Anti-splashing fabric applied to metal smelting industry

By using interweaving and pretreatment technology of wool, para-aramid fiber and other materials in fabrics in the metallurgical industry, the problem of insufficient protective performance of existing fabrics in high-temperature molten metal splash environments has been solved, and a higher protective effect has been achieved and improved fiber mechanical properties.

CN118792783APending Publication Date: 2024-10-18SHANGHAI LABON TECHNICAL FIBER CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410797121.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Operators in the metallurgical industry face life safety threats in high-temperature baking and molten metal splashing environments. Existing protective fabrics have deficiencies in protective performance and wearing comfort, especially in close-range operating positions such as welding and casting. It is difficult to meet higher protection requirements.

Method used

The fabric is made of interwoven warp and weft yarns, made of wool, para-aramid fiber, nylon, conductive fiber and flame-retardant viscose blend. It has been processed by strip making, recombing, steaming and warping, and is pre-made. Processing to improve fiber machinery Properties, including treatment with gamma-glycidoxypropyltrimethoxysilane, mixtures of polyamic acid and ethanol, dopamine solutions, antimony trichloride and zinc dichloride, to form fibers with reactive functional groups and macromolecular structure .

Benefits of technology

It improves the fabric's anti-molten metal splash performance and water-washing stability, enhances the mechanical properties of the fiber and the durability of the fabric, ensures that it is not easy to break during use, and improves the effect of metallurgical protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004902101300000111
    Figure BDA0004902101300000111
  • Figure BDA0004902101300000121
    Figure BDA0004902101300000121
Patent Text Reader

Abstract

The invention discloses an anti-splashing fabric applied to the metal smelting industry, the anti-splashing fabric is formed by interweaving warp yarns and weft yarns, and the warp yarns and the weft yarns are formed by blending wool, para-aramid fibers, nylon, conductive fibers and flame-retardant viscose as raw materials; the surface density of the fabric ranges from 250 g / m < 2 > to 500 g / m < 2 >, the warp density ranges from 70 pieces / cm to 120 pieces / cm, the weft density ranges from 40 pieces / cm to 100 pieces / cm, and the weave structure is satin weave. The fabric prepared through the method has good molten metal splashing prevention performance and washing stability, the durability of the fabric in the metal metallurgy protection purpose is improved, the mechanical performance of pretreated fibers is remarkably improved, the strength of the fabric is correspondingly improved, and the fabric is not prone to breakage in the using process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal smelting protective fabrics, and in particular to a splash-proof fabric used in the metal smelting industry. Background Art

[0002] As the main raw material industry in my country, the metallurgical industry bears important responsibilities such as social development, national security, and people's needs. Affected by the harsh environment such as high temperature and molten metal splashing during operation, the life safety of operators is often threatened. Especially in close-range operation positions such as electric welding, casting, and metal cutting, operators must wear protective clothing supported by anti-molten metal splash fabrics to protect the body from high temperature invasion or prevent splashing high-temperature substances from causing harm to the human body. With the development of new textile materials and the improvement of social and economic levels in my country, new anti-molten metal splash fabrics must not only meet more professional requirements in terms of protective performance, but also optimize wearing comfort and wearability. Summary of the invention

[0003] To this end, the present invention provides a splash-proof fabric for use in the metal smelting industry, which is interwoven with warp yarns and weft yarns, wherein the warp yarns and weft yarns are blended with wool, para-aramid fiber, nylon, conductive fiber and flame-retardant viscose as raw materials; the fabric surface density is 250-500 g / m 2 , the warp density is 70-120 yarns / cm, the weft density is 40-100 yarns / cm, and the weft structure is satin weave; the preparation process includes:

[0004] (1) slivering the para-aramid fiber to make the para-aramid fiber length between 5 and 1 mm, then combining the para-aramid fiber with the wool and flame-retardant viscose blended sliver, combing the sliver after merging to remove short hair and hair particles; performing four pre-spinning needle combing steps, and then performing two roving steps, and storing the roving at a humidity of 80% for 5 to 6 days;

[0005] (2) Performing a spinning process, the spinning draft is set to 23.9, the twist is 930 T / m, the spindle speed is set to 7000 r / min, and the spinning density is 9.1 tex; after spinning, the winding density is 9.1 tex, and the speed is set to 670 m / min; the yarn is doubled and twisted once, the double twist density is set to 18 tex, and the twist is 1100 T / m; then the yarn is steamed at 85 ° C for 12 min to fix the yarn;

[0006] (3) After the yarn is steamed, it is warped on a warping machine with a warping speed of 300 m / min and a tension of 15 cN. After warping, the yarn is drawn in and woven with the tension of a single warp yarn controlled at 0.3 cN and a machine speed of 350 r / min. After weaving, the yarn is desized at 95 °C for 1 h to remove the size on the surface of the fabric. The yarn is then dried at 120 °C on a setting machine and steamed to improve the setting effect. The steam pressure is set to 275 kPa.

[0007] Furthermore, the mass percentages of wool, para-aramid fiber, nylon, conductive fiber and flame retardant viscose in the yarn are respectively 30% wool, 10% para-aramid fiber, 10% nylon, 48% flame retardant viscose and 2% conductive fiber.

