cracks from penetrating along the network carbides during steel rolling, reducing the depth of the fatigue layer, and thus reducing the amount of grinding; by increasing the amount of Ni added, the thermal fatigue resistance of the alloy is improved. Through the optimization of the formula, the grain size and thermal fatigue resistance of the pearlite ductile iron blank are improved, and the life of the roller is twice that of similar products in the same industry.
[0015] (2) The present invention adopts the method of high temperature quenching + medium temperature tempering to change the matrix structure of the roller body, thereby obtaining a bainite + tempered troostite + carbide structure with higher strength and better applicability, thereby improving the wear resistance of the product. After quenching, the hardness difference between the inside and outside of the working layer of the roller body is very small, thereby ensuring consistent performance during the use of the product. The wear resistance and thermal cracking resistance of the product are higher, and the surface quality of the groove bottom of the roller is good during use, thereby improving the rolling quality of steel.
[0016] (3) The cooling method of the present invention adopts a water spray + indirect cooling + air cooling method. This method is not only environmentally friendly, but also low in cost. The circulating water can be reused. After the high-temperature working roll is taken out of the furnace, the roll body is immediately sprayed with water for rapid cooling, so that the matrix structure avoids the pearlite transformation zone from austenite to the bainite phase transformation zone to complete the bainite transformation and achieve the purpose of refining the structure. Afterwards, in order to ensure the depth of the hardened layer of the roll body and the safety of the product after the temperature continues to drop, a more gentle water stop and heat recovery, circulating spray heat recovery and air cooling are used. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is the metallographic image of the product prepared in Example 1 (100 times); Figure 2 This is the metallographic image of the product prepared in Example 1 (400 times); Figure 3 The surface state of the groove bottom of the roughing mill working roll after it comes off the mill obtained in Example 1 (partial 1); Figure 4 The surface state of the groove bottom of the roughing mill working roll after it comes off the mill obtained in Example 1 (partial 2); Figure 5 The surface state of the groove bottom of the roughing mill work roll after it comes off the mill obtained in Example 1 (overall); Figure 6 This is the metallographic image of the product prepared in Comparative Example 1 (100 times); Figure 7 This is the metallographic image of the product prepared in Comparative Example 1 (400 times); Figure 8 This is the surface state of the groove bottom after the working roll of the rough rolling mill obtained in Comparative Example 1 comes off the mill. DETAILED DESCRIPTION
[0018] The specific implementation modes of the present invention will be described clearly and completely below with reference to the accompanying drawings.
[0019] Example 1
[0020] A manufacturing process for a roughing mill working roll, the chemical composition of the roughing mill working roll and the weight percentage of each component are: C 3.42%; Si 1.58%; Mn 0.55%; Cr 0.36%; Ni 2.01%; Mo 0.35%; P 0.04%; S 0.012%; Mg 0.05%; Y 0.03%; the rest are Fe and unavoidable impurities; wherein 0.1% niobium iron alloy is added during smelting, and the niobium iron alloy is FeNb65.
