Manufacturing method of aluminum bonding pad on power semiconductor device

By electroplating aluminum, aluminum pads are formed directly on the surface of the semiconductor chip, which solves the problems of long cycle time, high consumption, and difficulty in manufacturing in the existing aluminum pad production methods, and achieves cost reduction and production efficiency improvement.

CN118792708APending Publication Date: 2024-10-18SANLEI (NINGBO) NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410831449.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In the existing aluminum pad production method, the physical vapor deposition process cycle is long, consumes high-purity aluminum targets, photoresists, and cleaning solutions. As the power of power semiconductor devices increases, the thickness of the aluminum layer increases, making manufacturing difficult and etching time. extend.

Method used

Using the method of electroplating aluminum, the ionic liquid plating solution is used for electroplating in a protective gas environment to form aluminum pads directly on the surface of the semiconductor chip, eliminating the need for glue coating, etching, glue removal, wet cleaning and other process steps, and reducing equipment investment. and time.

Benefits of technology

It significantly reduces costs, shortens aluminum deposition time, improves deposition efficiency, reduces process links, and ensures the thickness and quality stability of aluminum pads.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792708A_ABST
    Figure CN118792708A_ABST
Patent Text Reader

Abstract

The invention provides a method for manufacturing an aluminum bonding pad on a power semiconductor device, which comprises the following steps of: S1, taking a wafer which is made into a semiconductor chip and is cleaned and dried as a cathode, taking an aluminum wire as an anode, taking ionic liquid as a plating solution and taking a glass beaker as a plating bath, and placing the components in a box body filled with protective gas; s2, the anode is electrically connected with the positive electrode of a direct-current power source, and the cathode is electrically connected with the negative electrode of the direct-current power source; and S3, electrifying to carry out electroplating, then taking out the wafer, and carrying out solvent ultrasonic cleaning and water washing drying treatment to obtain the power semiconductor device electroplated with the aluminum bonding pad. The method has the beneficial effects that the aluminum bonding pad can be manufactured without a photoetching cleaning step, the cost is reduced, the aluminum deposition efficiency is improved, and the etching time is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a method for manufacturing an aluminum pad on a power semiconductor device. Background Art

[0002] Power semiconductor devices refer to semiconductor devices that can withstand large currents or high voltages. As core components of power electronics technology, power semiconductor devices are widely used in industrial control, communications, consumer electronics, electric vehicles, wind power and solar power generation.

[0003] The main process flow of power semiconductor devices includes: chip processing on wafers (thin film manufacturing, exposure and etching, etc.), chip packaging, and performance testing. Chip packaging is the process of connecting the device to the external circuit and protecting the device. In this step, it is first necessary to deposit a metal film on the surface of the chip to form a pad. Thereafter, the pad is connected to the external components of the chip package by welding. The metal films deposited currently include copper, aluminum, etc., among which aluminum pads are the main ones.

[0004] The existing aluminum pad manufacturing method is to use physical vapor deposition (PVD) process to form an aluminum film layer on the entire wafer surface, and then use glue coating, photosensitization, cleaning, corrosion, and glue removal processes to remove the aluminum coating on the insulating part, so as to form an aluminum pad on the chip surface. Figure 1 As shown, Figure 1 In order to process the wafer into a chip (including the insulating part), aluminum is firstly plated by PVD, thereby forming an aluminum coating on the entire wafer surface, and then glue is applied on the aluminum coating, such as Figure 2 As shown, the glue on the insulating part is then removed by photosensitive and cleaning. Figure 3 As shown; then the aluminum coating on this part is corroded to form Figure 4 The structure shown in the figure is finally cleaned off the glue on the aluminum coating to form Figure 5 In the structure shown, there is an aluminum coating (aluminum pad) on the chip and no aluminum on the insulating part of the wafer. Then, the wafer is cut along the insulating part to finally form multiple power semiconductor devices (chips).

[0005] However, the above aluminum pad manufacturing method has the following problems:

[0006] 1. After aluminum is deposited using the physical vapor deposition (PVD) process, it needs to go through photolithography, cleaning and other steps. The entire cycle takes about 24 hours, and it consumes raw materials such as photoresist and cleaning fluid, which is costly. The cleaning process is also prone to crystal defects, affecting the packaging quality;

[0007] 2. The physical vapor deposition (PVD) process is a vacuum deposition technology, which requires large equipment investment and has low efficiency in depositing aluminum;

[0008] 3. As the power of semiconductor devices increases, a thicker aluminum layer is required, which greatly increases the difficulty of manufacturing aluminum pads by etching (high requirements for the film and long etching time). Summary of the invention

[0009] The technical problem to be solved by the present invention is to realize the manufacture of aluminum pads without the need for photolithography and cleaning steps, thereby reducing costs, improving the efficiency of depositing aluminum, and reducing etching time. In order to overcome the defects of the above-mentioned prior art (or related technology), the present invention provides a method for manufacturing aluminum pads on power semiconductor devices.