[0008] Furthermore, the para-aramid fiber is subjected to a pretreatment process, and the pretreatment method is:

[0009] Step 1, in a reactor, γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol are mixed uniformly to form a mixture, para-aramid fiber is added to the mixture, and then the reactor is sealed, filled with carbon dioxide to drive out the air in the reactor, and then pressurized to 20 standard atmospheres in the reactor, heated to 65±3° C. in a water bath for 30 to 40 minutes, and then the reactor is opened, solid-liquid separation is carried out, the solid phase is heated to 180° C. in a nitrogen atmosphere for more than 100 minutes, and cooled to room temperature to obtain a once treated fiber;

[0010] Step 2: prepare a Tris solution with a concentration of 10 mmol / L and a pH of 8.5, add dopamine to the Tris solution to prepare a dopamine solution, add the primary treated fiber to the dopamine solution, heat it in a water bath to 50±3° C. for more than 10 minutes, then separate the solid and liquid, and dry the solid phase at 60° C. for more than 30 minutes to obtain a secondary treated fiber;

[0011] Step 3: Add antimony trichloride and zinc dichloride to anhydrous ethanol to form a mixed liquid, stir for more than 10 minutes, then add the secondary treated fiber in a stirring state, continue stirring for 8 to 10 minutes under an ultrasonic environment after the addition is completed, then heat to 65±3°C in a water bath for insulation, condense and reflux, add sodium hydroxide, continue stirring at 65±3°C for more than 30 minutes after the addition is completed, then separate the solid and liquid, wash the solid phase with deionized water for more than 5 times, and dry at 60°C for more than 30 minutes to obtain the pretreated para-aramid fiber.

[0012] Furthermore, in the step one, the mass ratio of γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol is γ-glycidyloxypropyltrimethoxysilane: polyamic acid: ethanol = 5:3:92; the mass ratio of the para-aramid fiber added to the mixture is para-aramid fiber: mixture = 2:100.

[0013] Furthermore, in the step 2, the concentration of dopamine in the dopamine solution is 2-3 g / L, and the mass ratio of the once treated fiber added to the dopamine solution is once treated fiber: dopamine solution = 1:50.

[0014] Furthermore, in the step three, the mass ratio of antimony trichloride and zinc dichloride added to anhydrous ethanol is antimony trichloride: zinc dichloride: anhydrous ethanol = 4-6:10-12:100; the mass ratio of the added mass of the secondary treated fiber and sodium hydroxide to the mixed liquid is secondary treated fiber: sodium hydroxide: mixed liquid = 1:0.5-0.6:50.

[0015] The beneficial effects of the present invention are as follows: the fabric prepared by the method of the present invention has good molten metal splash resistance and water washing stability, which improves the durability of the fabric in metal metallurgical protection applications, and the mechanical properties of the fiber after pretreatment are significantly improved, which correspondingly improves the strength of the fabric and makes it less likely to break during use. DETAILED DESCRIPTION

[0016] The present invention will be further described below in conjunction with the embodiments.

[0017] Example 1

[0018] A splash-proof fabric used in the metal smelting industry, which is interwoven with warp yarns and weft yarns, which are blended with wool, 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose as raw materials; the wool, 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose in the yarn have a mass percentage of 30% wool, 10% 1414 para-aramid fiber, 10% nylon, 48% flame-retardant viscose and 2% nylon-based conductive fiber. The fabric surface density is 300g / m 2 , the warp density is 100 yarns / cm, the weft density is 80 yarns / cm, and the weft structure is satin weave; the preparation process includes:

[0019] (1) slivering the 1414 para-aramid fiber to make the para-aramid fiber length between 5 and 1 mm, then combining the slivered 1414 para-aramid fiber with the wool and flame-retardant viscose blended sliver, combing the slivered 1414 para-aramid fiber to remove short hair and hair particles, performing four pre-spinning needle combing steps, and then performing two roving steps, and storing the roving at a humidity of 80% for 5 days;

[0020] (2) Performing a spinning process, the spinning draft is set to 23.9, the twist is 930 T / m, the spindle speed is set to 7000 r / min, and the spinning density is 9.1 tex; after spinning, the winding density is 9.1 tex, and the speed is set to 670 m / min; the yarn is doubled and twisted once, the double twist density is set to 18 tex, and the twist is 1100 T / m; then the yarn is steamed at 85 ° C for 12 min to fix the yarn;

[0021] (3) After the yarn is steamed, it is warped on a warping machine with a warping speed of 300 m / min and a tension of 15 cN. After warping, the yarn is drawn into the reeds and woven with the tension of a single warp yarn controlled at 0.3 cN and a machine speed of 350 r / min. After weaving, the yarn is desized at 95 °C for 1 h to remove the sizing on the surface of the fabric. The yarn is then dried on a setting machine at 120 °C and steamed to improve the setting effect to obtain the fabric. The desizing pressure is set to 275 kPa.

