Fano resonance color filter and preparation method thereof

By introducing the Fano resonance effect and vanadium dioxide phase change control into the color filter, and combining the resonance of broadband and narrowband filters, the problem of the inability of existing color filters to dynamically modulate color is solved, achieving high responsivity and high brightness. color filters for a variety of applications.

CN118795583APending Publication Date: 2024-10-18UNIV OF SHANGHAI FOR SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410927000.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing color filters cannot dynamically modulate color after preparation, which limits their practical application. Moreover, the color response of structural color devices based on vanadium dioxide is poor.

Method used

The Fano resonance color filter structure is adopted, including a metal base layer, a silicon dielectric layer, an intermediate metal layer, a vanadium dioxide layer and a top metal layer. By adjusting the temperature of the vanadium dioxide layer, its refractive index is changed to achieve dynamic control. Combined with The resonance effect of broadband filters and narrowband filters enhances color response.

Benefits of technology

It realizes the dynamic modulation ability of color filters, has good color response, and has structural colors with high saturation and high brightness. It is suitable for optical instruments, color display, anti-counterfeiting and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118795583A_ABST
    Figure CN118795583A_ABST
Patent Text Reader

Abstract

The invention provides a Fano resonance color filter and a preparation method thereof, and the color filter comprises a metal substrate layer, a silicon dielectric layer, a middle metal layer, a vanadium dioxide layer and a top metal layer which are sequentially arranged from bottom to top. Wherein a square groove is etched on the top metal layer, and the depth of the square groove is equal to the thickness of the top metal layer. According to the invention, the phase change characteristic of vanadium dioxide is utilized, and the vanadium dioxide layer is heated or cooled, so that the device can be modulated to generate fano resonance, the structural color reflected by the device is controlled, and the function of a dynamic color filter is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of color filters, and in particular relates to a Fano resonance color filter and a preparation method thereof. Background Art

[0002] Structural colors have been widely studied and applied in the fields of color printing, optical anti-counterfeiting, and data encryption due to their advantages of high resolution, non-fading, and environmental friendliness. In recent years, a series of subwavelength artificial micro-nano structures (surface plasmon structures, metasurfaces, etc.) have shown significant advantages in controlling and manipulating light-matter interactions at the subwavelength scale, and have been favored in the field of micro-nano optical regulation.

[0003] Generally speaking, the special spectral characteristics of these metamaterials are generated by the optical resonance caused by the composite nanostructure. This type of static micro-nanostructure device has fixed optical functions after preparation, and it is difficult to cope with the complex and changeable practical application needs. Previously, there was a color filter, the Chinese invention patent "A cross-hole structure adjustable luminescent color filter and its preparation method", patent publication number: CN116594092A. The structural color reflected by the color filter has the advantages of high saturation and high brightness, and the color can be tuned by changing the period of the periodic cross hole, but when the device is prepared, it is impossible to dynamically modulate the color according to actual needs, which limits its practical application.

[0004] In order to solve the above problems, by introducing an optically adjustable material into a subwavelength structure, the optical properties of the device can be adjusted by changing the electric field, temperature or mechanical state, thereby realizing dynamic tuning of the optical device. Vanadium dioxide undergoes an insulator-metal phase transition near its phase transition temperature (340K), and the crystal structure also changes from a monoclinic structure to a rutile structure. The vanadium dioxide phase transition can be made by thermal excitation, and because it has a significant difference in refractive index before and after the phase transition, it is suitable for dynamic regulation of optical devices. However, the existing structural color devices based on vanadium dioxide have good dynamic modulation performance (color difference caused by the phase transition of vanadium dioxide), but the color response of the device (color purity and brightness) is poor. Previously, there was a color filter, a Chinese invention patent "a vanadium dioxide film and its preparation method and application", patent publication number: CN108796452A. The vanadium dioxide film has a simple structure, good uniformity, is suitable for large-scale industrialization, has the ability to dynamically modulate color, but the color saturation of the structural color is not high. Summary of the invention