[0010] The present invention provides a method for manufacturing an aluminum pad on a power semiconductor device, comprising:

[0011] Step S1, using a semiconductor chip wafer that has been cleaned and dried as a cathode, an aluminum wire as an anode, an ionic liquid as a plating solution, and a glass beaker as a plating tank, all of which are placed in a box filled with a protective gas;

[0012] Step S2, electrically connecting the anode to the positive electrode of a DC power supply, and electrically connecting the cathode to the negative electrode of the DC power supply;

[0013] Step S3, power is turned on for electroplating, and then the wafer is taken out and subjected to solvent ultrasonic cleaning and water washing and drying treatment to obtain a power semiconductor device electroplated with an aluminum pad.

[0014] Compared with the prior art, the manufacturing method of an aluminum pad on a power semiconductor device in the present application has the following advantages: the aluminum pad is manufactured by the method of electroplating aluminum in the present application, and there is no need for process steps such as coating, etching, degumming, wet cleaning, etc., so the consumption of materials such as high-purity aluminum target, photoresist, degumming liquid, cleaning liquid, etc. can be greatly reduced, and the investment in PVD, coating, cleaning and other equipment can be reduced, or the occupancy time of these equipment can be reduced, thereby achieving a significant reduction in costs. In addition, while reducing the process steps, the etching time can also be significantly shortened, and the efficiency of depositing aluminum can be improved.

[0015] In a possible implementation, in step S1, the ionic liquid used is aluminum chloride-imidazole, aluminum chloride-pyridine, aluminum chloride-quaternary ammonium, or aluminum chloride-pyrrole.

[0016] In a possible implementation, in the step S1, the ionic liquid is an AlCl3-EMIC ionic liquid with a molar ratio of 1.5 to 2.0.

[0017] In a possible implementation, in step S3, the molar ratio of the AlCl3-EMIC ionic liquid used is 2.0.

[0018] Compared with the prior art, after adopting the above technical scheme, considering that in the AlCl3-EMIC ionic liquid, aluminum can be electroplated only when the molar ratio of AlCl3 and EMIC is greater than 1, and the molar ratio of 2.0 is optimal, the effect of aluminum electroplating can be significantly enhanced.

[0019] In a possible implementation manner, in step S3, at a current density in the range of 5 to 80 mA / cm 2 The electroplating is carried out under the conditions of a temperature range of 25 to 80°C and a plating speed range of 1 to 10 μm / min.

[0020] In a possible implementation, in step S3, the wafer is ultrasonically cleaned using a solvent, and the solvent is alcohol or toluene.

[0021] In a possible implementation manner, in step S3, after the wafer is taken out and subjected to solvent ultrasonic cleaning and water washing and drying treatment, the following step is further included:

[0022] The wafer after the solvent ultrasonic cleaning and water washing and drying treatment is subjected to a heat treatment at 500° C. for 30 minutes. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A schematic diagram of a wafer processed into a chip in the prior art;

[0024] Figure 2 It is a schematic diagram of a wafer after aluminum plating and glue coating in the prior art;

[0025] Figure 3 It is a schematic diagram of a wafer after debonding in the prior art;

[0026] Figure 4 It is a schematic diagram of a wafer after etching the aluminum coating in the prior art;

[0027] Figure 5 It is a schematic diagram of a wafer after cleaning the glue in the prior art;

[0028] Figure 6 is a flow chart of the steps of the present invention;

[0029] Figure 7 is a schematic diagram of an aluminum electroplating device of the present invention;

[0030] Figure 8 This is a schematic diagram of the appearance of a 4-inch wafer after electroplating aluminum pads in Example 1 of the present invention;

[0031] Fig. 9 is a stereoscopic schematic diagram of the wafer surface in Example 1 of the present invention;

[0032] Fig.10is a schematic diagram of a scanning electron microscope of the surface of the aluminum pad in Example 1 of the present invention;

[0033] Fig.11 is a schematic cross-sectional view of an aluminum pad in Example 1 of the present invention;

[0034] Fig.12 This is a schematic diagram of the appearance of a wafer after aluminum plating in Example 2 of the present invention;

[0035] Fig.13 It is a schematic cross-sectional view of the aluminum pad in Example 2 of the present invention. DETAILED DESCRIPTION

[0036] First, those skilled in the art should understand that these implementations are only used to explain the technical principles of the embodiments of the present application, and are not intended to limit the protection scope of the embodiments of the present application. Those skilled in the art can make adjustments to them as needed to adapt to specific application scenarios.

