Printed circuit board manufacturing method and circuit board
By carrying out steps such as ultra-roughening pre-treatment, drying, baking, laminating, exposure and development during the production process of PCB printed circuit boards, the problem of board warping and bending is solved, the defective scrap rate is reduced, and the product quality is improved. reliability.
Patent Information
- Application Number
- CN202410782291.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-18
AI Technical Summary
In the production process of PCB printed circuit boards, the design leads to board warping and bending problems, resulting in a high defective scrap rate. In particular, the high residual copper rate on the back of the SIP carrier board affects the reliability of the product.
By performing ultra-roughening pre-treatment, drying treatment, baking, pre-alignment film application, vacuum leveling, exposure treatment and development and solidification on the circuit board, the shape and solder mask pattern of the circuit board are adjusted to balance the top and bottom surfaces. Expansion and contraction deformation, reducing the risk of board warping and bending.
It effectively reduces the defective scrap rate, improves product reliability, reduces the residual copper rate, reduces board warping and bending problems, and improves the economic benefits of production.
Smart Images

Figure CN118804477A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of printed circuit boards, and in particular to a printed circuit board manufacturing method and a circuit board. Background Art
[0002] In the PCB industry, SIP substrates are mostly used on ICS packaging substrates, and are mainly used to bond high-end chips and chipsets, and are used in the design of telecommunications network signal module groups. Therefore, they are often designed as single independent small pads on one side (used for welding BGA / chips and other welding electronic components), and the back side is mainly designed to heat dissipation or welding battery modules as the main heat dissipation electrical components. Considering the area and effectiveness of heat dissipation, the welding pad is generally designed as a large round pad or a long rectangular pad, which will result in a single unit with a top surface residual copper rate of only 15-25%, while the back side of the SIP substrate has a residual copper rate of up to 50-70%. In the process of PCB production, this similar design, ignoring the influence of factors such as the expansion and contraction of the board itself, is very prone to board warping, expansion and contraction. Even in the process of online welding and reflow soldering at the client, warping and deformation occur, and the electronic components and SIP substrates are poorly welded, resulting in scrapping, and also affecting the reliability of the product. According to comprehensive industry data, the current scrap rate is as high as 10-20%. Due to the uniqueness of its design at the source, it poses challenges to the SIP substrate production process. Summary of the invention
[0003] In order to solve the above technical problems, the embodiments of the present invention provide a printed circuit board manufacturing method and a circuit board, which solve the problem of board warping and bending occurring during board manufacturing and reduce the defect scrap rate.
[0004] A first aspect of an embodiment of the present invention provides a method for manufacturing a printed circuit board, the method comprising:
[0005] Drying the circuit board after the super-roughening pre-treatment to obtain a dried circuit board, and baking the dried circuit board to obtain a baked circuit board;
[0006] After pre-aligning the dried circuit board, laminating the top surface of the dried circuit board with a solder resist dry film of a first thickness, laminating the bottom surface of the dried circuit board with a solder resist dry film of a second thickness, vacuuming and leveling the laminating circuit board to obtain a laminated circuit board, wherein the first thickness is greater than the second thickness;
[0007] Expose the laminated circuit board so that the intervals between the units in the laminated circuit board are adjusted to a preset shape to obtain an exposed circuit board;
[0008] The exposed circuit board is developed so that the solder resist pattern in the unexposed area of the exposed circuit board is developed, and the developed circuit board is cured and baked to obtain a final circuit board.
[0009] In a possible implementation of the first aspect, the ultra-roughening pre-treatment includes:
[0010] After degreasing and cleaning the circuit board, the circuit board is treated with an organic acid micro-etching solution with a micro-etching amount in the range of 1.3um to 1.4um;
[0011] The processed circuit boards are pickled and washed with water for multiple times.
[0012] In a possible implementation of the first aspect, baking the dried circuit board to obtain a baked circuit board includes:
[0013] The circuit board is dried using three upper and lower air knives to obtain a dried circuit board.
[0014] In a possible implementation of the first aspect, baking the dried circuit board to obtain a baked circuit board includes:
[0015] The dried circuit board is dried using a vertical furnace drying plate to obtain a dried circuit board.
[0016] In a possible implementation manner of the first aspect, after obtaining the laminated circuit board, the method further includes:
[0017] Insert the laminated circuit board into the rack and use tape to fix the left and right sides of the laminated circuit board.
