Preparation method of ultra-high molecular weight polyethylene nanofiber

Through island spinning and crystal structure control methods, combined with extrusion and extraction technology, the problem of low efficiency and high cost in the preparation of ultra-high molecular weight polyethylene nanofibers in the existing technology has been solved, and the preparation of nanofibers with a diameter of less than 300nm has been achieved, improving the Fiber strength and application range.

CN118792746AActive Publication Date: 2024-10-18WUHAN TEXTILE UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410957132.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-18
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

It is difficult to prepare ultra-high molecular weight polyethylene nanofibers with existing technology, especially nanofibers with a size below 300 nm, and the preparation efficiency is low and the cost is high.

Method used

Using a method that combines island spinning and crystal structure control, the batch preparation of ultra-high molecular weight polyethylene nanofibers is achieved through multiple control functions such as extrusion, stretching, and grain refinement of the two components. The specific steps include pre-processing. Swelling, melt blending, extrusion and acetone extraction, utilizing nucleating agents such as titanium oxalate and cellulose acetate butyrate to promote crystal refinement.

Benefits of technology

The macro-scale preparation of ultra-high molecular weight polyethylene nanofibers was successfully achieved, with the fiber diameter less than 300nm, which improved the draftability and strength of the fiber and expanded its application scope.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792746A_ABST
    Figure CN118792746A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of ultra-high molecular weight polyethylene nanofiber. The method comprises the following steps: firstly, carrying out liquid paraffin pre-swelling on UHMWPE powder (the ratio of UHMWPE to liquid paraffin is 2: 8), then carrying out melt blending on the swelled UHMWPE gel, a nucleating agent and CAB by using a twin-screw extruder, drafting and refining the UHMWPE by virtue of UHMWPE online crystal regulation and control in an extrusion process and stretching and extruding effects of CAB blending on the UHMWPE, then extracting a CAB phase and liquid paraffin by adopting acetone, and finally, carrying out melt blending on the CAB and the UHMWPE by using a twin-screw extruder. The UHMWPE nanofibers are obtained, and macro-quantity preparation of the UHMWPE nanofibers with the diameter being 300 nm or below is achieved. According to the method, macro preparation of the UHMWPE nanofibers is achieved through a method combining sea-island spinning and crystal structure regulation and control, flexible regulation and control of the UHMWPE nanofibers are achieved by changing the component ratio and experimental parameters, controllable preparation of the UHMWPE nanofibers of various sizes is met, and the problems that the UHMWPE nanofibers are difficult to prepare and the product is single are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ultra-high molecular weight nanofibers, and in particular to a method for preparing ultra-high molecular weight polyethylene nanofibers. Background Art

[0002] Ultra-high molecular weight polyethylene (UHMWPE) has the problems of poor melt fluidity and difficult molding and processing. The preparation of UHMWPE nanofibers has always been an industry problem that is difficult to solve, especially nanofibers with a size below 300nm. The best preparation method at present is to use electrospinning, but most of them are above 500nm. At the same time, this method has low preparation efficiency and high cost.

[0003] In the prior art, the patent with publication number CN102041557B discloses a method for producing high-strength and high-modulus polyethylene fibers, which comprises swelling and dissolving, filtering, spinning, freezing and solidifying, pre-stretching, extraction, drying, super-stretching, and winding, wherein the swelling and dissolving step is carried out in a kneader, and the transparent uniform spinning solution obtained by the swelling and dissolving step is quantitatively fed into a single-screw extruder while stirring for extrusion to obtain high-strength and high-modulus polyethylene fibers. However, the polyethylene fibers prepared by this method are still at the micron level, which greatly limits its application range, and the preparation of ultra-high molecular weight polyethylene nanofibers is still a bottleneck problem.

[0004] In view of this, it is necessary to design an improved method for preparing ultra-high molecular weight polyethylene nanofibers to solve the above problems. Summary of the invention

[0005] In view of the defects of the above-mentioned prior art, the purpose of the present invention is to provide a method for preparing ultra-high molecular weight polyethylene nanofibers. The preparation method adopts a method combining island spinning and crystal structure regulation to achieve batch preparation of UHMWPE nanofibers, and further refines UHMWPE fibers by combining multiple regulation effects such as extrusion, stretching and grain refinement of the two components, so as to achieve large-scale preparation of fibers with a diameter of less than 300nm.