[0022] Example 2

[0023] A splash-proof fabric used in the metal smelting industry, which is interwoven with warp yarns and weft yarns, which are blended with wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose as raw materials; the wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose in the yarn have a mass percentage of 30% wool, 10% pretreated 1414 para-aramid fiber, 10% nylon, 48% flame-retardant viscose and 2% nylon-based conductive fiber. The fabric surface density is 300g / m 2 , the warp density is 100 yarns / cm, the weft density is 80 yarns / cm, and the weft structure is satin weave; the preparation process includes:

[0024] (1) slivering the pretreated 1414 para-aramid fiber to make the para-aramid fiber length between 5 and 1 mm, then combining the slivered para-aramid fiber with the wool and flame-retardant viscose blended sliver, combing the slivered fiber to remove short hair and hair particles, performing four pre-spinning needle combing steps, and then performing two roving steps, and storing the roving at a humidity of 80% for 5 days;

[0025] (2) Performing a spinning process, the spinning draft is set to 23.9, the twist is 930 T / m, the spindle speed is set to 7000 r / min, and the spinning density is 9.1 tex; after spinning, the winding density is 9.1 tex, and the speed is set to 670 m / min; the yarn is doubled and twisted once, the double twist density is set to 18 tex, and the twist is 1100 T / m; then the yarn is steamed at 85 ° C for 12 min to fix the yarn;

[0026] (3) After the yarn is steamed, it is warped on a warping machine with a warping speed of 300 m / min and a tension of 15 cN. After warping, the yarn is drawn into the reeds and woven with the tension of a single warp yarn controlled at 0.3 cN and a machine speed of 350 r / min. After weaving, the yarn is desized at 95 °C for 1 h to remove the sizing on the surface of the fabric. The yarn is then dried on a setting machine at 120 °C and steamed to improve the setting effect to obtain the fabric. The desizing pressure is set to 275 kPa.

[0027] The pretreatment method is:

[0028] Step 1, in a reactor, γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol are mixed uniformly to form a mixture, wherein the mass ratio of γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol is γ-glycidyloxypropyltrimethoxysilane: polyamic acid: ethanol = 5:3:92; 1414 para-aramid fiber is added to the mixture, and the mass ratio of para-aramid fiber to the mixture is para-aramid fiber: mixture = 2:100; then the reactor is sealed, filled with carbon dioxide to drive out the air in the reactor, and then pressurized to 20 standard atmospheres in the reactor, heated to 65±3°C in a water bath for 30 minutes, and then opened the reactor, solid-liquid separation, the solid phase is heated to 180°C in a nitrogen atmosphere for 100 minutes, and cooled to room temperature to obtain a once treated fiber;

[0029] Step 2, prepare a Tris solution with a concentration of 10 mmol / L and a pH of 8.5, add dopamine to the Tris solution to prepare a dopamine solution, wherein the concentration of dopamine is 2 g / L, add the primary treated fiber to the dopamine solution, and the mass ratio of the primary treated fiber to the dopamine solution is primary treated fiber: dopamine solution = 1:50; heat in a water bath to 50±3°C for 10 min, then separate the solid and liquid, and dry the solid phase at 60°C for 30 min to obtain the secondary treated fiber;

[0030] Step 3, antimony trichloride and zinc dichloride are added to anhydrous ethanol to form a mixed solution, the mass ratio of antimony trichloride and zinc dichloride added to anhydrous ethanol is antimony trichloride: zinc dichloride: anhydrous ethanol = 4:10:100; stirring for 10 minutes, and then adding the secondary treated fiber in a stirring state. After the addition is completed, stirring is continued for 8 minutes in an ultrasonic (600W, 20kHz) environment, and then heated to 65±3°C in a water bath for insulation, condensed and refluxed, and sodium hydroxide is added. The mass ratio of the added mass of the secondary treated fiber and sodium hydroxide to the mixed solution is secondary treated fiber: sodium hydroxide: mixed solution = 1:0.5:50; after the addition is completed, stirring is continued at 65±3°C for 30 minutes, and then solid-liquid separation is performed, the solid phase is washed 5 times with deionized water, and dried at 60°C for 30 minutes to obtain the pretreated 1414 para-aramid fiber.

[0031] Example 3

[0032] A splash-proof fabric used in the metal smelting industry, which is interwoven with warp yarns and weft yarns, which are blended with wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose as raw materials; the wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose in the yarn have a mass percentage of 30% wool, 10% pretreated 1414 para-aramid fiber, 10% nylon, 48% flame-retardant viscose and 2% nylon-based conductive fiber. The fabric surface density is 300g / m 2 , the warp density is 100 yarns / cm, the weft density is 80 yarns / cm, and the weft structure is satin weave; the preparation process includes:

[0033] (1) slivering the pretreated 1414 para-aramid fiber to make the para-aramid fiber length between 5 and 1 mm, then combining the slivered para-aramid fiber with the wool and flame-retardant viscose blended sliver, combing the slivered fiber to remove short hair and hair particles, performing four pre-spinning needle combing steps, and then performing two roving steps, and storing the roving at a humidity of 80% for 5 days;