[0018] In a possible implementation manner of the first aspect, performing an exposure process on the laminated circuit board so as to adjust the intervals between the units in the laminated circuit board to a preset shape includes:
[0019] The exposure energy is set to 280-300mj / cm2, the exposure scale is set to 7-9 levels, and the laminated circuit board is exposed so that the interval area between each unit in the laminated circuit board is adjusted to a window design.
[0020] In a possible implementation manner of the first aspect, before developing the exposed circuit board, the method further includes:
[0021] Place the exposed circuit board in a box and use a sulfur-free paper separator to separate the exposed circuit board from the box.
[0022] In a possible implementation of the first aspect, developing the exposed circuit board so as to develop the solder resist pattern in the unexposed area of the exposed circuit board includes:
[0023] Place the top surface of the exposed circuit board facing upward, remove the protective film on the solder resist dry film in the exposed circuit board, and immerse the exposed circuit board in K2CO3 or NaCO3 with a concentration of 8-9g / L to develop the solder resist pattern in the unexposed area, wherein the immersion time is 40s to 50s.
[0024] In a possible implementation of the first aspect, curing and baking the developed circuit board includes:
[0025] After the first UV curing of the developed circuit board, the circuit board after the first curing is post-baked using a vertical furnace baking plate, wherein the UV curing energy of the first UV curing is 500mj / cm2~600mj / cm2, and the temperature is 80 degrees~120 degrees;
[0026] The post-baked circuit board is subjected to a second UV curing, wherein the UV curing energy of the second UV curing is 500mj / cm2 to 800mj / cm2 and the temperature is 80 degrees to 120 degrees.
[0027] A second aspect of an embodiment of the present invention provides a circuit board, which is obtained by adopting the above-mentioned printed circuit board manufacturing method.
[0028] The printed circuit board manufacturing method provided by the embodiment of the present invention comprises the following steps: drying the circuit board after the ultra-roughening pre-treatment to obtain the dried circuit board, baking the dried circuit board to obtain the baked circuit board, pre-aligning the dried circuit board, applying a solder resist dry film of a first thickness to the top surface of the dried circuit board, applying a solder resist dry film of a second thickness to the bottom surface of the dried circuit board, vacuuming and leveling the film-applied circuit board to obtain the laminated circuit board, wherein the first thickness is greater than the second thickness, exposing the laminated circuit board to adjust the area between the units in the laminated circuit board to a preset shape to obtain the exposed circuit board, developing the exposed circuit board to develop the solder resist pattern in the unexposed area of the exposed circuit board, and curing and baking the developed circuit board to obtain the final circuit board. The above method solves the problem of board warping and bending during board manufacturing, and reduces the defect scrap rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 : A schematic diagram of a process flow of a printed circuit board manufacturing method according to an embodiment of the present invention;
[0030] Figure 2 : A schematic diagram of a circuit board with water vapor in one embodiment of the printed circuit board manufacturing method provided by the present invention;
[0031] Figure 3 : A schematic diagram of a kilo-layer rack according to an embodiment of a printed circuit board manufacturing method provided by the present invention;
[0032] Figure 4 : A schematic diagram of a circuit board after being heated according to an embodiment of the printed circuit board manufacturing method provided by the present invention;
[0033] Figure 5 : A schematic diagram of a rack device for an embodiment of a printed circuit board manufacturing method provided by the present invention;
[0034] Figure 6 : A design diagram of a top surface window opening of layer L4 of a printed circuit board before optimization according to an embodiment of a printed circuit board manufacturing method provided by the present invention;
[0035] Figure 7 : A graphical design diagram of a bot surface window opening on the L4 layer of a printed circuit board before optimization according to an embodiment of the printed circuit board manufacturing method provided by the present invention;
[0036] Figure 8 : The original graphic design drawings of each layer of the printed circuit board according to one embodiment of the printed circuit board manufacturing method provided by the present invention;
[0037] Fig. 9 : A schematic diagram of circuit board warping in one embodiment of the printed circuit board manufacturing method provided by the present invention;
[0038] Fig.10 : A schematic diagram of circuit board bending according to an embodiment of the printed circuit board manufacturing method provided by the present invention;
[0039] Fig.11 : A schematic diagram of the design of the L4 surface of a circuit board with a high residual copper rate before optimization according to an embodiment of the printed circuit board manufacturing method provided by the present invention;
[0040] Fig.12 : A schematic diagram of the design of the L4 surface of the circuit board after optimization according to an embodiment of the printed circuit board manufacturing method provided by the present invention. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] At present, in the PCB industry, it is often designed that one side is mostly a single independent small Pad (for welding BGA / chips and other welding electronic components), and the other back side is mainly designed to play a heat dissipation purpose or weld the heat dissipation electrical components with battery modules as the main body. Considering the area and effectiveness of heat dissipation, the welding Pad is generally designed as a large round Pad or a long rectangular Pad, which will result in a single unit with a top surface residual copper rate of only 15-25%, while the back side residual copper rate of the SIP carrier is as high as 50-70%. In the process of PCB production, this similar design, ignoring the influence of factors such as the expansion and contraction of the simple board itself, is very prone to board warping, expansion and contraction.