[0006] To achieve the above object, the present invention provides a method for preparing ultra-high molecular weight polyethylene nanofibers, comprising the following steps:

[0007] S1, pre-swelling an ultra-high molecular weight polyethylene powder having a relative average molecular weight of 4.5 million and liquid paraffin in a mass ratio of ultra-high molecular weight polyethylene powder: liquid paraffin = 2:8 to obtain an ultra-high molecular weight polyethylene gel;

[0008] S2, feeding ultra-high molecular weight polyethylene gel, a nucleating agent, and cellulose acetate butyrate into a twin-screw extruder for melt blending and extrusion to obtain a modified gel ultra-high molecular weight polyethylene fiber; the nucleating agent is dibenzylidene sorbitol, di(p-methylbenzylidene) sorbitol, or titanium oxalate;

[0009] S3, soaking the modified gel ultra-high molecular weight polyethylene fiber obtained in step S2 in an acetone solution, extracting the CAB phase and liquid paraffin with acetone to obtain UHMWPE nanofibers with a diameter of less than 300 nm.

[0010] Furthermore, in step S2, the mass ratio of the ultra-high molecular weight polyethylene, the nucleating agent, and the cellulose acetate butyrate is 20:(0.5-2):(78-79.5). Preferably, the mass ratio of the ultra-high molecular weight polyethylene, the nucleating agent, and the cellulose acetate butyrate is 20:1:79.

[0011] The mass concentration of the nucleating agent is 0.5-2.0 wt %. Preferably, the mass concentration of the nucleating agent is 1.0 wt %.

[0012] Further, in step S2, the temperature of melt blending is 200-240°C.

[0013] The beneficial effects of the present invention are:

[0014] 1. The preparation method of ultra-high molecular weight polyethylene nanofibers provided by the present invention comprises the following steps: firstly, UHMWPE powder is pre-swollen with liquid paraffin (UHMWPE: liquid paraffin=2:8), and then the swollen UHMWPE gel, nucleating agent and CAB are melt-blended by a twin-screw extruder, and the drawing and refinement of UHMWPE in the melt-blending process are achieved by online crystal regulation of UHMWPE during the extrusion process and the stretching and extrusion effect of CAB blending on UHMWPE, and then acetone is used to extract the CAB phase and liquid paraffin to obtain UHMWPE nanofibers, thereby realizing the large-scale preparation of UHMWPE nanofibers with a diameter of less than 300 nm.

[0015] 2. The present invention uses a nucleating agent such as dibenzylidene sorbitol, di(p-methylbenzylidene) sorbitol or titanium oxalate, and uses the nucleating agent to cause local stress instability, induces the generation of a large number of new crystal nuclei, achieves the purpose of refining the grain size, increasing the number of crystals, and promoting UHMWPE to be easier to draw and the fiber size to be easier to refine. The nucleating agent is preferably titanium oxalate, because when UHMWPE is melted and crystallized, the titanium oxalate surface forms a hydrogen bond with the methylene of UHMWPE as an electron donor, and the molecular chain of the UHMWPE wafer grows more easily on the titanium oxalate surface to form a transcrystalline region between the interfaces, which is more effective in refining the grain size and increasing the number of crystals. Grain refinement enhances the interaction between the molecular chains, making UHMWPE less likely to break after being drawn at a large ratio, and the fiber size is smaller. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic diagram of the process of preparing the ultra-high molecular weight polyethylene nanofibers of the present invention.

[0017] Figure 2 This is an electron microscope image of the ultra-high molecular weight polyethylene nanofibers prepared in Example 1.

[0018] Figure 3 This is a XRD comparison diagram of the ultra-high molecular weight polyethylene fiber prepared in Example 1 and Comparative Example 1.

[0019] Figure 4 This is an optical microscope comparison of the ultra-high molecular weight polyethylene fibers prepared in Example 1 and Comparative Example 1 after being hot pressed into sheets.

[0020] Figure 5 This is an electron microscope image of the ultra-high molecular weight polyethylene nanofibers prepared in Example 2.

[0021] Figure 6 This is an electron microscope image of the ultra-high molecular weight polyethylene nanofibers prepared in Example 3.

