Conductive fiber coated with liquid metal as well as preparation method and application of conductive fiber
The method of wrapping the insulating layer through dilute hydrochloric acid treatment and conjugated electrospinning technology solves the problem of insufficient flexibility and stretchability of traditional wires, and prepares low-cost, highly conductive and flexible fibers suitable for smart clothing.
Patent Information
- Application Number
- CN202410878804.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional metal wires lack flexibility and stretchability. Improved flexibility and stretchability of existing conductive fibers lead to high production costs, complicated processes, and uncomfortable wearing.
Conductive fibers are treated with dilute hydrochloric acid and coated with low-temperature liquid metal, combined with conjugate electrospinning technology to wrap the insulating layer to form fibers with high conductivity.
The preparation of high conductivity fibers is achieved with low cost and simplified process. The fibers have similar properties to fabrics and prevent oxidation and leakage of liquid metal, making them suitable for smart wearable clothing.
Smart Images

Figure CN118792777A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of textile fiber preparation, and in particular to a conductive fiber coated with liquid metal, and a preparation method and application thereof. Background Art
[0002] With the continuous development and progress of electronic technology and textile technology, research such as "smart clothing" has become a hot topic. Among them, how to make conductive fibers comfortable and wearable is one of the difficult problems. Traditional metal wires not only lack flexibility and stretchability, but also have unsatisfactory wearing experience. This makes it particularly important to develop a fiber that has excellent conductivity, flexibility and stretchability. In recent years, liquid metals with metallic conductivity and excellent deformation ability have solved the above problems well, solving a major problem for researchers in this research direction. Most of the journal papers we often see now are to inject liquid metal into silicone tubes and then seal them to make fibers. However, although silicone tubes have good flexibility and stretchability as fibers, there are still certain inconveniences in actual operation and product effects. Based on the above research, how to make this type of new conductive fiber have the common characteristics of common textile fibers on the basis of good flexibility and stretchability is the current research hotspot and difficulty.
[0003] The research on making liquid metal conductive fibers have textile fiber properties under the condition of good conductive properties mainly includes the following aspects: ① manufacturing highly tensile conductive fibers through one-step spiral hot stretching technology to improve their tensile properties (journal of Materials Science & Technology 195 (2024) 136-145); ② manufacturing intrinsically stretchable and porous elastic fibers and patterning conductive liquid metal circuits on them (Adv. Funct. Mater. 2023, 2308150); ③ by drawing LM-injected hollow thermoplastic polyester elastomer preforms at room temperature, long, thin, wire-like liquid metal fibers can be manufactured (Chemical Engineering Journal 480 (2024) 147944). However, these methods of improving fiber properties often increase input costs, make the processing technology more complicated, and are difficult to mass-produce on a large scale. Summary of the invention
[0004] In view of this, the purpose of the present invention is to propose a conductive fiber coated with liquid metal and a preparation method and application thereof, so as to overcome the lack of flexibility and stretchability of traditional metal wires, and the defects of the prior art that although the conductive fiber has flexibility and stretchability, it causes discomfort to wear, high production cost, and complex process.
[0005] Based on the above purpose, the present invention provides a conductive fiber coated with liquid metal, comprising an acid-treated conductive fiber, a liquid metal coating layer and an outer wrapping layer arranged in sequence from the inside to the outside, wherein the acid-treated conductive fiber is obtained by treating the conductive fiber in a dilute hydrochloric acid bath with a concentration of 8-10%.
[0006] Preferably, the surface of the fiber treated as above is wrapped with several insulating layers as outer wrapping layers by conjugated electrospinning technology, that is, conjugated electrospinning is performed back and forth for multiple times.
[0007] The conductive fiber is passed through the hydrochloric acid bath by a collecting roller, and the speed of the collecting roller is 15-100r / min. The short-term treatment with dilute hydrochloric acid is to allow the liquid metal to fully adhere to the surface of the nanosilver fiber, thereby increasing the adhesion capacity. Short-term treatment: The roller collecting device is used to pull the fiber to move so that the conductive fiber passes through the dilute hydrochloric acid bath and the liquid metal bath in turn.
