Method for modifying internal interface of fiber-based polymer electrolyte by high-energy electron beam irradiation
The interface structure of the fiber-based polymer electrolyte is improved through high-energy electron beam irradiation technology, which solves the problem of loose molecular chain arrangement, improves the migration efficiency of lithium ions, and improves the overall performance and safety of the electrolyte.
Patent Information
- Application Number
- CN202410802455.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-18
AI Technical Summary
The molecular chains of existing fiber-based polymer electrolytes are loosely arranged and irregular, which hinders the migration of lithium ions and affects the overall conductive performance.
High-energy electron beam irradiation technology is used to pretreat and compound fiber-based polymers. By promoting atomic bonding of polymer chain segments in the amorphous region, the electrolyte interface structure is improved and the movement efficiency of lithium ions is increased. Specific steps include pretreatment of biomass materials, dewaxing treatment, removal of hemicellulose and lignin, hydrolysis treatment and high-energy electron beam irradiation, and finally compounding with polymer solid electrolyte matrix material.
Significantly improves the migration ability of lithium ions, improves the overall performance and safety of the electrolyte, and reduces battery safety hazards.
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of chemical energy storage and relates to a novel method for modifying the internal interface of fiber-based polymer electrolyte by high-energy electron beam irradiation. This innovative method aims to promote the development of solid-state battery technology by reducing costs and improving material performance to meet the requirements of modern energy storage systems for high efficiency, safety, and economy. Background Art
[0002] The continuous progress of energy technology is a key factor in promoting the development of human society. With the continuous growth of energy demand, it is particularly urgent to develop new energy storage technologies that are efficient, environmentally friendly and economical. In order to reduce dependence on fossil energy and reduce carbon emissions, researchers are committed to studying new energy storage technologies. Among the many energy storage technologies, lithium metal batteries have become the focus of research due to their excellent rate performance and long cycle life. This battery has wide application potential in the field of secondary batteries.
[0003] However, there are some safety hazards in the current use of lithium metal batteries. Most lithium metal batteries use organic solvents as electrolytes. These solvents are not only flammable, but may also corrode equipment, increasing safety risks. Researchers such as Guo Shumin explored the potential of using wood powder as a lithium-ion battery separator material. In lithium metal batteries, the commonly used electrolyte is an organic solvent, and this choice brings the risk of flammability and corrosion. In addition, during the charge and discharge cycle of the battery, lithium dendrites may form at the negative electrode. These dendrites may pierce the diaphragm, causing the battery to short-circuit, causing serious safety hazards. In order to solve these problems, polymer solid electrolytes have been proposed as a substitute for liquid electrolytes. The use of solid electrolytes fundamentally eliminates the flammability and leakage risks of organic solvents, greatly improving the safety of batteries.
[0004] In addition, the plasticity of polymer materials helps stabilize the electrode structure, further enhancing the cycle stability and service life of the battery. Therefore, as an emerging energy storage technology, polymer solid-state batteries not only have higher safety performance, but also show great potential in practical application, becoming one of the most promising research directions in future energy storage systems. As the technology continues to mature, polymer solid-state batteries are expected to provide strong support for the sustainable development of society.
[0005] The room temperature conductivity of polyethylene oxide (PEO) is low, about 10 -6 Up to 10 -7 S cm -1This property is mainly attributed to its high crystallinity. In this type of polymer, the migration of lithium ions mainly occurs in the amorphous region, while a large part of the complex formed by oxygen atoms and lithium salts is contained in the crystalline region. Due to the restricted movement of polymer chain segments in the crystalline region, the dissociation and migration of lithium ions are hindered, thus affecting the overall conductive properties.
[0006] Researchers have carried out a series of work in the field of cellulose irradiation processing and have made some progress. Chinese patent CN 104294693B discloses a method for preparing micro-nano cellulose. Natural cellulose is first irradiated with a high-energy electron beam to destroy its internal structure, and then the irradiated cellulose materials are coarsely crushed by mechanical dry method, and then finely crushed by water milling, and finally micro-nano cellulose can be obtained. This patent first pre-treats cellulose mechanically and chemically, and then further treats nanocellulose using high-energy irradiation technology to optimize the orientation difference of the molecular chains in its amorphous region. This process improves the structure of nanocellulose, so that it can better exert its performance in the process of composite film formation with polymer solid electrolyte matrix materials.
[0007] Chinese patent CN 108677581 A discloses a method for preparing low-polymerization and low-crystallinity cellulose by high-energy electron beam irradiation. The method uses an electron accelerator device to irradiate cellulose at a suitable dose, effectively destroying hydrogen bonds in cellulose molecules, thereby reducing the crystallinity and polymerization degree of the cellulose molecules at the same time, and increasing the dissolution activity of cellulose.