[0022] Figure 7 This is an electron microscope image of the ultra-high molecular weight polyethylene nanofiber prepared in Comparative Example 2. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0024] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0025] See also Figure 1 As shown, the present invention provides a method for preparing ultra-high molecular weight polyethylene nanofibers, comprising the following steps:

[0026] S1, pre-swelling an ultra-high molecular weight polyethylene powder having a relative average molecular weight of 4.5 million and liquid paraffin in a mass ratio of ultra-high molecular weight polyethylene powder: liquid paraffin = 2:8 to obtain an ultra-high molecular weight polyethylene gel;

[0027] S2, feeding ultra-high molecular weight polyethylene gel, nucleating agent and cellulose acetate butyrate into a twin-screw extruder for melt blending and extrusion to obtain modified gel ultra-high molecular weight polyethylene fiber; the nucleating agent is dibenzylidene sorbitol, di(p-methylbenzylidene) sorbitol or titanium oxalate; the melt blending temperature is 220°C, the screw pressure is 2.0-2.2MPa, and the spinneret hole size is 200μm.

[0028] S3, soaking the modified gel ultra-high molecular weight polyethylene fiber obtained in step S2 in an acetone solution, extracting the CAB phase and liquid paraffin with acetone to obtain UHMWPE nanofibers with a diameter of less than 300 nm.

[0029] Wherein, in step S2, the mass ratio of the ultra-high molecular weight polyethylene, the nucleating agent, and the cellulose acetate butyrate is 20:(0.5-2):(78-79.5), preferably 20:1:79.

[0030] The mass concentration of the nucleating agent is 0.5-2.0 wt %, preferably 1.0 wt %.

[0031] The preparation method of the ultra-high molecular weight polyethylene nanofiber provided by the present invention is described below with reference to specific examples.

[0032] Example 1

[0033] This embodiment provides a method for preparing ultra-high molecular weight polyethylene nanofibers, comprising the following steps:

[0034] S1, pre-swelling an ultra-high molecular weight polyethylene powder having a relative average molecular weight of 4.5 million and liquid paraffin in a mass ratio of ultra-high molecular weight polyethylene powder: liquid paraffin = 2:8 to obtain an ultra-high molecular weight polyethylene gel;

[0035] S2, feeding UHMWPE gel containing 20g solid content, 1g titanium oxalate, and 79g cellulose acetate butyrate into a twin-screw extruder for melt blending and extrusion to obtain modified gel ultra-high molecular weight polyethylene fiber; the melt blending temperature is 220°C, the screw pressure is 2.0-2.2MPa, and the spinneret hole size is 200μm.

[0036] S3, soaking the modified gel ultra-high molecular weight polyethylene fiber obtained in step S2 in an acetone solution, extracting the CAB phase and liquid paraffin with acetone to obtain UHMWPE nanofibers with a diameter of 100-300 nm.

[0037] See also Figure 2 As shown, it is an electron microscope image of the UHMWPE nanofibers prepared in Example 1. It can be seen from the figure that the average fiber diameter is 266nm, and the large-scale preparation of UHMWPE nanofibers below 300nm is achieved.

[0038] Comparative Example 1

[0039] Comparative Example 1 provides a method for preparing nanofibers. Compared with Example 1, the difference is that no nucleating agent titanium oxalate is added in step S2, and the rest is substantially the same as Example 1, which will not be described herein.

[0040] Figure 3 The XRD comparison diagram of the ultra-high molecular weight polyethylene fiber prepared in Example 1 and Comparative Example 1 shows that the peak intensity of the α-crystal diffraction peak at the position of 17.3° in the diffraction spectrum obtained in Example 1 is significantly increased, indicating that the addition of the nucleating agent titanium oxalate greatly promotes the formation of the α-crystal. According to the Scherrer formula, the grain size becomes smaller and the number increases. That is, the titanium oxalate added in Example 1 makes the UHMWPE wafer more susceptible to the action of interfacial hydrogen bonds, forming a transcrystalline region, greatly refining the grain size, greatly increasing the number of grains, and forming more α-crystals. In Comparative Example 1, the crystal structure shows the XRD spectrum of conventional UHMWPE, and the enhanced α-crystal diffraction peak cannot be obtained, resulting in insufficient drawing ratio in the final UHMWPE melting process and the fiber size cannot reach below 300nm.