[0043] Among them, ICS means the questions that are fed back by the board factory before production after the PCB data is sent to the board factory after communication and confirmation with customers and engineering. PCB means printed circuit board, also known as printed circuit board, which is an important electronic component, a support for electronic components, and a carrier for electrical connection of electronic components. SIP means single in-line package, which is a packaging form of components. The packaged chip is also easier to install and transport. The quality of packaging technology directly affects the performance of the chip itself and the design and manufacture of the PCB (printed circuit board) connected to it. Pad means solder pad, which refers to the small metallized area on the board surface, used as a contact point with component pins or other interconnect elements. Unit refers to the unit graphic in the board surface.
[0044] Based on this, the embodiments of the present application provide a printed circuit board manufacturing method and a circuit board, which aim to solve the problem of board warping and bending in the manufacturing process of the circuit board, thereby reducing the defect scrap rate.
[0045] Please refer to Figure 1 , which is a flow chart of an embodiment of a printed circuit board manufacturing method provided by an embodiment of the present invention, including steps S101 to S104, each step is specifically as follows:
[0046] S101, drying the circuit board after the super-roughening pre-treatment to obtain a dried circuit board, and baking the dried circuit board to obtain a baked circuit board.
[0047] In this embodiment, after the circuit board is subjected to the ultra-roughening pre-treatment, it is dried, and then the dried circuit board is baked to obtain the baked circuit board. Because the SIP board design has NPTH holes and PTH holes, the baking is mainly to dry the water vapor on the board surface. A vertical furnace baking plate is added after the drying section to provide a medium and low temperature baking plate, and the time from drying to film pasting is controlled. The vacuum film pressing process is carried out when the board surface is heated to release stress. At the same time, after testing and research, adding a baking plate can effectively reduce defects such as vacuum film pressing bubbles, such as Figure 2 As shown, Figure 2 For circuit boards with moisture present, the defect rate dropped from 0.3% to 0.01%.
[0048] In some embodiments, the “performing ultra-roughening pre-treatment” in step S101 includes but is not limited to the following steps:
[0049] After degreasing and cleaning the circuit board, the circuit board is treated with an organic acid micro-etching solution with a micro-etching amount in the range of 1.3um to 1.4um;
[0050] The processed circuit boards are pickled and washed with water for multiple times.
[0051] Specifically, the specific process of the ultra-roughening pre-treatment drying section is: after degreasing the circuit board, it is washed with water, and then the circuit board is treated with an organic acid micro-etching solution with a micro-etching amount in the range of 1.3um to 1.4um, the circuit board is washed with water and acid again, and then washed with water again, and then after antioxidant treatment, the circuit board is dried.
[0052] In some embodiments, step S101 of "baking the dried circuit board to obtain a baked circuit board" includes but is not limited to the following steps:
[0053] The circuit board is dried using three upper and lower air knives to obtain a dried circuit board.
[0054] Specifically, the specific process of drying the circuit board is: using three upper and lower air knives to blow and dry the circuit board to obtain a dried circuit board. The drying temperature is maintained at 80 degrees and the drying time is 15 seconds to 20 seconds.
[0055] In some embodiments, step S101 of "drying the circuit board to obtain a dried circuit board" includes but is not limited to the following steps:
[0056] The dried circuit board is dried using a vertical furnace drying plate to obtain a dried circuit board.
[0057] Specifically, the dried circuit board is baked by placing a vertical furnace baking plate under the lycra rack, the baking temperature is 80 degrees, and the baking time is 30 minutes. In addition, the lycra rack used in the baking process, Figure 3 It is a Thousand Layer Shelf, the grid is 50m*50mm, the grid is as dense as possible, the overall length*width is 650*550mm, the board surface is laid flat, which is more conducive to releasing thermal stress on the board surface.