[0005] The purpose of the present invention is to provide a Fano resonance color filter and a preparation method thereof, which realizes dynamic tuning of the color filter by combining a broadband filter with a narrowband filter based on the Fano resonance effect and introducing vanadium dioxide for phase change regulation. The method has the advantages of convenient implementation, easy regulation, good dynamic modulation capability and color response, and can be applied to the fields of optical instruments, color display and anti-counterfeiting. The technical scheme adopted is as follows:

[0006] A Fano resonance color filter, comprising:

[0007] A metal base layer, a silicon dielectric layer, an intermediate metal layer, a vanadium dioxide layer and a top metal layer are sequentially arranged from bottom to top;

[0008] Wherein, periodic square grooves are etched on the top metal layer, and the depth of the square grooves is equal to the thickness of the top metal layer.

[0009] Preferably, the refractive index of vanadium dioxide in the visible light band is adjusted by adjusting the temperature of the vanadium dioxide layer.

[0010] Preferably, the metal base layer is an Ag layer.

[0011] Preferably, the intermediate metal layer is an Ag layer.

[0012] Preferably, the top metal layer is an Ag layer.

[0013] Preferably, the thickness of the silicon dielectric layer is 50 nm, the thickness of the middle metal layer is 40 nm, the thickness of the vanadium dioxide layer is 40 nm, and the thickness of the top metal layer is 40 nm.

[0014] Preferably, the square groove is located in the middle of the top metal layer.

[0015] A method for preparing a Fano resonance color filter comprises the following steps:

[0016] Step 1: Depositing a silicon dielectric layer on the metal substrate layer using a plasma enhanced chemical vapor deposition process;

[0017] Step 2: depositing an intermediate metal layer on the silicon dielectric layer by magnetron sputtering;

[0018] Step 3, depositing a vanadium dioxide layer on the intermediate metal layer by magnetron sputtering;

[0019] Step 4, depositing a top metal layer on the vanadium dioxide layer by magnetron sputtering;

[0020] Step 5: Spin-coat photoresist, and use a photolithography process to expose, photolithograph, and etch the top metal layer to obtain periodic square grooves.

[0021] Preferably, the thin film deposition process is a plasma enhanced chemical vapor deposition process.

[0022] Compared with the prior art, the advantages of the present invention are:

[0023] 1. The color can be modulated dynamically.

[0024] The vanadium dioxide film is a semiconductor when the temperature is below the phase transition temperature and is a metal when the temperature is above the phase transition temperature. The refractive index of the material in the visible light band (400nm-800nm) changes significantly before and after the phase transition.

[0025] Using this principle, the vanadium dioxide layer can be electrically heated or cooled to change the refractive index of the material, causing the resonance of the upper broadband filter (a structure composed of the top metal layer 1, the vanadium dioxide layer 2 and the middle metal layer 3) to change, thereby tuning the electric field coupling between the upper broadband filter and the underlying narrowband filter (a structure composed of the silicon dielectric layer 4 and the metal base layer 5) to produce Fano resonance, thereby realizing the function of a dynamic color filter.

[0026] 2. The color response (color purity and brightness) of the filter is good. Specifically: Fano resonance can enhance the color response of the color filter and produce structural colors with high saturation and high brightness.

[0027] 3. The present invention is easy to implement, avoids the moving parts of a mechanical switch, has good dynamic color rendering ability and color response, and can be widely used in optical instruments, color display, anti-counterfeiting and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Schematic diagram of the Fano resonance color filter structure;

[0029] Figure 2 for Figure 1 A top view of

[0030] Figure 3 is the reflection spectrum of the device in the range of 400nm-800nm ​​when vanadium dioxide is in the dielectric state and the metallic state;

[0031] Figure 4 yes Figure 3 The color coordinates corresponding to the reflected spectrum shown are located on the CIE 1931 chromaticity diagram;

[0032] Figure 5 A cross-sectional view of a conductive element.