[0034] (2) Performing a spinning process, the spinning draft is set to 23.9, the twist is 930 T / m, the spindle speed is set to 7000 r / min, and the spinning density is 9.1 tex; after spinning, the winding density is 9.1 tex, and the speed is set to 670 m / min; the yarn is doubled and twisted once, the double twist density is set to 18 tex, and the twist is 1100 T / m; then the yarn is steamed at 85 ° C for 12 min to fix the yarn;

[0035] (3) After the yarn is steamed, it is warped on a warping machine with a warping speed of 300 m / min and a tension of 15 cN. After warping, the yarn is drawn into the reeds and woven with the tension of a single warp yarn controlled at 0.3 cN and a machine speed of 350 r / min. After weaving, the yarn is desized at 95 °C for 1 h to remove the sizing on the surface of the fabric. The yarn is then dried on a setting machine at 120 °C and steamed to improve the setting effect to obtain the fabric. The desizing pressure is set to 275 kPa.

[0036] The pretreatment method is:

[0037] Step 1, in a reactor, γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol are mixed uniformly to form a mixture, wherein the mass ratio of γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol is γ-glycidyloxypropyltrimethoxysilane: polyamic acid: ethanol = 5:3:92; 1414 para-aramid fiber is added to the mixture, and the mass ratio of para-aramid fiber to the mixture is para-aramid fiber: mixture = 2:100; then the reactor is sealed, filled with carbon dioxide to drive out the air in the reactor, and then pressurized to 20 standard atmospheres in the reactor, heated to 65±3°C in a water bath for 30 minutes, and then opened the reactor, solid-liquid separation, the solid phase is heated to 180°C in a nitrogen atmosphere for 100 minutes, and cooled to room temperature to obtain a once treated fiber;

[0038] Step 2, prepare a Tris solution with a concentration of 10 mmol / L and a pH of 8.5, add dopamine to the Tris solution to prepare a dopamine solution, wherein the concentration of dopamine is 3 g / L, add the primary treated fiber to the dopamine solution, and the mass ratio of the primary treated fiber to the dopamine solution is primary treated fiber: dopamine solution = 1:50; heat in a water bath to 50±3°C for 10 min, then separate the solid and liquid, and dry the solid phase at 60°C for 30 min to obtain the secondary treated fiber;

[0039] Step 3, antimony trichloride and zinc dichloride are added to anhydrous ethanol to form a mixed solution, the mass ratio of antimony trichloride and zinc dichloride added to anhydrous ethanol is antimony trichloride: zinc dichloride: anhydrous ethanol = 5:11:100; stirring for 10 minutes, and then adding the secondary treated fiber in a stirring state. After the addition is completed, stirring is continued for 8 minutes in an ultrasonic (600W, 20kHz) environment, and then heated to 65±3°C in a water bath for insulation, condensed and refluxed, and sodium hydroxide is added. The mass ratio of the added mass of the secondary treated fiber and sodium hydroxide to the mixed solution is secondary treated fiber: sodium hydroxide: mixed solution = 1:0.6:50; after the addition is completed, stirring is continued at 65±3°C for 30 minutes, and then solid-liquid separation is performed, the solid phase is washed 5 times with deionized water, and dried at 60°C for 30 minutes to obtain the pretreated 1414 para-aramid fiber.

[0040] Example 4

[0041] A splash-proof fabric used in the metal smelting industry, which is interwoven with warp yarns and weft yarns, which are blended with wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose as raw materials; the wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose in the yarn have a mass percentage of 30% wool, 10% pretreated 1414 para-aramid fiber, 10% nylon, 48% flame-retardant viscose and 2% nylon-based conductive fiber. The fabric surface density is 300g / m 2 , the warp density is 100 yarns / cm, the weft density is 80 yarns / cm, and the weft structure is satin weave; the preparation process includes:

[0042] (1) slivering the pretreated 1414 para-aramid fiber to make the para-aramid fiber length between 5 and 1 mm, then combining the slivered para-aramid fiber with the wool and flame-retardant viscose blended sliver, combing the slivered fiber to remove short hair and hair particles, performing four pre-spinning needle combing steps, and then performing two roving steps, and storing the roving at a humidity of 80% for 5 days;

[0043] (2) Performing a spinning process, the spinning draft is set to 23.9, the twist is 930 T / m, the spindle speed is set to 7000 r / min, and the spinning density is 9.1 tex; after spinning, the winding density is 9.1 tex, and the speed is set to 670 m / min; the yarn is doubled and twisted once, the double twist density is set to 18 tex, and the twist is 1100 T / m; then the yarn is steamed at 85 ° C for 12 min to fix the yarn;

[0044] (3) After the yarn is steamed, it is warped on a warping machine with a warping speed of 300 m / min and a tension of 15 cN. After warping, the yarn is drawn into the reeds and woven with the tension of a single warp yarn controlled at 0.3 cN and a machine speed of 350 r / min. After weaving, the yarn is desized at 95 °C for 1 h to remove the sizing on the surface of the fabric. The yarn is then dried on a setting machine at 120 °C and steamed to improve the setting effect to obtain the fabric. The desizing pressure is set to 275 kPa.