[0021] The manufacturing process of the roughing mill work roll includes: S1, integrally casting to prepare a pearlite ductile iron blank, and performing hot unpacking high temperature annealing treatment to obtain an annealed pearlite ductile iron blank; 1.1) Modeling: composite sand box is used, metal sand box is used for roller body, and 2~3mm high aluminum powder casting coating is sprayed on the metal sand box of upper roller neck and lower roller neck; 1.2) Melting: Smelting is carried out in a medium frequency furnace. The materials of the roller body, upper roller neck and lower roller neck are all ductile iron. The smelting temperature is 1500~1550℃. The inoculant added to the molten iron before leaving the furnace is 75 ferrosilicon and long-acting silicon-barium, and the addition amount is 0.4% of the total amount of molten iron. The spheroidizing agent is heavy rare earth magnesium alloy, and the addition amount is 0.8% of the total amount of molten iron. The molten iron is inoculated and spheroidized. 1.3) Pouring: Use bottom pouring method, after pouring, point the gate to supplement the shrinkage riser; 1.4) Unpacking: Cool to 900℃ and unpack, then quickly transfer to an insulation material box for high temperature annealing. When the pearlite ductile iron blank cools to 600℃, remove it for air cooling, and then cool to room temperature for rough processing; S2. The pearlite ductile iron blank after annealing is subjected to rough machining and quenching heat treatment to obtain a rough rolling mill working roll, wherein the quenching heat treatment is specifically as follows: 2.1) High temperature quenching: After rough processing, the semi-finished working roll is heated to 850℃ in an air furnace for high temperature quenching. The high temperature quenching holding time is 4h. The semi-finished working roll body diameter is φ610mm; 2.2) Cooling: After the semi-finished working roll is taken out of the furnace at high temperature, it is first cooled by water spraying for 15 minutes, with a water pressure of 0.4MPa and a water flow rate of 6.0m 3 / h, stop water and return to heat for 120 seconds, then spray water again, after the cycle return to heat, the total intermittent water spraying time is 38 minutes, the cooling time in the air is 40 minutes, and the final cooling temperature is 350℃; 2.3) Medium temperature tempering: The cooled semi-finished working roll is placed in an air furnace, heated to the tempering temperature and kept warm for a predetermined time. The tempering temperature is 380°C, the tempering holding time is 18h, and the roll is cooled to 120°C at a rate of 15°C / min before being taken out of the furnace.
[0022] The metallographic structure of the working rolls for the roughing mill prepared in Example 1 was observed and tested using a metallographic detector. Figure 1-2 As shown in the figure, it can be seen that through the optimization of the formula, the grain size of the pearlite ductile iron blank is improved, the crystal structure is refined, the density of the structure is improved, and the decline of the large-section ductile iron is prevented; 0.1%~0.4% of ferroniobium alloy is added to refine the matrix structure, so that the network carbides in the eutectic structure are broken and small blocks or granular, ensuring that the eutectic network carbides are broken and dispersed, preventing fatigue cracks from penetrating along the network carbides during steel rolling, reducing the depth of the fatigue layer, and thus reducing the amount of grinding; by increasing the amount of Ni added, the thermal fatigue resistance of the alloy is improved.
[0023] The tensile strength of the working roll for the rough rolling stand prepared in Example 1 was tested using a universal material testing machine. The higher the tensile strength, the higher the ability of the roll to resist accidents during use. The test results of this example show that the tensile strength of the roll diameter is 690 MPa.
[0024] The working rolls for the rough rolling stand prepared in Example 1 were tested in the third rough rolling stand of Xianggang High-speed Wire Route. The single rolling volume reached 16,000 tons, which is twice that of the pearlite product. The surface quality of the product after unloading was good, without thermal cracks or pits. The grinding amount was ≤10mm, which was 40% lower than that of the pearlite product 25mm. The surface of the groove bottom after unloading was as follows: Figure 3-5 As shown, the roller life is twice that of similar products in the same industry.
[0025] Example 2
[0026] A manufacturing process for a roughing mill working roll, the chemical composition of the roughing mill working roll and the weight percentage of each component are: C 3.55%; Si 1.78%; Mn 0.65%; Cr 0.68%; Ni 2.2%; Mo 0.45%; P 0.04%; S 0.012%; Mg 0.06%; Y 0.04%; the rest are Fe and unavoidable impurities; wherein 0.22% of niobium iron alloy is added during smelting, and the niobium iron alloy is FeNb50.