[0033] Among them, 1-top metal layer, 2-vanadium dioxide layer, 3-middle metal layer, 4-silicon dielectric layer, 5-metal base layer, 6-conductive element, and 61-opening. DETAILED DESCRIPTION

[0034] The Fano resonant color filter and its preparation method of the present invention will be described in more detail below in conjunction with the schematic diagram, wherein the preferred embodiment of the present invention is shown, and it should be understood that those skilled in the art can modify the present invention described herein, and still achieve the advantageous effects of the present invention. Therefore, the following description should be understood as being widely known to those skilled in the art, and not as a limitation of the present invention.

[0035] like Figure 1 As shown, a Fano resonance color filter comprises:

[0036] The metal substrate 5, the silicon dielectric layer 4, the middle metal layer 3, the vanadium dioxide layer 2 and the top metal layer 1 are arranged in sequence from bottom to top;

[0037] Wherein, periodic square grooves are etched on the top metal layer 1 , and the depth of the square grooves is equal to the thickness of the top metal layer 1 . The square grooves are located in the middle of the top metal layer 1 .

[0038] In this embodiment, the metal substrate 5 , the middle metal layer 3 , and the top metal layer 1 are all Ag layers.

[0039] The thickness of the silicon dielectric layer 4 is 50 nm, the thickness of the intermediate metal layer 3 is 40 nm, the thickness of the vanadium dioxide layer 2 is 40 nm, and the thickness of the top metal layer 1 is 40 nm.

[0040] The side length w of the square groove is 180nm, the groove depth d is 40nm, and the period p of the device in both directions is 200nm. Figure 2 shown.

[0041] The refractive index of vanadium dioxide in the visible light band is adjusted by adjusting the temperature of the vanadium dioxide layer 2 .

[0042] Specifically, the temperature of the vanadium dioxide layer 2 can be changed by heating on a heating platform, placing the device on the heating platform, or by electrical heating, such as Figure 5 , which is a top view of the conductive element 6 .

[0043] The conductive element 6 is a frame structure with an opening 61 formed on its inner wall. The conductive element 6 is conductive.

[0044] The vanadium dioxide layer 2 is embedded in the opening 61 .

[0045] When the conductive element 6 is energized, the vanadium dioxide layer 2 is heated.

[0046] When the conductive element 6 is de-energized, the vanadium dioxide layer 2 is cooled.

[0047] This color filter utilizes the Fano resonance and phase change characteristics of vanadium dioxide, enabling the device to maintain good color response and dynamic color rendering capabilities, successfully realizing the function of a dynamic color filter.

[0048] Specifically, the color filter couples a broadband nanocavity with a narrowband Fabry-Perot nanocavity, and the resonant interference between the nanocavities can produce an asymmetric Fano resonance line shape.

[0049] The Fano resonance line shape was discovered by Fano in 1935 and was first observed in the absorption spectrum of noble gases. Its microscopic mechanism is the interference effect between different transition paths during the transition of atoms from the initial state to the final state: when one transition path exhibits a narrow spectrum resonance (corresponding to the transition from discrete state to discrete state), and the other transition path exhibits a wide spectrum resonance (corresponding to the transition from discrete state to continuous state), the interference between the two transition paths will cause the overall absorption spectrum of the system to exhibit an asymmetric Fano resonance line shape.

[0050] In this embodiment, the color filter can generate Fano resonance by controlling the phase change of vanadium dioxide, that is, by heating or cooling the vanadium dioxide layer.

[0051] Fano resonance can achieve dynamic color modulation and good color response.

[0052] The method for preparing the Fano resonance color filter comprises the following steps:

[0053] Step 1: Deposit a uniform silicon dielectric layer 4 with a thickness of 50 nm on the Ag substrate layer using a plasma enhanced chemical vapor deposition process;

[0054] Step 2: depositing a uniform Ag layer with a thickness of 40 nm on the silicon dielectric layer 4 by magnetron sputtering;

[0055] Step 3, depositing a uniform vanadium dioxide layer 2 with a thickness of 40 nm on the middle Ag layer by magnetron sputtering;

[0056] Step 4: depositing a uniform Ag layer with a thickness of 40 nm on the vanadium dioxide layer 2 by magnetron sputtering;

[0057] Step 5: Etch a square groove on the top Ag layer.