[0045] The pretreatment method is:

[0046] Step 1, in a reactor, γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol are mixed uniformly to form a mixture, wherein the mass ratio of γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol is γ-glycidyloxypropyltrimethoxysilane: polyamic acid: ethanol = 5:3:92; 1414 para-aramid fiber is added to the mixture, and the mass ratio of para-aramid fiber to the mixture is para-aramid fiber: mixture = 2:100; then the reactor is sealed, filled with carbon dioxide to drive out the air in the reactor, and then pressurized to 20 standard atmospheres in the reactor, heated to 65±3°C in a water bath for 30 minutes, and then opened the reactor, solid-liquid separation, the solid phase is heated to 180°C in a nitrogen atmosphere for 100 minutes, and cooled to room temperature to obtain a once treated fiber;

[0047] Step 2, prepare a Tris solution with a concentration of 10 mmol / L and a pH of 8.5, add dopamine to the Tris solution to prepare a dopamine solution, wherein the concentration of dopamine is 3 g / L, add the primary treated fiber to the dopamine solution, and the mass ratio of the primary treated fiber to the dopamine solution is primary treated fiber: dopamine solution = 1:50; heat in a water bath to 50±3°C for 10 min, then separate the solid and liquid, and dry the solid phase at 60°C for 30 min to obtain the secondary treated fiber;

[0048] Step 3, antimony trichloride and zinc dichloride are added to anhydrous ethanol to form a mixed solution, the mass ratio of antimony trichloride and zinc dichloride added to anhydrous ethanol is antimony trichloride: zinc dichloride: anhydrous ethanol = 6:12:100; stirring for 10 minutes, and then adding the secondary treated fiber in a stirring state. After the addition is completed, stirring is continued for 8 minutes in an ultrasonic (600W, 20kHz) environment, and then heated to 65±3°C in a water bath for insulation, condensed and refluxed, and sodium hydroxide is added. The mass ratio of the added mass of the secondary treated fiber and sodium hydroxide to the mixed solution is secondary treated fiber: sodium hydroxide: mixed solution = 1:0.6:50; after the addition is completed, stirring is continued at 65±3°C for 30 minutes, and then solid-liquid separation is performed, the solid phase is washed 5 times with deionized water, and dried at 60°C for 30 minutes to obtain the pretreated 1414 para-aramid fiber.

[0049] Comparative Example 1

[0050] A splash-proof fabric used in the metal smelting industry, which is interwoven with warp yarns and weft yarns, which are blended with wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose as raw materials; the wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose in the yarn have a mass percentage of 30% wool, 10% pretreated 1414 para-aramid fiber, 10% nylon, 48% flame-retardant viscose and 2% nylon-based conductive fiber. The fabric surface density is 300g / m 2 , the warp density is 100 yarns / cm, the weft density is 80 yarns / cm, and the weft structure is satin weave; the preparation process includes:

[0051] (1) slivering the pretreated 1414 para-aramid fiber to make the para-aramid fiber length between 5 and 1 mm, then combining the slivered para-aramid fiber with the wool and flame-retardant viscose blended sliver, combing the slivered fiber to remove short hair and hair particles, performing four pre-spinning needle combing steps, and then performing two roving steps, and storing the roving at a humidity of 80% for 5 days;

[0052] (2) Performing a spinning process, the spinning draft is set to 23.9, the twist is 930 T / m, the spindle speed is set to 7000 r / min, and the spinning density is 9.1 tex; after spinning, the winding density is 9.1 tex, and the speed is set to 670 m / min; the yarn is doubled and twisted once, the double twist density is set to 18 tex, and the twist is 1100 T / m; then the yarn is steamed at 85 ° C for 12 min to fix the yarn;

[0053] (3) After the yarn is steamed, it is warped on a warping machine with a warping speed of 300 m / min and a tension of 15 cN. After warping, the yarn is drawn into the reeds and woven with the tension of a single warp yarn controlled at 0.3 cN and a machine speed of 350 r / min. After weaving, the yarn is desized at 95 °C for 1 h to remove the sizing on the surface of the fabric. The yarn is then dried on a setting machine at 120 °C and steamed to improve the setting effect to obtain the fabric. The desizing pressure is set to 275 kPa.

[0054] The pretreatment method is:

[0055] Step 1, prepare a Tris solution with a concentration of 10 mmol / L and a pH of 8.5, add dopamine to the Tris solution to prepare a dopamine solution, wherein the concentration of dopamine is 3 g / L, add 1414 para-aramid fiber to the dopamine solution, and the mass ratio of the 1414 para-aramid fiber to the dopamine solution is 1414 para-aramid fiber: dopamine solution = 1:50; heat in a water bath to 50±3°C for 10 minutes, then separate the solid and liquid, and dry the solid phase at 60°C for 30 minutes to obtain the primary treated fiber of this comparative example;

[0056] Step 2, antimony trichloride and zinc dichloride are added to anhydrous ethanol to form a mixed solution, the mass ratio of antimony trichloride and zinc dichloride added to anhydrous ethanol is antimony trichloride: zinc dichloride: anhydrous ethanol = 5:11:100; stirring for 10 minutes, and then adding the once treated fiber under stirring. After the addition is completed, stirring is continued for 8 minutes under an ultrasonic (600W, 20kHz) environment, and then heated to 65±3°C in a water bath for insulation, condensed and refluxed, and sodium hydroxide is added. The mass ratio of the once treated fiber and sodium hydroxide added to the mixed solution is once treated fiber: sodium hydroxide: mixed solution = 1:0.6:50; after the addition is completed, stirring is continued at 65±3°C for 30 minutes, and then solid-liquid separation is performed, the solid phase is washed 5 times with deionized water, and dried at 60°C for 30 minutes to obtain the pretreated 1414 para-aramid fiber described in this comparative example.