[0008] Chinese patent CN 114106378 A discloses a method for preparing a natural cellulose-based polymer electrolyte, wherein a natural cellulose polymer membrane is prepared by tape casting, pouring, coating, papermaking, hot pressing, screen printing, freeze drying, electrostatic spinning, phase inversion, impregnation, foaming, and Bellcore method. Although the preparation of a diaphragm with a uniform microporous structure can significantly improve the ionic conductivity of electrochemical energy storage devices such as batteries, the process is complicated and involves multiple process steps, which is not conducive to industrial production.
[0009] Nanocellulose is mainly composed of D-pyranose glucose rings connected by β-1,4 glycosidic bonds. In the amorphous region, the orientation of the molecular chains varies greatly, resulting in loose and irregular molecular arrangement and weak intermolecular binding forces. Atomic bonding that is conducive to ion transport cannot occur during the composite process with the polymer electrolyte. High-energy electron beam irradiation can efficiently and in situ promote the reaction, thereby optimizing the polymer electrolyte interface structure and performance. Summary of the invention
[0010] The purpose of the present invention is to overcome the problems of loose and irregular arrangement of molecular chains, large orientation differences, and weakened intermolecular bonding forces in the prior art, and to provide a method for modifying the internal interface of fiber-based polymer electrolytes by high-energy electron beam irradiation.
[0011] The present invention has the following beneficial effects:
[0012] The present invention adopts high-energy electron beam irradiation technology to specifically address the problem of low ion conductivity in solid electrolytes by improving the interface structure of polymer electrolytes. This technology can promote atomic bonding between polymer segments in amorphous regions, thereby facilitating the movement of lithium ions and improving the overall performance of the electrolyte.
[0013] The present invention provides a method for modifying the internal interface of a fiber-based polymer electrolyte by irradiating a high-energy electron beam. The method needs to follow the following detailed steps:
[0014] (1) Biomass material pretreatment: washing with deionized water and drying for degumming;
[0015] (2) placing the dried biomass material in a Soxhlet extractor and dewaxing it with a benzene-alcohol mixture (volume ratio 1.5:1) for 3-4 hours at a temperature of 130-140° C., then washing it with anhydrous ethanol and drying it;
[0016] (3) The dewaxed biomass material is placed in a 0.8 w / v.% sodium hypochlorite solution, glacial acetic acid is added to maintain acidic conditions (pH is controlled at 3-6), heated in a water bath at 60-70°C for 4-6 hours, and then washed with deionized water and dried;
[0017] (4) The material was placed in a 14-16 w / v.% potassium hydroxide solution, heated in a water bath at 60-70°C for 7-8 hours, washed with deionized water and dried to remove hemicellulose and lignin;
[0018] (5) heating and stirring the dried fiber in 45% 98% analytical grade sulfuric acid for 5-7 hours;
[0019] (6) centrifuging the sulfuric acid hydrolyzed solution to neutralize the precipitate, and repeating the centrifugation step until the solution is neutral;
[0020] (7) placing the prepared nanocellulose under a 1-3 MeV high energy electron beam irradiation source for irradiation. The irradiation environment is normal temperature and pressure, the irradiation current is 7 mA, the irradiation dose is 1 kGy to 100 kGy, and the irradiation time is 15 to 100 minutes;
[0021] (8) The nanocellulose irradiated by high-energy electron beam is composited with a polymer solid electrolyte matrix material (such as PEO, PAN, PVDF, PVDF-HFP, etc.) to form a film. DETAILED DESCRIPTION
[0022] The method for improving the fiber-based polymer electrolyte interface based on high-energy electron beam irradiation provided by the present invention is described in detail below in conjunction with specific embodiments.
[0023] Embodiment 1:
[0024] The pretreated banana peel was placed in a Soxhlet extractor and extracted with a benzene alcohol mixture with a volume ratio of 1.5:1 at 130°C for 4 hours. The dried banana peel was placed in a 0.8w / v.% sodium hypochlorite solution with a bath ratio of 1:50, pH controlled at 4, and heated in a water bath at 90°C for 1 hour. After heating, it was repeatedly washed with deionized water and dried at room temperature. After treatment, it was placed in a 14w / v.% potassium hydroxide solution, heated in a water bath at 60°C for 7 hours, and then repeatedly washed with deionized water and dried at room temperature. The dried fiber was placed in 45% sulfuric acid with a bath ratio of 1:45, and heated and stirred on a 45°C magnetic heating stirrer for 5 hours. After sulfuric acid hydrolysis, it was repeatedly centrifuged until the solution was neutral. High-energy electron beam irradiation treatment was carried out at room temperature and pressure, with an absorbed irradiation dose of 10kGy and irradiation for 100 minutes. After irradiation, the sample was composited with PEO and cast into a film at a volume ratio of 1:10. The composite process was magnetically stirred for 4 hours and dried at 30°C for 24 hours to obtain a banana peel / PEO composite material.