[0058] Specifically: using a spin coater, 40 nm of electron beam glue is evenly coated on the upper surface of the top Ag layer, and then a photolithography machine is used for photolithography exposure and an ion beam etching device is used for etching to form a periodic square groove structure.

[0059] Figure 3 It is the reflection spectrum of the device in the range of 400nm-800nm ​​when vanadium dioxide is in the dielectric state and the metallic state.

[0060] When vanadium dioxide is in a dielectric state, the peak maximum reflectivity can reach 43%, the short-wave spectral reflection of the device is more significant, and the Fano resonance intensity at 695nm is the strongest.

[0061] When heated, vanadium dioxide changes into a metallic state, the short-wave spectral reflection of the device is suppressed, the long-wave spectral reflectivity increases significantly, and the Fano resonance at 688nm is significantly enhanced, with the peak reflectivity caused by its resonance peak reaching 59%.

[0062] Depend on Figure 3 It is known that Fano resonance is generated in the color filter by heating or cooling the vanadium dioxide layer through electrical conduction.

[0063] Figure 4 yes Figure 3 The reflected spectra shown correspond to the positions of the color coordinates on the CIE 1931 chromaticity diagram.

[0064] Figure 4 In the figure, x represents CIE x.

[0065] When vanadium dioxide is in a dielectric state, the color coordinates are in the blue region; when heated, vanadium dioxide changes to a metallic state, and the color coordinates change to the red region. The color difference ΔE caused by the phase change of vanadium dioxide 2000 It can reach 36.7.

[0066] Depend on Figure 4 It is known that the color response (color purity and brightness) of this color filter is good.

[0067] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any technician in the relevant technical field, without departing from the scope of the technical solution of the present invention, makes any form of equivalent replacement or modification to the technical solution and technical content disclosed in the present invention, which does not depart from the content of the technical solution of the present invention and still falls within the protection scope of the present invention.

Claims

1. A Fano resonance color filter, characterized in that: include: A metal base layer, a silicon dielectric layer, an intermediate metal layer, a vanadium dioxide layer and a top metal layer are sequentially arranged from bottom to top; Wherein, a square groove is etched on the top metal layer, and the depth of the square groove is equal to the thickness of the top metal layer.

2. The Fano resonance color filter according to claim 1, characterized in that The refractive index of vanadium dioxide in the visible light band is adjusted by adjusting the temperature of the vanadium dioxide layer.

3. The Fano resonance color filter according to claim 1, characterized in that: The metal base layer is an Ag layer.

4. The Fano resonance color filter according to claim 3, characterized in that: The intermediate metal layer is an Ag layer.

5. The Fano resonance color filter according to claim 4, characterized in that: The top metal layer is an Ag layer.

6. The Fano resonance color filter according to claim 5, characterized in that: The thickness of the silicon dielectric layer is 50 nm, the thickness of the middle metal layer is 40 nm, the thickness of the vanadium dioxide layer is 40 nm, and the thickness of the top metal layer is 40 nm.

7. The Fano resonance color filter according to claim 6, characterized in that: The square groove is located in the middle of the top metal layer.

8. A method for preparing a Fano resonance color filter according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step 1: Depositing a silicon dielectric layer on the metal substrate layer using a plasma enhanced chemical vapor deposition process; Step 2: depositing an intermediate metal layer on the silicon dielectric layer by magnetron sputtering; Step 3, depositing a vanadium dioxide layer on the intermediate metal layer by magnetron sputtering; Step 4, depositing a top metal layer on the vanadium dioxide layer by magnetron sputtering; Step 5: Spin-coat photoresist, and use a photolithography process to expose, photolithograph, and etch the top metal layer to obtain periodic square grooves.

Citation Information

Cited By

  • Colorful radiation refrigeration film based on fano resonance and preparation method thereof

    CN119805640A