[0027] The manufacturing process of the roughing mill work roll includes: S1, integrally casting to prepare a pearlite ductile iron blank, and performing hot unpacking high temperature annealing treatment to obtain an annealed pearlite ductile iron blank; 1.1) Modeling: composite sand box is used, metal sand box is used for roller body, and 2~3mm high aluminum powder casting coating is sprayed on the metal sand box of upper roller neck and lower roller neck; 1.2) Melting: Smelting is carried out in a medium frequency furnace. The materials of the roller body, upper roller neck and lower roller neck are all ductile iron. The smelting temperature is 1500~1550℃. The inoculant added to the molten iron before leaving the furnace is 75 ferrosilicon and long-acting silicon-barium, and the addition amount is 0.6% of the total amount of molten iron. The spheroidizing agent is heavy rare earth magnesium alloy, and the addition amount is 0.7% of the total amount of molten iron. The molten iron is inoculated and spheroidized. 1.3) Pouring: Use bottom pouring method, after pouring, point the gate to supplement the shrinkage riser; 1.4) Unpacking: Cool to 900℃ and unpack, then quickly transfer to an insulation material box for high temperature annealing. When the pearlite ductile iron blank cools to 600℃, remove it for air cooling, and then cool to room temperature for rough processing; S2. The pearlite ductile iron blank after annealing is subjected to rough machining and quenching heat treatment to obtain a rough rolling mill working roll, wherein the quenching heat treatment is specifically as follows: 2.1) High temperature quenching: After rough processing, the semi-finished working roll is heated to 900℃ in an air furnace for high temperature quenching. The high temperature quenching holding time is 4h. The semi-finished working roll body diameter is φ610mm; 2.2) Cooling: After the semi-finished working roll is taken out of the furnace at high temperature, it is first cooled by water spraying for 15 minutes, with a water pressure of 0.45MPa and a water flow rate of 8.0m 3 / h, after the water is turned off and the heat is returned for 120 seconds, water spraying is carried out again. After the cycle is returned to heat, the total intermittent water spraying time is 37 minutes, the cooling time in the air is 40 minutes, and the final cooling temperature is 400℃; 2.3) Medium-temperature tempering: The cooled semi-finished working roll is placed in an air furnace, heated to the tempering temperature and kept warm for a predetermined time. The tempering temperature is 420°C, the tempering holding time is 18h, and the roll is cooled to 120°C at a rate of 15°C / min before being taken out of the furnace.
[0028] The tensile strength of the working roll for the rough rolling stand prepared in Example 2 was tested using a universal material testing machine. The test results of this example showed that the tensile strength of the roll diameter was 620 MPa.
[0029] The working rolls for the rough rolling stand prepared in Example 2 were tested on the third rough rolling stand of Xianggang High-speed Wire Route, with a single rolling volume of 12,000 tons, which is twice that of pearlite products. After leaving the machine, the surface quality of the working rolls was good, without thermal cracks, and the grinding amount was 8 mm, which was 50% lower than the 15 mm of pearlite products.
[0030] Example 3
[0031] A manufacturing process for a roughing mill working roll, the chemical composition of the roughing mill working roll and the weight percentage of each component are: C 3.65%; Si 2.1%; Mn 0.6%; Cr 0.7%; Ni 2.38%; Mo 0.58%; P 0.04%; S 0.011%; Mg 0.05%; Y 0.03%; the rest are Fe and unavoidable impurities; wherein 0.4% niobium iron alloy is added during smelting, and the niobium iron alloy is FeNb60.