[0057] Comparative Example 2

[0058] A splash-proof fabric used in the metal smelting industry, which is interwoven with warp yarns and weft yarns, which are blended with wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose as raw materials; the wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose in the yarn have a mass percentage of 30% wool, 10% pretreated 1414 para-aramid fiber, 10% nylon, 48% flame-retardant viscose and 2% nylon-based conductive fiber. The fabric surface density is 300g / m 2 , the warp density is 100 yarns / cm, the weft density is 80 yarns / cm, and the weft structure is satin weave; the preparation process includes:

[0059] (1) slivering the pretreated 1414 para-aramid fiber to make the para-aramid fiber length between 5 and 1 mm, then combining the slivered para-aramid fiber with the wool and flame-retardant viscose blended sliver, combing the slivered fiber to remove short hair and hair particles, performing four pre-spinning needle combing steps, and then performing two roving steps, and storing the roving at a humidity of 80% for 5 days;

[0060] (2) Performing a spinning process, the spinning draft is set to 23.9, the twist is 930 T / m, the spindle speed is set to 7000 r / min, and the spinning density is 9.1 tex; after spinning, the winding density is 9.1 tex, and the speed is set to 670 m / min; the yarn is doubled and twisted once, the double twist density is set to 18 tex, and the twist is 1100 T / m; then the yarn is steamed at 85 ° C for 12 min to fix the yarn;

[0061] (3) After the yarn is steamed, it is warped on a warping machine with a warping speed of 300 m / min and a tension of 15 cN. After warping, the yarn is drawn into the reeds and woven with the tension of a single warp yarn controlled at 0.3 cN and a machine speed of 350 r / min. After weaving, the yarn is desized at 95 °C for 1 h to remove the sizing on the surface of the fabric. The yarn is then dried on a setting machine at 120 °C and steamed to improve the setting effect to obtain the fabric. The desizing pressure is set to 275 kPa.

[0062] The pretreatment method is:

[0063] Step 1, in a reactor, γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol are mixed uniformly to form a mixture, wherein the mass ratio of γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol is γ-glycidyloxypropyltrimethoxysilane: polyamic acid: ethanol = 5:3:92; 1414 para-aramid fiber is added to the mixture, and the mass ratio of para-aramid fiber to the mixture is para-aramid fiber: mixture = 2:100; then the reactor is sealed, filled with carbon dioxide to drive out the air in the reactor, and then pressurized to 20 standard atmospheres in the reactor, heated to 65±3°C in a water bath for 30 minutes, and then opened the reactor, solid-liquid separation, the solid phase is heated to 180°C in a nitrogen atmosphere for 100 minutes, and cooled to room temperature to obtain a once treated fiber;

[0064] Step 2, antimony trichloride and zinc dichloride are added to anhydrous ethanol to form a mixed solution, the mass ratio of antimony trichloride and zinc dichloride added to anhydrous ethanol is antimony trichloride: zinc dichloride: anhydrous ethanol = 5:11:100; stirring for 10 minutes, and then adding the once treated fiber under stirring. After the addition is completed, stirring is continued for 8 minutes under an ultrasonic (600W, 20kHz) environment, and then heated to 65±3°C in a water bath for insulation, condensed and refluxed, and sodium hydroxide is added. The mass ratio of the once treated fiber and sodium hydroxide added to the mixed solution is once treated fiber: sodium hydroxide: mixed solution = 1:0.6:50; after the addition is completed, stirring is continued at 65±3°C for 30 minutes, and then solid-liquid separation is performed, the solid phase is washed 5 times with deionized water, and dried at 60°C for 30 minutes to obtain the pretreated 1414 para-aramid fiber described in this comparative example.