[0041] Figure 4 This is an optical microscope comparison of the ultra-high molecular weight polyethylene fiber prepared in Example 1 and Comparative Example 1 after hot pressing into a sheet. It can be seen that compared with the picture without adding a nucleating agent, the number of grains in the microscope picture containing a nucleating agent is greatly increased, and the crystal size is greatly reduced, while the picture without adding a nucleating agent shows a larger grain size and a smaller number of crystals. This once again shows that titanium oxalate can refine the grain size, increase the number of crystals, promote the ultra-high molecular weight polyethylene to be easier to draw, and the fiber size is easier to refine.

[0042] Examples 2-3 and Comparative Example 2

[0043] Examples 2-3 and Comparative Example 2 provide a method for preparing ultra-high molecular weight polyethylene nanofibers, which differ from Example 1 in that the nucleating agent used in step S2 is changed, as shown in Table 1 below, and the remaining steps are substantially the same as those in Example 1. No further description is given here.

[0044] Table 1

[0045]

[0046]

[0047] See also Figure 5 As shown in FIG. 1 , it is an electron microscope image of the UHMWPE nanofiber prepared in Example 2. It can be seen from the figure that the size of the prepared UHMWPE nanofiber is 200-300 nm, which is mainly attributed to the hydrogen bonds formed between dibenzylidene sorbitol and the surface of UHMWPE, which enhances the shuffle area formed by UHMWPE on the surface of dibenzylidene sorbitol, effectively increases the drawing ratio of the UHMWPE phase during the melt drawing process, and the fiber size reaches below 300 nm.

[0048] See also Figure 6 As shown in FIG. 1 , it is an electron microscope image of the UHMWPE nanofiber prepared in Example 3. It can be seen from the figure that the size of the prepared UHMWPE fiber is 180-280 nm. This is mainly attributed to the hydrogen bond formed between di(p-methylbenzylidene)sorbitol and the surface of UHMWPE, which enhances the transcrystalline region formed by UHMWPE on the surface of di(p-methylbenzylidene)sorbitol, effectively increases the drawing ratio of the UHMWPE phase during the melt drawing process, and the fiber size reaches below 300 nm.

[0049] See also Figure 7 As shown, it is an electron microscope image of the UHMWPE nanofiber prepared in Comparative Example 2. It can be seen from the figure that the UHWMPE fiber prepared with talc as the nucleating agent is relatively large in size, all greater than 300nm.

[0050] The UHMWPE nanofibers prepared in Examples 1-3 and Comparative Examples 1-2 were tested, and the results are shown in Table 2.

[0051] Table 2

[0052]

[0053] Comparing Examples 1-3 with Comparative Example 1, it can be seen that when no nucleating agent is added, the fiber diameter obtained is larger due to the larger size and smaller number of UHMWPE crystals. Compared with the comparative example, the UHMWPE fibers prepared in the examples have smaller diameters, all less than 300 nm, and better fiber strength.

[0054] Comparing Examples 1-3 with Comparative Example 2, it can be seen that when the added nucleating agent is talcum powder, although the size of the obtained UHMWPE fiber is reduced (1000-1500nm), due to the limited regulation of talcum powder on the crystal structure of UHMWPE, the formation effect of UHMWPE nanofibers is not good.

[0055] Examples 4-8 and Comparative Examples 3-4

[0056] The main difference between Examples 4-8 and Comparative Examples 3-4 and Example 1 is that the type of nucleating agent in step S2 and the ratio of the solid content of ultra-high molecular weight polyethylene gel, the nucleating agent, and the cellulose acetate butyrate are changed, as shown in Table 3 below. The rest is roughly the same as Example 1 and will not be repeated here.

[0057] Table 3

[0058]

[0059] The UHMWPE nanofibers prepared in Examples 4-8 and Comparative Examples 3-4 were tested, and the results are shown in Table 4.

[0060] Table 4

[0061]

[0062]

[0063] According to the above table, for different nucleating agents, the optimal addition amount is 1wt%, and both the fiber strength and modulus are optimal. When the amount of nucleating agent added is too little, the nucleating agent is limited in regulating the crystal structure of UHMWPE, which is mainly manifested in a significant reduction in nucleation sites, a limited number of new crystal nuclei, and a large crystal size with a small number. In Comparative Example 3, since the addition amount of nucleating agent titanium oxalate is only 0.2wt%, the fiber diameter reaches 600-1600nm.