[0032] The manufacturing process of the roughing mill work roll includes: S1, integrally casting to prepare a pearlite ductile iron blank, and performing hot unpacking high temperature annealing treatment to obtain an annealed pearlite ductile iron blank; 1.1) Modeling: composite sand box is used, metal sand box is used for roller body, and 2~3mm high aluminum powder casting coating is sprayed on the metal sand box of upper roller neck and lower roller neck; 1.2) Melting: Smelting is carried out in a medium frequency furnace. The materials of the roller body, upper roller neck and lower roller neck are all ductile iron. The smelting temperature is 1500~1550℃. The inoculant added to the molten iron before leaving the furnace is 75 ferrosilicon and long-acting silicon-barium, and the addition amount is 0.65% of the total amount of molten iron. The spheroidizing agent is heavy rare earth magnesium alloy, and the addition amount is 0.7% of the total amount of molten iron. The molten iron is inoculated and spheroidized. 1.3) Pouring: Use bottom pouring method, after pouring, point the gate to supplement the shrinkage riser; 1.4) Unpacking: Cool to 900℃ and unpack, then quickly transfer to an insulation material box for high temperature annealing. When the pearlite ductile iron blank cools to 600℃, remove it for air cooling, and then cool to room temperature for rough processing; S2. The pearlite ductile iron blank after annealing is subjected to rough machining and quenching heat treatment to obtain a rough rolling mill working roll, wherein the quenching heat treatment is specifically as follows: 2.1) High temperature quenching: After rough processing, the semi-finished working roll is heated to 920℃ in an air furnace for high temperature quenching. The high temperature quenching holding time is 2.5h. The semi-finished working roll body diameter is φ610mm; 2.2) Cooling: After the semi-finished working roll is taken out of the furnace at high temperature, it is first cooled by water spraying for 15 minutes, with a water pressure of 0.4MPa and a water flow rate of 8.0m 3 / h, stop water and return to heat for 120 seconds, then spray water again, after the cycle returns to heat, the total intermittent water spraying time is 40 minutes, the cooling time in the air is 60 minutes, and the final cooling temperature is 380℃; 2.3) Medium-temperature tempering: The cooled semi-finished working roll is placed in an air furnace, heated to the tempering temperature and kept warm for a predetermined time. The tempering temperature is 400°C, the tempering holding time is 12h, and the roll is cooled to 120°C at a rate of 15°C / min before being taken out of the furnace.
[0033] The tensile strength of the working roll for the rough rolling stand prepared in Example 3 was tested using a universal material testing machine. The test results of this example showed that the tensile strength of the roll diameter was 715 MPa.
[0034] The working rolls for the rough rolling stand prepared in Example 3 were tested on the third rough rolling stand of Xiangtan Steel's high-speed wire. The single rolling volume reached 20,000 tons, which is 2.5 times that of the pearlite product. After leaving the machine, the surface quality of the product was good, without thermal cracks. The grinding amount was 8 mm, which was 40% lower than the 20 mm of the pearlite product.
[0035] Comparative Example 1
[0036] The process steps of this comparative example are the same as those of Example 1, and the difference from Example 1 is that: Mg, Y and ferro-niobium alloy are not added in Comparative Example 1; the metallographic image of the product prepared in Comparative Example 1 is as follows: Figure 6-7 shown.
[0037] The tensile strength of the working roll for the rough rolling stand prepared in Comparative Example 1 was tested using a universal material testing machine. The test results of this embodiment showed that the tensile strength of the roll diameter was 480 MPa.
[0038] The working rolls for the rough rolling stand prepared in Comparative Example 1 were tested on the third rough rolling stand of Xianggang High-speed Wire Route, with a single rolling volume of 8,000 tons. After the product was unloaded from the machine, the surface cracks were severe. Figure 8 As shown, thermal cracks appeared on the bottom surface of the tank after it was removed from the machine, and its service life was reduced.
[0039] In summary, the present invention rationally designs the chemical composition of the roll, and ensures the dispersed distribution of the eutectic carbide network by adding Mg, Y and an appropriate amount of niobium iron alloy, thereby preventing the thermal cracks from extending along the carbides, and obtaining a work roll structure of bainite + tempered troostite + carbide, thereby improving the thermal cracking resistance of the roll body, and reducing the production cost while ensuring the thermal cracking resistance; by optimizing the formula, the grain size of the pearlite ductile iron blank is increased, and ultimately the roll life is increased.
[0040] The above are only preferred embodiments of the present invention, and only describe the implementation methods of the present invention. They do not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A manufacturing process for a roughing mill working roll, characterized in that: include: S1, integrally casting to prepare a pearlite ductile iron blank, and performing hot unpacking high temperature annealing treatment to obtain an annealed pearlite ductile iron blank; S2. The pearlite ductile iron blank after annealing is subjected to rough machining and quenching heat treatment to obtain a roughing mill working roll; the chemical composition of the roughing mill working roll and the weight percentage of each component are: C 3.4%~3.7%; Si 1.5%~2.1%; Mn 0.4%~1.0%; Cr 0.35%~1.0%; Ni 2.01%~2.5%; Mo 0.35%~0.6%; P≤0.05%; S≤0.03%; Mg ≥ 0.04%; Y≥0.02%; The rest is Fe and unavoidable impurities; Wherein, ferroniobium alloy is added during smelting, and the amount of ferroniobium alloy added is 0.1% to 0.4% of the total weight of the raw materials.