[0037] The present application is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0038] See also Figure 6 and Figure 7 The embodiment of the present application discloses a method for manufacturing an aluminum pad on a power semiconductor device, wherein a wafer made of a semiconductor chip and cleaned and dried is used as a cathode, an aluminum wire is used as an anode, an ionic liquid is used as a plating solution, and a glass beaker is used as a plating tank. The entire device is placed in an argon protective atmosphere glove box, and the cathode and anode are respectively connected to the negative and positive electrodes of a DC power supply, and the current is set according to the total area of ​​the chip. After power is turned on, the wafer is taken out, and after solvent ultrasonic cleaning, it is washed and dried to obtain a power semiconductor device with an aluminum pad electroplated.

[0039] Continue to see Figure 6 In this application, an aluminum pad is manufactured by an electroplating aluminum method. Through electroplating, a metal coating can be obtained on a conductive chip, while the insulating portion is not conductive, so no aluminum coating is produced. In this way, an aluminum pad can be directly obtained on the surface of a conductive chip through electroplating aluminum.

[0040] Continue to see Figure 6 Since aluminum cannot be electrodeposited from an aqueous solution, a non-aqueous electrolyte is required. Currently, there are inorganic molten salt systems, organic solvent systems, and ionic liquid systems for aluminum electroplating. Among them, the inorganic molten salt system has a high operating temperature and has strict requirements on equipment; the organic solvent system is flammable and explosive and is not environmentally friendly; the ionic liquid system has a low operating temperature during aluminum plating, no wastewater and exhaust gas emissions, is green and environmentally friendly, and is the most practical aluminum coating.

[0041] Continue to see Figure 6In the ionic liquid aluminum plating system, there are aluminum chloride-imidazole, aluminum chloride-pyridine, aluminum chloride-quaternary ammonium, and aluminum chloride-pyrrole. Among them, aluminum chloride-1-ethyl-3-methylimidazole chloride (AlCl3-EMIC) has a very low melting point and high electrical conductivity, and is the ionic liquid aluminum plating solution with the most promising engineering application prospects.

[0042] Continue to see Figure 6 In the AlCl3-EMIC ionic liquid, only the composition with a molar ratio of AlCl3 to EMIC greater than 1 can electroplate aluminum, among which the plating solution with a molar ratio of 1.5 to 2.0 is optimal.

[0043] Continue to see Figure 6 When aluminum is plated, the desired aluminum coating can be obtained through process parameters such as current density, temperature, and time. The general current density range is 5-80mA / cm2, the temperature is 25-80℃, the plating speed is 1-10μm / min, and the time can be adjusted according to the required thickness of aluminum plating. A variety of additives can be added to the plating solution to obtain a more uniform and dense aluminum coating, and the bonding strength between the aluminum coating and the chip can be improved through heat treatment.

[0044] Continue to see Figure 6 The aluminum pad is manufactured by electroplating aluminum, which does not require glue coating, etching, glue removal, wet cleaning and other process steps. Therefore, it can greatly reduce the consumption of high-purity aluminum target, photoresist, glue removal liquid, cleaning liquid and other materials, reduce the investment in PVD, glue coating, cleaning and other equipment, or reduce the occupancy time of these equipment. This can achieve a significant reduction in costs.

[0045] Continue to see Figure 6 Considering that the thickness of the aluminum pad is generally 2 to 8 μm, the aluminum plating time of the manufacturing method of the present application is 2 to 50 minutes. Together with the cleaning process, the entire cycle is within 2 hours. When the aluminum pad is manufactured by the PVD method, the aluminum plating time takes about 5 hours. Together with the glue coating, etching, glue removal, cleaning and other processes, the entire process takes more than 24 hours. Therefore, the aluminum electroplating method of the present application can significantly shorten the process time and improve production efficiency. Moreover, it is easy to obtain a thick aluminum coating through the electroplating method, thereby meeting the demand for aluminum pads put forward by the development of high-power devices. Since no etching process is required, the problem of difficulty in etching thick aluminum can be solved, and there is no hidden danger of aluminum corrosion quality, and the quality stability is high.