[0058] S102, after pre-aligning the dried circuit board, laminating the top surface of the dried circuit board with a first thickness of solder resist dry film, laminating the bottom surface of the dried circuit board with a second thickness of solder resist dry film, evacuating and leveling the film-laminated circuit board to obtain a laminated circuit board, wherein the first thickness is greater than the second thickness.
[0059] In this embodiment, after the dried circuit board is pre-aligned, a solder resist dry film of a first thickness is applied to the top surface of the dried circuit board, and a solder resist dry film of a second thickness is applied to the bottom surface of the dried circuit board. The film-applied circuit board is vacuumed, leveled, film-teared, and conveyed to obtain a laminated circuit board, wherein the first thickness is greater than the second thickness.
[0060] If the first thickness and the second thickness of the solder mask dry film are the same thickness, it is easy to deform when heated. Specifically, if the thickness of both sides is 18um or 22um dry film, deformation will be found when heated. Figure 4 As shown, the circuit board will bend upward.
[0061] As an example of this embodiment, a solder resist dry film with a thickness of 23um is used for the Top surface (low residual copper rate) of the circuit board after drying, and a solder resist dry film with a thickness of 18um is used for the Bot surface (high residual copper rate). Due to the difference in residual copper rate, the material changes when heated, the L1 surface expands and contracts slowly, and the L4 surface expands and contracts rapidly, causing the board surface to bend toward the L1 surface and open upward. On the L1 surface, because the copper pad is smaller, the ink in the dry film will flow to the surroundings after vacuum pressing, causing L1 to be thinner than the L4 surface, aggravating the bending deformation of the board surface. Therefore, a thicker dry film is needed on the L1 surface to balance the ink thickness on both sides, and the thicker L1 ink suppresses the bending of the L1 surface, thereby achieving a balance between the expansion and contraction of both sides.
[0062] It should be noted that the top surface refers to the Top surface, the side with a low residual copper rate, and the bottom surface refers to the Bot surface, the side with a high residual copper rate.
[0063] In some embodiments, "after obtaining the laminated circuit board" in step S102 includes but is not limited to the following steps:
[0064] Insert the laminated circuit board into the rack and use tape to fix the left and right sides of the laminated circuit board.
[0065] In this embodiment, after the circuit board is filmed, the ink is not exposed and the ink surface is easy to stick to the board, so a rack is needed to separate the board surface. After the rack is inserted, red tape is used to fix the board surface on both sides to avoid the handling process. Since the SIP board is 0.15-0.3mm thick, it is easy to sink and fall apart after the rack is inserted. Figure 5 Picture of the device used for the insert.
[0066] Taking into account the factors of falling apart and bending, red tape is needed on the left and right sides to fix the board after inserting the rack.
[0067] S103, performing exposure processing on the laminated circuit board so that the interval area between each unit in the laminated circuit board is adjusted to a preset shape to obtain an exposed circuit board.
[0068] In this embodiment, the laminated circuit board is exposed in the SET unit shipped to the customer, so as to adjust the spacing between units and add rectangular window strip grooves (with a width of 7-10 mil) to make up for the design defects of the residual copper rate on both sides.
[0069] It should be noted that SET is the shipping unit, that is, the finished product, and one board shipped is one SET.
[0070] In some embodiments, in step S103, "exposing the laminated circuit board so as to adjust the intervals between the units in the laminated circuit board to a preset shape" includes but is not limited to the following steps:
[0071] The exposure energy is set to 280-300 mj / cm2, the exposure scale is set to level 7-9, and the laminated circuit board is exposed so that the interval area between each unit in the laminated circuit board is adjusted to a window design.
[0072] In this embodiment, the laminated circuit board is exposed at an exposure energy of 280-300 mj / cm2 and an exposure scale of 7-9 (14-level exposure scale), so that the intermediate spacing area between adjacent units on the left and right is designed as a window design.
[0073] Because the surface and bottom surfaces of the SIP series boards correspond to chips and heat-dissipating electronic components respectively, there is a difference of more than 20% in the residual copper rate between the two sides. After the green oil window is opened, the difference in the residual copper rate between the top and bot surfaces is as high as more than 35%. Figure 6 This is the L4 top window graphic design. Figure 7This is the L4 bot surface window graphic design diagram. Figure 8 For the original graphic design at each level, due to the difference in residual copper rate, after the green oil is cured and the gong plate is formed, after being heated, due to the characteristics of thermal expansion and contraction of the material, the board is warped and deformed after reflow soldering, with a defect rate of about 80%-90%. After being shipped to the customer, after the client performs the component assembly, the bending deformation is serious, resulting in the inability to flatten the electronic components during the mounting process, which can seriously lead to poor welding and empty welding, affecting the reliability of the product, such as Fig. 9 and Fig.10 shown.