[0008] The liquid metal is a low-temperature or room-temperature liquid alloy having a melting point of -15-40° C., including gallium-indium liquid alloy, indium-tin liquid alloy, gallium-indium-tin liquid alloy, and the like.
[0009] The outer wrapping layer is selected from one or more of PVDF, nylon 6, polylactic acid, and polyacrylonitrile.
[0010] The conductive fiber is selected from one or more of stainless steel metal fiber, conductive carbon fiber, silver-plated nylon fiber and polypropylamine conductive fiber.
[0011] The present invention also provides a method for preparing the conductive fiber coated with liquid metal, comprising the following steps:
[0012] Step 1: The conductive fiber is treated in a dilute hydrochloric acid bath with a concentration of 8-10%;
[0013] Step 2, coating the conductive fibers treated in step 1 with liquid metal;
[0014] Step 3: Electrospinning the conductive fibers treated in step 2 to prepare an outer wrapping layer.
[0015] Step 3: The electrospinning is performed by conjugated electrospinning, and the spinning parameters are: the spinning solution concentration is 16-18wt%, the spinning solvent is acetone and N, N-dimethylformamide mixed in a weight ratio of 2:3, the spinning positive voltage is 12.5kV, the spinning negative voltage is 7.5kV, the propulsion speed is 3ml / h, the drum collection speed is 15-100r / min, and the bell mouth is 800r / min. After the material and the solution are mixed, they are placed in a constant temperature oven for heating to completely fuse the material and the solution.
[0016] The outer wrapping layer prepared by electrospinning is obtained by performing conjugate electrospinning back and forth 3-5 times. The purpose of conjugate spinning technology is to wrap the surface of the fiber that has been coated with liquid metal on the surface with a protective layer that is isolated from the outside world, that is, an insulating outer wrapping layer. It can prevent the liquid metal from being oxidized. Performing conjugate spinning back and forth 3-5 times can better wrap the liquid metal to prevent leakage. It can be concluded from multiple experimental results that conjugate spinning once is not enough to completely cover the liquid metal.
[0017] The present invention also provides application of the conductive fiber coated with liquid metal in flexible materials, clothing or functional devices.
[0018] The functional device is a wearable wireless communication device, and its preparation method comprises the following steps:
[0019] Step 1: preparing the conductive fiber coated with liquid metal as a basic material for constructing a body area network;
[0020] Step 2: Design a reasonable wireless communication response pattern on the computer, such as circle, square, star, ellipse, etc., to be suitable for the construction of the body area network;
[0021] Step 3: Using digital integration technology to respond to the pattern, the designed pattern is imported into a digital sewing machine and the prepared conductive fiber coated with liquid metal is used as a bobbin for digital sewing;
[0022] Step 4: Patterns are sewn on at least two areas of the fabric, the distance between each pattern is adjusted according to the planned body area network, and the patterns are connected and adapted with the conductive fiber coated with liquid metal, so as to achieve the effect of transmitting information data.
[0023] Beneficial effects of the present invention: The conductive fiber treated with hydrochloric acid can better allow liquid metal to adhere to it, so as to achieve the effect of making a high-conductivity fiber, and the insulating layer is wrapped on the outer layer of the high-conductivity fiber through the electrostatic spinning technology to achieve the technology of preventing the oxidation and leakage of liquid metal, which simplifies the preparation process of high-conductivity fiber made of liquid metal in the prior art. Only by using common materials on the market and relatively low costs, high-conductivity fibers can be achieved, and the fibers have similar properties to textile fibers. The present invention is simple to prepare and has obvious actual gain effects, and can provide a feasible solution for the field of conductive fibers in smart wearable clothing. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 The figure is a production flow chart of the high conductivity fiber of the present invention and a schematic diagram of the finished fiber structure;
[0026] Figure 2 Comparison of images of the three stages of the present invention; (a) real photo (the order is conductive fiber, fiber coated with liquid metal, fiber wrapped), (b) SEM image;
[0027] Figure 3 The different resistances of the product fibers obtained by different methods during the research process of the present invention;
[0028] Figure 4 The resistance value change of the product fiber obtained at different speeds of the collecting drum of the present invention;
[0029] Figure 5 The resistance value changes at different bending angles after the present invention is bent 500 times;
[0030] Figure 6 This is a practical example of combining the present invention with clothing fabric and transmitting information using the principle of wireless communication. DETAILED DESCRIPTION
[0031] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0032] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should have the common meanings understood by persons having ordinary skills in the field to which the present invention belongs.