[0046] Example 1

[0047] A 4-inch wafer made of semiconductor chips, cleaned and dried, was used as the cathode, aluminum wire was used as the anode, AlCl3-EMIC ionic liquid with a molar ratio of 2.0 was used as the plating solution, and a glass beaker was used as the plating tank. The entire device was placed in an argon protective atmosphere glove box. The cathode and anode were connected to the negative and positive electrodes of a DC power supply, respectively.

[0048] The current was set according to the total area of ​​the chip so that the current density was 10 mA / cm2. After 40 minutes of power-on, the wafer was taken out, cleaned with alcohol ultrasonic wave, washed and dried with water, and then heat treated at 500°C for 30 minutes.

[0049] See also Figure 8-Figure 11 , Figure 8 This is the appearance of the wafer after aluminum plating. Fig. 9 This is a stereoscopic photo of the wafer surface. The small white squares are aluminum-plated chips with a size of 0.6*0.6mm. The small squares are insulating areas. After cutting along the insulating areas, independent semiconductor chips can be obtained, and the white areas are aluminum pads. Fig.10 This is a scanning electron microscope (SEM) photo of the aluminum pad surface, showing that the aluminum particles are small and uniform. Fig.11 This is a cross-sectional view of an aluminum pad. It can be seen that the aluminum coating obtained by the method of the present application is dense and tightly bonded to the chip.

[0050] Example 2

[0051] A 4-inch wafer made of semiconductor chip and plated with gold is used as cathode, aluminum wire is used as anode, AlCl3-EMIC ionic liquid with a molar ratio of 1.5 is used as plating solution, the temperature is 80°C, and a glass beaker is used as a plating tank. The whole device is placed in an argon protective atmosphere glove box, and the cathode and anode are connected to the negative and positive electrodes of a DC power supply respectively.

[0052] The current was set according to the total area of ​​the chip so that the current density was 80 mA / cm2. After energizing for 4 minutes, the wafer was taken out, ultrasonically cleaned with toluene, and then washed and dried with water.

[0053] See also Fig.12 and Fig.13 , Fig.12 This is the appearance of the wafer after aluminum plating. Fig.13 This is a cross-sectional view of an aluminum pad. The average thickness of the aluminum coating is 6um. The white color is the gold coating. It can be seen that the aluminum coating and the gold coating are tightly bonded.

[0054] In the description of the present application, the description with reference to the terms "one embodiment", "some embodiments", "in the present embodiment", "specific example", or "some examples" etc. means that the specific features, mechanisms, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, mechanisms, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0055] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A method for manufacturing an aluminum pad on a power semiconductor device, characterized in that: The following steps are involved: Step S1, using a semiconductor chip wafer that has been cleaned and dried as a cathode, an aluminum wire as an anode, an ionic liquid as a plating solution, and a glass beaker as a plating tank, all of which are placed in a box filled with a protective gas; Step S2, electrically connecting the anode to the positive electrode of a DC power supply, and electrically connecting the cathode to the negative electrode of the DC power supply; Step S3, power is turned on for electroplating, and then the wafer is taken out and subjected to solvent ultrasonic cleaning and water washing and drying treatment to obtain a power semiconductor device electroplated with an aluminum pad.

2. The manufacturing method according to claim 1, characterized in that: In the step S1, the ionic liquid used is aluminum chloride-imidazole, aluminum chloride-pyridine, aluminum chloride-quaternary ammonium, or aluminum chloride-pyrrole.

3. The manufacturing method according to claim 2, characterized in that: In the step S1, the ionic liquid is AlCl3-EMIC ionic liquid with a molar ratio of 1.5 to 2.

0.

4. The manufacturing method according to claim 3, characterized in that: In the step S3, the molar ratio of the AlCl3-EMIC ionic liquid used is 2.

0.

5. The manufacturing method according to claim 1, characterized in that: In step S3, the current density range is 5-80 mA / cm 2 The electroplating is carried out under the conditions of a temperature range of 25 to 80°C and a plating speed range of 1 to 10 μm / min.

6. The manufacturing method according to claim 1, characterized in that: In the step S3, the wafer is ultrasonically cleaned using a solvent, and the solvent is alcohol or toluene.

7. The manufacturing method according to claim 1, characterized in that: In the step S3, after the wafer is taken out and subjected to solvent ultrasonic cleaning and water washing and drying treatment, the following steps are further included: The wafer after the solvent ultrasonic cleaning and water washing and drying treatment is subjected to a heat treatment at 500° C. for 30 minutes.