[0025] Embodiment 2:
[0026] The pretreated rice straw was placed in a Soxhlet extractor and extracted with a benzene alcohol mixture with a volume ratio of 1.5:1 at 135°C for 3.5 hours. The dried rice straw was placed in a 0.8w / v.% sodium hypochlorite solution with a bath ratio of 1:50, pH controlled at 5, and heated in a water bath at 65°C for 2 hours. After heating, it was repeatedly washed with deionized water and dried at room temperature. After treatment, it was placed in a 15w / v.% potassium hydroxide solution, heated in a water bath at 50°C for 7.5 hours, and then repeatedly washed with deionized water and dried at room temperature. The dried fiber was placed in 45% sulfuric acid with a bath ratio of 1:45, and heated and stirred on a 45°C magnetic heating stirrer for 6 hours. After sulfuric acid hydrolysis, it was repeatedly centrifuged until the solution was neutral. High-energy electron beam irradiation treatment was carried out at room temperature and pressure, with an absorbed irradiation dose of 50kGy and irradiation for 40 minutes. After irradiation, the sample was composited with PAN to form a film with a volume ratio of 1:100. The magnetic stirring time during the composite process was 16 hours and dried at 50°C for 18 hours to obtain the straw / PAN composite material.
[0027] Embodiment 3:
[0028] The pretreated wheat straw was placed in a Soxhlet extractor and extracted with a benzene alcohol mixture with a volume ratio of 1.5:1 at 140°C for 3 hours. The dried wheat straw was placed in a 0.8w / v.% sodium hypochlorite solution with a bath ratio of 1:50, pH controlled at 6, and heated in a water bath at 70°C for 3 hours. After heating, it was repeatedly washed with deionized water and dried at room temperature. After treatment, it was placed in a 16w / v.% potassium hydroxide solution, heated in a water bath at 40°C for 8 hours, and then repeatedly washed with deionized water and dried at room temperature. The dried fiber was placed in 45% sulfuric acid with a bath ratio of 1:45, and heated and stirred on a 45°C magnetic heating stirrer for 7 hours. After sulfuric acid hydrolysis, it was repeatedly centrifuged until the solution was neutral. High-energy electron beam irradiation treatment was carried out at room temperature and pressure, with an irradiation absorption dose of 100kGy and irradiation for 15 minutes. After irradiation, the sample was composited with PVDF and cast into a film at a volume ratio of 1:500. The composite process was magnetically stirred for 24 hours and dried at 80°C for 6 hours to obtain a straw / PVDF composite material.
Claims
1. A method for modifying the internal interface of a fiber-based polymer electrolyte by irradiating with a high-energy electron beam, characterized in that Optimizing the polymer electrolyte interface structure, especially for polymers that affect the movement of lithium ions in amorphous region segments, using high-energy electron beam irradiation to efficiently and in situ promote the occurrence of reactions to produce atomic bonding that is beneficial to ion transport, thereby solving the problem of low ion conductivity of solid electrolytes and optimizing their structure and performance. The method comprises the following steps: (1) pretreating cellulose-based materials; (2) placing the prepared nanocellulose under a high-energy electron beam irradiation source for irradiation; (3) The nanocellulose irradiated by high-energy electron beam is composited with a polymer solid electrolyte matrix material to form a film.
2. The method of modifying the internal interface of a fiber-based polymer electrolyte by high-energy electron beam irradiation according to claim 1, characterized in that In the step (2), the current of the high energy electron beam is 7 mA, and the irradiation time is 15 to 100 minutes.
3. The method of modifying the internal interface of a fiber-based polymer electrolyte by high-energy electron beam irradiation according to claim 1, characterized in that The absorbed dose of high energy electron beam irradiation in step (2) is 1 kGy to 100 kGy.
4. The method for improving the fiber-based polymer electrolyte interface by high-energy electron beam irradiation according to claim 1, characterized in that The energy of the high energy electron irradiation in step (2) is 1 to 3 MeV.
5. The method of modifying the internal interface of a fiber-based polymer electrolyte by high-energy electron beam irradiation according to claim 1, characterized in that The ionic conductivity of the composite film formed by the cellulose-based material and the polymer solid electrolyte matrix material after high-energy electron beam irradiation in step (3) is 10 -2 ~10 -6 S cm -1 .
6. The method of modifying the internal interface of a fiber-based polymer electrolyte by high-energy electron beam irradiation according to claim 1, characterized in that In the step (3), the volume ratio of the cellulose-based material to the polymer solid electrolyte matrix material for composite film formation is 1:10 to 1:1000.
7. The method of modifying the internal interface of a fiber-based polymer electrolyte by high-energy electron beam irradiation according to claim 1, characterized in that In the step (3), the thickness of the diaphragm formed by the composite film of the cellulose-based material and the polymer solid electrolyte matrix material is 20 to 600 microns.
8. The method of modifying the internal interface of a fiber-based polymer electrolyte by high-energy electron beam irradiation according to claim 1, characterized in that In the step (3), the cellulose-based material and the polymer solid electrolyte matrix material are composited into a film and dried, the magnetic stirring time of the composite process is controlled to be 4 to 24 hours, the drying temperature range is 30 to 80° C., and the drying time is controlled to be 4 to 24 hours.