[0033] Raw materials and sources in the examples: polyvinylidene fluoride (Arkema PVDF Kynar MG15, France), nylon 6 (DuPont 73G45, USA), polylactic acid (molecular weight Mw = 20.0×10 4 American NatureWorks), polyacrylonitrile (molecular weight Mw = 25.0 × 10 4 , Sipin Technology), NN dimethylformamide (ACS spectral grade, ≥99.8%, Aladdin reagent), acetone (molecular weight Mw=58.08, Zhanyun reagent), hydrochloric acid (Mw=36.46, Zhanyun reagent), scientific research wire (d=0.2mm, purity 99.99%), carbon fiber (6K), nano silver wire (specification 200D / 48f FDY, twist 350T / M), liquid metal (gallium indium liquid alloy). Teflon tube, syringe, needle, and roller are all commercially available materials. The resistance performance of high conductivity fiber was tested using multimeter 9205A.
[0034] Example 1
[0035] (1) Assembly of dilute hydrochloric acid bath and liquid metal bath (structure as Figure 1 ): Take an open square box with a size of 1cm*cm*1cm to hold 8% dilute hydrochloric acid and liquid metal with a distance of 1cm in between, and let the conductive fiber pass through it to coat the liquid metal on its surface.
[0036] (2) The spinning parameters for preparing the surface insulating layer of the high-conductivity fiber by electrospinning are as follows: the spinning solution concentration is 16wt%, the spinning solute is PVDF, the spinning solvent is acetone and N,N-dimethylmethylamine, the spinning positive voltage is 12.50kV, the spinning negative voltage is -7.50kV, the propulsion speed is 3ml / h, the drum collection speed is 15r / min (i.e. 2.83cm / s), and the bell mouth is 800r / min. Using the same parameter conditions, the spinning solution is used to wrap it 3, 4, and 5 times.
[0037] The high conductivity fiber obtained in this embodiment has a measured length of 1 cm, and the resistance values measured at multiple groups of different positions are respectively taken, such as Figure 3 shown.
[0038] Example 2
[0039] (1) Assembly of dilute hydrochloric acid bath and liquid metal bath (structure as Figure 1 ): Take an open square box with a size of 1cm*cm*1cm and place it in a container with a distance of 1cm between 10% dilute hydrochloric acid and liquid metal.
[0040] (2) The spinning parameters for preparing the surface insulating layer of high-conductivity fiber by electrospinning are as follows: the spinning solution concentration is 18wt%, the spinning solute is PVDF, the spinning solvent is acetone and N,N-dimethylmethylamine, the spinning positive voltage is 12.50kV, the spinning negative voltage is -7.50kV, the propulsion speed is 3ml / h, the drum collection speed is 15r / min (i.e. 2.83cm / s), and the bell mouth is 800r / min. Using the same parameter conditions, the spinning solution is used to wrap it 3, 4, and 5 times.
[0041] (3) Bend the fiber at 30°, 60°, 90°, 120°, 150°, and 180° to measure the resistance change. Figure 5 shown.
[0042] Example 3
[0043] The difference between this embodiment and embodiment 1 is that the drum collection speed in step (2) is 23 r / min (ie 4.24 cm / s).
[0044] Example 4
[0045] The difference between this embodiment and embodiment 1 is that the drum collection speed in step (2) is 30 r / min (ie, 5.65 cm / s).
[0046] Example 5
[0047] The difference between this embodiment and embodiment 2 is that the spinning solute is replaced with nylon 6.
[0048] Example 6
[0049] The difference between this embodiment and embodiment 2 is that the spinning solute is replaced with polylactic acid.