[0074] Fig.11 In order to optimize the L4 surface design with a high residual copper rate, the unit and unit are designed without windows, and the surface of the substrate is covered with continuous green oil, with a residual copper and residual oil rate of 75-77%. Fig.12 To optimize the L4 surface design, mainly for the L4 surface, the bottom surface with a higher residual copper rate, a rectangular window strip groove (width of 7mil-10mil) is added in the middle of the unit, and the residual copper rate is reduced from 77% to 8-10%. Table 1 shows the residual copper (oil) rate before optimization, and Table 2 shows the residual copper (oil) rate after optimization, where 1mil = 25um.
[0075] Table 1 Residual copper (oil) rate before optimization
[0076] dmp01 36% dmp04 77% L1 33% L4 54% L2 57% L3 55%
[0077] Table 2 Residual copper (oil) rate after optimization
[0078] dmp01 36% dmp04 69% L1 33% L4 54% 57% L3 55% 57%
[0079] S104, developing the exposed circuit board so as to develop the solder resist pattern in the unexposed area of the exposed circuit board, and curing and baking the developed circuit board to obtain a final circuit board.
[0080] In this embodiment, L1 is placed facing up, the protective film on the surface of the solder resist dry film is torn off, K2CO3 or NaCO3 concentration is used at 8-9g / L, soaked for 40-50s, the unexposed solder resist pattern is developed, and the exposed pattern is left on the board surface, and developed using K2CO3 or NaCO3 developer.
[0081] In some embodiments, the step S104 “before developing the exposed circuit board” includes but is not limited to the following steps:
[0082] The exposed circuit board is placed in a box, and a sulfur-free paper separator is used to separate the exposed circuit board from the box.
[0083] Specifically, after exposure, the board is placed in a box, and sulfur-free paper is used as a separator to reduce scratches and board corners bending and deformation during the board handling process. The box is cleaned every shift to ensure cleanliness.
[0084] In some embodiments, the step S104 of "curing and baking the developed circuit board" includes but is not limited to the following steps:
[0085] After the developed circuit board is subjected to the first UV curing, the circuit board after the first curing is post-baked using a vertical furnace baking plate, wherein the UV curing energy of the first UV curing is 500mj / cm2-600mj / cm2, and the temperature is 80 degrees-120 degrees;
[0086] The circuit board that has been post-baked is subjected to a second UV curing, wherein the UV curing energy of the second UV curing is 500mj / cm2 to 800mj / cm2 and the temperature is 80 degrees to 120 degrees.
[0087] Specifically, the ink on the circuit board is cured on the surface with UV curing energy of 500-600mj / cm2, temperature of 80-120 degrees, and double-sided production. Then, a vertical furnace is used for post-baking, and the post-baking is performed according to the standard of 100 degrees*30min+135 degrees*30min+150 degrees*60min.
[0088] The post-baking and curing process uses a vertical furnace kilometres rack, which is designed with dense grids, with a grid of 50m*50mm, as dense as possible, and an overall length*width of 650*550mm. The board surface is laid flat, which is more conducive to releasing thermal stress on the board surface. The flat laying method reduces post-baking thermal deformation, and does not use the tunnel furnace clamping method. This step is used to adjust the board warping and further solidify the ink surface.
[0089] In addition, the L1 side of the circuit board faces upward and the L4 side faces downward, and the corresponding UV upper lamp energy is 800mj / cm2, and the lower lamp energy is 500mjcm2 to perform UV curing on the circuit board. This step is not only affected by the dry film thickness on both sides, but also uses UV light and heat curing to balance the thermal deformation and expansion and contraction on both sides, further reducing the warping of the board. By adopting segmented UV curing (UV1-post-bake-UV1 method), and each UV segment and surface uses different UV energy methods to cure the board surface, the comprehensive goal is to balance the expansion and contraction of the graphics on both sides and reduce the problem of warping after heating.
[0090] The circuit boards manufactured by using the above scheme and design reduce the defect scrap rate, and the defect rate drops from 10-20% to 0.5%, thereby improving economic benefits.