[0065] Comparative Example 3

[0066] A splash-proof fabric used in the metal smelting industry, which is interwoven with warp yarns and weft yarns, which are blended with wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose as raw materials; the wool, pretreated 1414 para-aramid fiber, nylon, nylon-based conductive fiber and flame-retardant viscose in the yarn have a mass percentage of 30% wool, 10% pretreated 1414 para-aramid fiber, 10% nylon, 48% flame-retardant viscose and 2% nylon-based conductive fiber. The fabric surface density is 300g / m 2 , the warp density is 100 yarns / cm, the weft density is 80 yarns / cm, and the weft structure is satin weave; the preparation process includes:

[0067] (1) slivering the pretreated 1414 para-aramid fiber to make the para-aramid fiber length between 5 and 1 mm, then combining the slivered para-aramid fiber with the wool and flame-retardant viscose blended sliver, combing the slivered fiber to remove short hair and hair particles, performing four pre-spinning needle combing steps, and then performing two roving steps, and storing the roving at a humidity of 80% for 5 days;

[0068] (2) Performing a spinning process, the spinning draft is set to 23.9, the twist is 930 T / m, the spindle speed is set to 7000 r / min, and the spinning density is 9.1 tex; after spinning, the winding density is 9.1 tex, and the speed is set to 670 m / min; the yarn is doubled and twisted once, the double twist density is set to 18 tex, and the twist is 1100 T / m; then the yarn is steamed at 85 ° C for 12 min to fix the yarn;

[0069] (3) After the yarn is steamed, it is warped on a warping machine with a warping speed of 300 m / min and a tension of 15 cN. After warping, the yarn is drawn into the reeds and woven with the tension of a single warp yarn controlled at 0.3 cN and a machine speed of 350 r / min. After weaving, the yarn is desized at 95 °C for 1 h to remove the sizing on the surface of the fabric. The yarn is then dried on a setting machine at 120 °C and steamed to improve the setting effect to obtain the fabric. The desizing pressure is set to 275 kPa.

[0070] The pretreatment method is:

[0071] Step 1, in a reactor, γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol are mixed uniformly to form a mixture, wherein the mass ratio of γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol is γ-glycidyloxypropyltrimethoxysilane: polyamic acid: ethanol = 5:3:92; 1414 para-aramid fiber is added to the mixture, and the mass ratio of para-aramid fiber to the mixture is para-aramid fiber: mixture = 2:100; then the reactor is sealed, filled with carbon dioxide to drive out the air in the reactor, and then pressurized to 20 standard atmospheres in the reactor, heated to 65±3°C in a water bath for 30 minutes, and then opened the reactor, solid-liquid separation, the solid phase is heated to 180°C in a nitrogen atmosphere for 100 minutes, and cooled to room temperature to obtain a once treated fiber;

[0072] Step 2, prepare a Tris solution with a concentration of 10 mmol / L and a pH of 8.5, add dopamine to the Tris solution to prepare a dopamine solution, wherein the concentration of dopamine is 3 g / L, add the primary treated fiber to the dopamine solution, and the mass ratio of the primary treated fiber to the dopamine solution is primary treated fiber: dopamine solution = 1:50; heat in a water bath to 50±3°C for 10 min, then separate the solid and liquid, and dry the solid phase at 60°C for 30 min to obtain the secondary treated fiber;

[0073] Step 3, zinc dichloride is added to anhydrous ethanol to form a mixed solution, the mass ratio of zinc dichloride to anhydrous ethanol is zinc dichloride: anhydrous ethanol = 11:100; stirring for 10 minutes, and then adding the secondary treated fiber under stirring. After the addition is completed, stirring is continued for 8 minutes under an ultrasonic (600W, 20kHz) environment, and then heated to 65±3°C in a water bath for insulation, condensed and refluxed, and sodium hydroxide is added. The mass ratio of the added mass of the secondary treated fiber and sodium hydroxide to the mixed solution is secondary treated fiber: sodium hydroxide: mixed solution = 1:0.6:50; after the addition is completed, stirring is continued at 65±3°C for 30 minutes, and then the solid-liquid is separated, the solid phase is washed with deionized water 5 times, and dried at 60°C for 30 minutes to obtain the pretreated 1414 para-aramid fiber described in this comparative example.

[0074] Example 5

[0075] The anti-molten aluminum splash level and the anti-molten iron splash level of the fabrics prepared by the methods described in the above embodiments and comparative examples were tested according to the requirements of standard ISO11612-2008. In addition, the shrinkage rate of each fabric after washing 5 times at 60°C was tested respectively. In addition, the breaking strength of the fiber monofilament after pretreatment described in each embodiment and comparative example was measured. The results are shown in Table 1.

[0076] As shown in Table 1, the fabric prepared by the method of the present invention has good molten metal splash resistance and water washing stability, improves the durability of the fabric in metal metallurgical protection, and the mechanical properties of the fiber after pretreatment are significantly improved, and the strength of the fabric is correspondingly improved, and it is not easy to break during use. This is mainly because a large number of active functional groups and macromolecular structures are grafted on the microstructure surface of the fiber after pretreatment, and the active functional groups and macromolecular structures are entangled or hydrogen bonds are formed between each other, which improves the overall mechanical strength of the fiber. At the same time, the hydrogen bonds on the microstructure surface are reconstructed through zinc-antimony treatment, so that the microstructure connection in the fiber is more tightly connected, and the strength of the single fiber is improved.