[0050] Example 7
[0051] The difference between this embodiment and embodiment 2 is that the spinning solute is replaced by polyacrylonitrile.
[0052] Comparative Example 1
[0053] (1) Take an open square box with a size of 1 cm*cm*1 cm to hold liquid metal, and rub the conductive fiber against it so that the liquid metal is coated on its surface.
[0054] (2) The spinning parameters for preparing the surface insulating layer of the high-conductivity fiber by electrospinning are as follows: the spinning solution concentration is 18wt%, the spinning solute is PVDF, the spinning solvent is acetone and N,N-dimethylmethylamine, the spinning positive voltage is 12.50kV, the spinning negative voltage is -7.50kV, the propulsion speed is 3ml / h, the drum collection speed is 15r / min (i.e. 2.83cm / s), and the bell mouth is 800r / min. Using the same parameter conditions, the spinning solution is used to wrap it 3, 4, and 5 times.
[0055] The obtained high conductivity fiber has a measuring length of 1 cm and the resistance values measured at different positions are taken separately, such as Figure 3 shown.
[0056] Comparative Example 2
[0057] (1) Take an open square box with a size of 1 cm*cm*1 cm to hold liquid metal, and let the conductive fiber pass through it (compared with Example 1, the process of passing through dilute hydrochloric acid is missing), so that the liquid metal is coated on the surface of the conductive fiber.
[0058] (2) The spinning parameters for preparing the surface insulating layer of high-conductivity fiber by electrospinning are: spinning solution concentration is 18wt%, spinning solute is PVDF, spinning solvent is acetone, N,N-dimethylmethylamine, spinning positive voltage is 12.50kV, spinning negative voltage is -7.50kV, propulsion speed is 3ml / h, roller collection speed is 15r / min (i.e. 2.83cm / s), and bell mouth is 800r / min. Using the same parameter conditions, the spinning solution is used to wrap it 3, 4, and 5 times. The high-conductivity fiber obtained has a measuring length of 1cm, and the resistance values measured at multiple groups of different positions are taken, such as Figure 3 shown.
[0059] The wrapping layers were prepared with PVDF, nylon 6, polylactic acid and polyacrylonitrile respectively, and the obtained products were tested. The results are shown in Table 1 below.
[0060] Table 1 Comparison of effects of different wrapping layers
[0061] Solute PVDF Nylon 6 Polylactic acid Polyacrylonitrile Effect Excellent results Not strong enough High surface stickiness Not easy to wrap
[0062] The results in the table above show that PVDF is the best wrapping layer. When nylon 6 is used as the spinning solute, the wrapping layer is not strong and is easily damaged; when polylactic acid is used as the spinning solvent, the surface viscosity of the wrapping layer is too large, and fibers are prone to adhesion during winding; when polyacrylonitrile is used as the spinning solute, no matter how the spinning process is improved, the wrapping effect is not good; when PVDF is used as the spinning solute, a good outer wrapping effect can be easily achieved.
[0063] The resistance values tested in each segment using different processing methods are shown in Table 2.
[0064] Table 2
[0065]
[0066] When the hanging drop method is used, the conductivity of the fibers produced is not significantly improved, and the resistance values of each segment between the fibers are not uniform; when the friction method is used, although the resistance values of each segment between the fibers are uniform, the improvement in conductivity is still low; when the immersion method and the middle-through method are used, the same problems of insufficient improvement in conductivity and uneven resistance values of each segment are faced; when treated with hydrochloric acid, the fibers produced by the middle-through method not only have a significant improvement in conductivity, but also the resistance values of each segment are also uniform.
[0067] The conductive fiber treated with hydrochloric acid in the present invention can better allow liquid metal to adhere to it. Liquid metal is coated on the surface of common conductive fibers so that the two are well organically combined to achieve the effect of making a high-conductivity fiber. An insulating layer is wrapped on the outer layer of the high-conductivity fiber through electrostatic spinning technology. Multiple conjugate spinning is used for wrapping to prevent leakage of liquid metal and to isolate air from oxidation by air, thereby simplifying the preparation process of high-conductivity fiber made by using liquid metal in the prior art.