[0091] It should be understood that although Figure 1 The steps in the flowchart are shown in sequence as indicated by the arrows, but these steps are not necessarily executed in the order indicated by the arrows. Unless otherwise specified in this document, there is no strict order restriction for the execution of these steps, and these steps can be executed in other orders. Moreover, Figure 1 At least part of the steps may include multiple steps or multiple stages. These steps or stages are not necessarily performed at the same time, but can be performed at different times. The execution order of these steps or stages is not necessarily sequential, but can be performed in turn or alternately with other steps or at least part of the steps or stages in other steps.
[0092] In one embodiment of the present application, a circuit board is provided. The circuit board provided in this embodiment is obtained by the above method, which will not be described in detail here.
[0093] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0094] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for manufacturing a printed circuit board, characterized in that: include: Drying the circuit board after the super-roughening pre-treatment to obtain a dried circuit board, and baking the dried circuit board to obtain a baked circuit board; After pre-aligning the dried circuit board, laminating the top surface of the dried circuit board with a solder resist dry film of a first thickness, laminating the bottom surface of the dried circuit board with a solder resist dry film of a second thickness, and vacuuming and leveling the laminating circuit board to obtain a laminated circuit board, wherein the first thickness is greater than the second thickness; performing an exposure process on the laminated circuit board so that the intervals between the units in the laminated circuit board are adjusted to a preset shape to obtain an exposed circuit board; The exposed circuit board is developed so that the solder resist pattern in the unexposed area of the exposed circuit board is developed, and the developed circuit board is cured and baked to obtain a final circuit board.
2. The method for manufacturing a printed circuit board according to claim 1, wherein: The ultra-roughening pre-treatment comprises: After degreasing and cleaning the circuit board, the circuit board is treated with an organic acid micro-etching solution with a micro-etching amount in the range of 1.3um to 1.4um; The processed circuit board is pickled and washed with water for multiple times.
3. The method for manufacturing a printed circuit board according to claim 1, wherein: The method of drying the circuit board after the ultra-roughening pre-treatment to obtain the dried circuit board comprises: The circuit board is dried using three upper and lower air knives to obtain a dried circuit board.
4. The method for manufacturing a printed circuit board according to claim 1, wherein: The step of baking the dried circuit board to obtain a baked circuit board comprises: The dried circuit board is dried using a vertical furnace drying plate to obtain a dried circuit board.
5. The method for manufacturing a printed circuit board according to claim 1, wherein: After obtaining the laminated circuit board, the method further comprises: The laminated circuit board is inserted into a rack, and adhesive tape is used to fix the left and right sides of the laminated circuit board.
6. The method for manufacturing a printed circuit board according to claim 1, wherein: The step of performing an exposure process on the laminated circuit board so as to adjust the intervals between the units in the laminated circuit board to a preset shape includes: The exposure energy is set to 280-300 mj / cm2, the exposure scale is set to level 7-9, and the laminated circuit board is exposed so that the interval area between each unit in the laminated circuit board is adjusted to a window design.
7. The method for manufacturing a printed circuit board according to claim 1, wherein: Before developing the exposed circuit board, the method further includes: The exposed circuit board is placed in a box, and a sulfur-free paper separator is used to separate the exposed circuit board from the box.
8. The method for manufacturing a printed circuit board according to claim 1, wherein: The step of developing the exposed circuit board so as to develop the solder resist pattern in the unexposed area of the exposed circuit board comprises: The top surface of the exposed circuit board is facing upward, the protective film on the solder resist dry film in the exposed circuit board is removed, and the exposed circuit board is immersed in K2CO3 or NaCO3 with a concentration of 8-9g / L to develop the solder resist pattern in the unexposed area, wherein the immersion time is 40s to 50s.
9. The method for manufacturing a printed circuit board according to claim 1, wherein: The curing and baking operation of the developed circuit board includes: After the developed circuit board is subjected to the first UV curing, the circuit board after the first curing is post-baked using a vertical furnace baking plate, wherein the UV curing energy of the first UV curing is 500mj / cm2-600mj / cm2, and the temperature is 80 degrees-120 degrees; The circuit board that has been post-baked is subjected to a second UV curing, wherein the UV curing energy of the second UV curing is 500mj / cm2 to 800mj / cm2 and the temperature is 80 degrees to 120 degrees.
10. A circuit board, characterized in that: The circuit board is obtained by using the printed circuit board manufacturing method according to any one of claims 1 to 9.