[0077] Table 1

[0078]

[0079]

[0080] The technical solution provided by the present invention is introduced in detail above. For those skilled in the art, according to the concept of the embodiments of the present invention, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A splash-proof fabric used in the metal smelting industry, characterized in that: The fabric is interwoven with warp yarn and weft yarn, wherein the warp yarn and weft yarn are blended with wool, para-aramid fiber, nylon, conductive fiber and flame-retardant viscose as raw materials; the fabric surface density is 250-500g / m 2 , the warp density is 70-120 yarns / cm, the weft density is 40-100 yarns / cm, and the weft structure is satin weave; The preparation process includes: (1) slivering the para-aramid fiber to make the para-aramid fiber length between 5 and 1 mm, then combining the para-aramid fiber with the wool and flame-retardant viscose blended sliver, combing the sliver after merging to remove short hair and hair particles; performing four pre-spinning needle combing steps, and then performing two roving steps, and storing the roving at a humidity of 80% for 5 to 6 days; (2) Performing a spinning process, the spinning draft is set to 23.9, the twist is 930 T / m, the spindle speed is set to 7000 r / min, and the spinning density is 9.1 tex; after spinning, the winding density is 9.1 tex, and the speed is set to 670 m / min; the yarn is doubled and twisted once, the double twist density is set to 18 tex, and the twist is 1100 T / m; then the yarn is steamed at 85 ° C for 12 min to fix the yarn; (3) After the yarn is steamed, it is warped on a warping machine with a warping speed of 300 m / min and a tension of 15 cN. After warping, the yarn is drawn in and woven with the tension of a single warp yarn controlled at 0.3 cN and a machine speed of 350 r / min. After weaving, the yarn is desized at 95 °C for 1 h to remove the size on the surface of the fabric. The yarn is then dried at 120 °C on a setting machine and steamed to improve the setting effect. The steam pressure is set to 275 kPa.

2. The splash-proof fabric used in the metal smelting industry according to claim 1, characterized in that: The mass percentages of wool, para-aramid fiber and flame retardant viscose in the yarn are respectively 30% wool, 10% para-aramid fiber, 10% nylon, 48% flame retardant viscose and 2% conductive fiber.

3. The splash-proof fabric used in the metal smelting industry according to claim 1, characterized in that: The para-aramid fiber is subjected to a pretreatment process, and the pretreatment method is: Step 1, in a reactor, γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol are mixed uniformly to form a mixture, para-aramid fiber is added to the mixture, and then the reactor is sealed, filled with carbon dioxide to drive out the air in the reactor, and then pressurized to 20 standard atmospheres in the reactor, heated to 65±3° C. in a water bath for 30 to 40 minutes, and then the reactor is opened, solid-liquid separation is carried out, the solid phase is heated to 180° C. in a nitrogen atmosphere for more than 100 minutes, and cooled to room temperature to obtain a once treated fiber; Step 2: prepare a Tris solution with a concentration of 10 mmol / L and a pH of 8.5, add dopamine to the Tris solution to prepare a dopamine solution, add the primary treated fiber to the dopamine solution, heat it in a water bath to 50±3° C. for more than 10 minutes, then separate the solid and liquid, and dry the solid phase at 60° C. for more than 30 minutes to obtain a secondary treated fiber; Step 3: Add antimony trichloride and zinc dichloride to anhydrous ethanol to form a mixed liquid, stir for more than 10 minutes, then add the secondary treated fiber in a stirring state, continue stirring for 8 to 10 minutes under an ultrasonic environment after the addition is completed, then heat to 65±3°C in a water bath for insulation, condense and reflux, add sodium hydroxide, continue stirring at 65±3°C for more than 30 minutes after the addition is completed, then separate the solid and liquid, wash the solid phase with deionized water for more than 5 times, and dry at 60°C for more than 30 minutes to obtain the pretreated para-aramid fiber.

4. The splash-proof fabric used in the metal smelting industry according to claim 3, characterized in that: In the step 1, the mass ratio of γ-glycidyloxypropyltrimethoxysilane, polyamic acid and ethanol is γ-glycidyloxypropyltrimethoxysilane: polyamic acid: ethanol = 5:3:92; the mass ratio of the para-aramid fiber added to the mixture is para-aramid fiber: mixture = 2:

100.

5. The splash-proof fabric used in the metal smelting industry according to claim 3, characterized in that: In the step 2, the concentration of dopamine in the dopamine solution is 2-3 g / L, and the mass ratio of the once treated fiber added to the dopamine solution is once treated fiber: dopamine solution = 1:

50.

6. The splash-proof fabric used in the metal smelting industry according to claim 3, characterized in that: In the step 3, the mass ratio of antimony trichloride and zinc dichloride added to anhydrous ethanol is antimony trichloride: zinc dichloride: anhydrous ethanol = 4-6:10-12:100; the mass ratio of the added mass of the secondary treated fiber and sodium hydroxide to the mixed liquid is secondary treated fiber: sodium hydroxide: mixed liquid = 1:0.5-0.6:50.

Citation Information

Patent Citations

  • Fabric capable of preventing metal splashing

    CN104674425A

  • Chemical modification method for surface of aramid fiber and application of same in preparation of silver-coated aramid composite fiber

    CN105839402A

  • Surface modified aramid fiber and preparation method thereof

    CN108642862A

  • Surface grafting treatment method for aramid fibers

    CN109468846A

  • Molten metal splashing protection fabric and production method thereof

    CN109797474A