[0068] Those skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the present invention is limited to these examples; under the concept of the present invention, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity. Any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A conductive fiber coated with liquid metal, characterized in that: The invention comprises acid-treated conductive fibers, a liquid metal coating layer and an outer wrapping layer which are arranged in sequence from the inside to the outside. The acid-treated conductive fibers are obtained by treating the conductive fibers in a dilute hydrochloric acid bath with a concentration of 8-10%.
2. The conductive fiber coated with liquid metal according to claim 1, characterized in that: The conductive fiber is passed through the hydrochloric acid bath by a collecting roller, and the speed of the collecting roller is 15-100 r / min.
3. The conductive fiber coated with liquid metal according to claim 1, characterized in that: The liquid metal is a low-temperature or room-temperature liquid alloy having a melting point of -15-40°C.
4. The conductive fiber coated with liquid metal according to claim 1, characterized in that: The outer wrapping layer is selected from one or more of PVDF, nylon 6, polylactic acid, and polyacrylonitrile.
5. The conductive fiber coated with liquid metal according to claim 1, characterized in that: The conductive fiber is selected from one or more of stainless steel metal fiber, conductive carbon fiber, silver-plated nylon fiber and polypropylamine conductive fiber.
6. The method for preparing a conductive fiber coated with liquid metal according to any one of claims 1 to 5, characterized in that: The steps include: Step 1: The conductive fiber is treated in a dilute hydrochloric acid bath with a concentration of 8-10%; Step 2, coating the conductive fibers treated in step 1 with liquid metal; Step 3: Electrospinning the conductive fibers treated in step 2 to prepare an outer wrapping layer.
7. The method for preparing the conductive fiber coated with liquid metal according to claim 6, characterized in that: The electrospinning described in step three adopts conjugate electrospinning, and the spinning parameters are: the spinning solution concentration is 16-18wt%, the spinning solvent is acetone and N, N-dimethylformamide mixed in a weight ratio of 2:3, the spinning positive voltage is 11.5-14.5kV, the spinning negative voltage is 7.5-9.5kV, the propulsion speed is 2-4ml / h, the drum collection speed is 15-100r / min, and the bell mouth is 800r / min.
8. The method for preparing the conductive fiber coated with liquid metal according to claim 7, characterized in that: The number of wrapping times of the outer wrapping layer prepared by electrospinning is related to whether the liquid metal leaks, the wear resistance of the conductive fiber and the application scenario.
9. Use of the conductive fiber coated with liquid metal according to claims 1-5 in flexible materials, clothing or functional devices.
10. The use according to claim 9, characterized in that: The functional device is a wearable wireless communication device, and its preparation method comprises the following steps: Step 1: preparing the conductive fiber coated with liquid metal as a basic material for constructing a body area network; Step 2: Design a reasonable wireless communication response pattern on the computer to be suitable for the construction of the body area network; Step 3: Using digital integration technology to respond to the pattern, the designed pattern is imported into a digital sewing machine and the prepared conductive fiber coated with liquid metal is used as a bobbin for digital sewing; Step 4: Patterns are sewn on at least two areas of the fabric, the distance between each pattern is adjusted according to the planned body area network, and the patterns are connected and adapted with the conductive fiber coated with liquid metal, so as to achieve the effect of transmitting information data.
Citation Information
Patent Citations
High-conduction-stability superelastic yarn, and preparation method and application thereof
CN111041820A
Yarn-shaped supercapacitor and preparation method thereof
CN115458338A
Liquid metal composite modified metal grid interface material and preparation method thereof
CN116218480A
Method for gesture recognition by using liquid metal sensor
CN117433408A
Embroidery sock system for monitoring and adjuvant therapy of diabetic foot and manufacturing process
CN117752301A
Cited By
Nanofiber yarn coated carbon fiber bundle composite filament and preparation method thereof
CN119980534A
Friction electricity yarn, preparation method thereof and friction nanometer power generation device
CN120649208A
In-situ coating preparation method of liquid metal core wire
CN122599190A