2. The manufacturing process of the roughing mill working roll according to claim 1, characterized in that: The ferroniobium alloy is one or more of FeNb50, FeNb60, FeNb65 and FeNb70.
3. The manufacturing process of the roughing mill working roll according to claim 1, characterized in that: In step S1, the integral casting is used to prepare a pearlite ductile iron blank, specifically: 1.1) Modeling: composite sand box is used, metal sand box is used for roller body, and 2~3mm high aluminum powder casting coating is sprayed on the metal sand box of upper roller neck and lower roller neck; 1.2) Melting: Smelting is carried out in a medium frequency furnace. The materials of the roller body, upper roller neck and lower roller neck are all ductile iron. The smelting temperature is 1500~1550℃. Inoculant and spheroidizing agent are added into the molten iron before it is taken out of the furnace to perform inoculation and spheroidization treatment on the molten iron; 1.3) Pouring: bottom pouring; 1.4) Unpacking: Cool to 800~950℃ and unpack. Quickly transfer to an insulation material box for high temperature annealing. When the pearlite ductile iron blank cools to 500~700℃, remove it for air cooling. After cooling to room temperature, perform rough processing.
4. The manufacturing process of the roughing mill working roll according to claim 3, characterized in that: In step 1.2), the inoculant added to the molten iron is 75% ferrosilicon and long-acting silicon-barium, and the added amount is 0.4%~1.0% of the total amount of the molten iron. The spheroidizer is heavy rare earth magnesium alloy, and the added amount is 0.6%~0.8% of the total amount of the molten iron.
5. The manufacturing process of the roughing mill working roll according to claim 1, characterized in that: In step S2, the quenching heat treatment is specifically: 2.1) High temperature quenching: The semi-finished working roll after rough processing is heated to 850~950℃ in an air furnace for high temperature quenching; The high-temperature quenching and holding time is determined according to the formula t=L÷25mm / h, where t represents the high-temperature quenching and holding time in h, and L represents the depth of the hardened layer of the semi-finished working roll in mm; 2.2) Cooling: After the semi-finished work rolls are taken out of the furnace at high temperature, they are first cooled by water spray for 5 to 60 minutes. After the water is stopped and the heat is returned for 10 to 300 seconds, water spray treatment is carried out again. After the cycle is returned to heat, the final cooling temperature is 300 to 420°C; 2.3) Medium temperature tempering: The cooled semi-finished working roll is placed in an air furnace, heated to the tempering temperature and kept warm for a predetermined time. The tempering temperature is 350~420℃, and the tempering holding time is 4~5 times the high temperature quenching holding time. Then the temperature is lowered to the set temperature and taken out of the furnace.
6. The manufacturing process of the roughing mill working roll according to claim 5, characterized in that: In step 2.2), the water pressure is 0.4~0.6MPa and the water flow rate is 6.0m 3 / h~8.0m 3 / h, intermittent water spraying time is 35~40 minutes in total, and cooling time in air is 30~60 minutes.
7. The manufacturing process of the roughing mill working roll according to claim 5, characterized in that: In step 2.3), after heating to the tempering temperature and keeping it for a predetermined time, the temperature is lowered to 80-160°C at a rate of 10-20°C / min and taken out of the furnace.
Citation Information
Patent Citations
Working roller for wire and bar roughing mill stand and manufacturing method thereof
CN111101053A
Hot continuous rolling two-roller rough rolling working roller and preparation method thereof
CN112831718A
Hardened roll for rolling and its manufacture
JP1993311334A
Manufacturing method of compound roll for hott rolling
JP2016093839A