[0064] When the amount of nucleating agent added is too much, the nucleating agent is easy to agglomerate and bond, which greatly reduces the control effect on the UHMWPE crystal, including the limited decrease in grain size and the small increase in the number of grains. In Comparative Example 4, since the amount of nucleating agent titanium oxalate added is 3.0wt%, the fiber diameter reaches 500-1500nm.

[0065] In summary, the present invention provides a method for preparing ultra-high molecular weight polyethylene nanofibers. First, UHMWPE powder is pre-swollen with liquid paraffin (UHMWPE: liquid paraffin = 2:8), and then the swollen UHMWPE gel, nucleating agent and CAB are melt-blended by a twin-screw extruder. The UHMWPE is stretched and refined by online crystal regulation of UHMWPE during the extrusion process and the stretching and extrusion of UHMWPE by CAB blending. Then, acetone is used to extract the CAB phase and liquid paraffin to obtain UHMWPE nanofibers, thereby realizing the large-scale preparation of UHMWPE nanofibers with a diameter of less than 300 nm.

[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing ultra-high molecular weight polyethylene nanofibers, characterized in that: The following steps are involved: S1, pre-swelling an ultra-high molecular weight polyethylene powder having a relative average molecular weight of 4.5 million and liquid paraffin in a mass ratio of ultra-high molecular weight polyethylene powder: liquid paraffin = 2:8 to obtain an ultra-high molecular weight polyethylene gel; S2, feeding ultra-high molecular weight polyethylene gel, a nucleating agent, and cellulose acetate butyrate into a twin-screw extruder for melt blending and extrusion to obtain a modified gel ultra-high molecular weight polyethylene fiber; the nucleating agent is dibenzylidene sorbitol, di(p-methylbenzylidene) sorbitol, or titanium oxalate; S3, soaking the modified gel ultra-high molecular weight polyethylene fiber obtained in step S2 in an acetone solution, extracting the CAB phase and liquid paraffin with acetone to obtain UHMWPE nanofibers with a diameter of less than 300 nm.

2. The method for preparing ultra-high molecular weight polyethylene nanofibers according to claim 1, characterized in that: In step S2, the mass ratio of the ultra-high molecular weight polyethylene, the nucleating agent, and the cellulose acetate butyrate is 20:(0.5-2):(78-79.5).

3. The method for preparing ultra-high molecular weight polyethylene nanofibers according to claim 1, characterized in that: The nucleating agent is dibenzylidene sorbitol, and the mass concentration of the dibenzylidene sorbitol is 0.5-2.0wt%.

4. The method for preparing ultra-high molecular weight polyethylene nanofibers according to claim 3, characterized in that: The mass ratio of the ultra-high molecular weight polyethylene, dibenzylidene sorbitol and cellulose acetate butyrate is 20:(0.5-2):(78-79.5).

5. The method for preparing ultra-high molecular weight polyethylene nanofibers according to claim 1, characterized in that: The nucleating agent is di(p-methylbenzylidene)sorbitol, and the mass concentration of the di(p-methylbenzylidene)sorbitol is 0.5-2.0wt%.

6. The method for preparing ultra-high molecular weight polyethylene nanofibers according to claim 5, characterized in that: The mass ratio of the ultra-high molecular weight polyethylene, di(p-methylbenzylidene) sorbitol and cellulose acetate butyrate is 20:(0.5-2):(78-79).

7. The method for preparing ultra-high molecular weight polyethylene nanofibers according to claim 1, characterized in that: The nucleating agent is titanium oxalate, and the mass concentration of the titanium oxalate is 0.5-2.0wt%.

8. The method for preparing ultra-high molecular weight polyethylene nanofibers according to claim 7, characterized in that: The mass ratio of the ultra-high molecular weight polyethylene, titanium oxalate and cellulose acetate butyrate is 20:(0.5-2):(78-79.5).

9. The method for preparing ultra-high molecular weight polyethylene nanofiber according to claim 1, characterized in that: In step S2, the temperature of melt blending is 200-240°C.

Citation Information

Patent Citations

  • Preparation method of thermal plasticity high polymer micro / nano fibrous membrane material

    CN101337158A

  • Carbon nano tube / polyolefin micro-nano fiber and preparation method thereof

    CN101864610A

  • Nano-fiber yarn and preparation method thereof

    CN108842242A

  • Nanofiber with surface containing nano convex structure and preparation method thereof

    CN110409010A

  • Thermoplastic polymer microfibers, nanofibers and composites

    US20100233458A1