Transistor and preparation method
By patterning the gate dielectric layer and active layer in organic thin film transistors, the problems of high mobility and low stability caused by the short channel effect are solved, achieving faster switching speeds and lower power consumption.
Patent Information
- Application Number
- CN202310397964.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-18
AI Technical Summary
Existing organic thin film transistors have high mobility and low stability at short channel scales, and are greatly affected by parasitic channels and current bypasses, resulting in increased turn-off leakage current, gate leakage current and sub-threshold swing, limiting the circuit switching speed and power consumption.
By forming a gate layer on the substrate, patterning the gate dielectric layer to form a through hole to expose the gate electrode, forming a protective layer and encapsulation layer on the active layer, performing patterning operations to cut off the connection between the gate electrode and the active layer current path between the source and drain electrodes to reduce unregulated current bypass.
The off-leakage current, gate leakage current and sub-threshold swing of the organic thin film transistor are reduced, the switching speed of the circuit is improved, and the power consumption is reduced.
Smart Images

Figure CN118804607A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to semiconductor The technical field relates particularly to a transistor and a method for manufacturing the same. Background Art
[0002] Compared with traditional single-crystal silicon metal-oxide-semiconductor field-effect transistors (MOS-FETs), thin-film transistors (TFTs) prepared based on organic semiconductor materials have the advantages of low preparation temperature, large-area production, and the ability to be formed on heterogeneous substrates. Therefore, they are widely used in display electronics, flexible electronics, transparent electronics, bioelectronics and other fields.
[0003] Since its discovery, organic semiconductors have attracted widespread attention due to their intrinsic flexibility, low process temperature, and large-area integration, and have been used in production as a type of thin-film transistor active area material. With the development of society, the demand for the speed of thin-film transistor circuits is getting higher and higher, and the standard requirements for circuit power consumption are getting lower and lower. In order to broaden the application scope of organic thin-film transistors, the mobility of organic thin-film transistors needs to be increased accordingly, the channel length needs to be reduced accordingly, and the off leakage current, gate leakage current and subthreshold swing need to be reduced accordingly. At present, there are many types of organic thin-film transistors, but at the short channel scale, only a small number of organic thin-film transistors have high mobility and stable low threshold voltage characteristics under the influence of short channel effects. Moreover, most organic thin-film transistors are greatly affected by parasitic channels and current bypasses, which increases the off leakage current, gate leakage current and subthreshold swing of organic thin-film transistors, limits the switching speed of organic thin-film transistor circuits, and greatly increases the power consumption of organic thin-film transistor circuits. Summary of the invention
[0004] In view of the above problems, the present invention is proposed to provide a transistor and a manufacturing method thereof that overcome the above problems or at least partially solve the above problems.
[0005] In a first aspect, a method for manufacturing a transistor is provided, comprising: forming a gate layer on a substrate; the gate layer comprises a gate electrode and a gate dielectric layer arranged in sequence;
[0006] Patterning the gate dielectric layer to form a first through hole connected to the gate electrode;
[0007] forming a source-drain electrode, an active layer, a protective layer, and a packaging layer on the gate layer in sequence;
[0008] The encapsulation layer, the protection layer, and the active layer are patterned in sequence at the position of the first through hole to form a second through hole connected to the gate electrode.
[0009] Optionally, forming a gate layer on the substrate includes:
[0010] forming a gate electrode on a substrate, and patterning the gate electrode to expose a portion of a surface of the substrate;
[0011] A gate dielectric layer is formed on the surface of the substrate and the surface of the gate electrode.
[0012] Optionally, patterning the gate dielectric layer to form a first through hole connected to the gate electrode includes:
[0013] The gate dielectric layer is patterned by a dry etching process to form a first through hole, and a portion of the surface of the gate electrode is exposed through the first through hole.
[0014] Optionally, forming a source-drain electrode, an active layer, a protective layer, and an encapsulation layer in sequence on the gate layer includes:
[0015] forming source and drain electrodes on the gate dielectric layer;
[0016] Patterning the source and drain electrodes to expose a portion of the surface of the gate dielectric layer;
[0017] Modifying the gate dielectric layer and the source-drain electrode;
[0018] forming an active layer on the surface of the gate dielectric layer, the surface of the source and drain electrodes, and the surface of the gate electrode;
[0019] forming a protective layer on the active layer;
[0020] An encapsulation layer is formed on the protection layer.
[0021] Optionally, the patterning of the source and drain electrodes includes:
[0022] The source and drain electrodes are patterned by photolithography and stripping processes, so that the channel length between the source and drain electrodes is 50nm-500μm.
[0023] Optionally, the modifying of the gate dielectric layer and the source / drain electrode comprises:
[0024] Modifying the gate dielectric layer by immersing it in a gate dielectric modification layer solution;
[0025] The source and drain electrodes are modified by immersing in a metal modification layer solution or by thermally evaporating a modification layer.
[0026] Optionally, the step of sequentially patterning the encapsulation layer, the protection layer, and the active layer at the position of the first through hole to form a second through hole connected to the gate electrode includes:
[0027] The encapsulation layer, the protection layer and the active layer at the location of the first through hole are patterned by photolithography and oxygen plasma etching processes to form a second through hole, and a portion of the surface of the gate electrode is exposed through the second through hole.
[0028] In a second aspect, a transistor is provided, comprising: a substrate, and a gate layer, a source-drain electrode, an active layer, a protective layer, and an encapsulation layer sequentially arranged on the substrate;
[0029] The gate layer includes a gate electrode and a gate dielectric layer arranged in sequence;
[0030] A through hole is arranged on the transistor, and the through hole passes through the encapsulation layer, the protection layer, the active layer and the gate dielectric layer in sequence and is connected with the gate electrode.
[0031] Optionally, the bottom surface of the gate electrode contacts and at least partially covers the substrate; the bottom surface of the source and drain electrodes contacts and at least partially covers the gate dielectric layer; the bottom surface of the active layer contacts and covers the surface of the gate dielectric layer and the surface of the source and drain electrodes.
[0032] Optionally, the thickness of the active layer is 2-4 nm.
[0033] The technical solution provided in the embodiments of the present invention has at least the following technical effects or advantages:
[0034] The transistor and preparation method provided by the embodiment of the present invention, on the one hand, form a through hole in the gate dielectric layer to expose the gate electrode, and then form a protective layer and a packaging layer on the active layer, so that the active layer can be patterned, while avoiding damage to the transistor by the patterning operation. On the other hand, through two patterning operations, through holes are processed on the gate dielectric layer and the active layer at the same position to connect to the gate electrode, so that patterning is achieved on the active layer, the current path between the gate and the active layer and the active layer current bypass between the source and drain electrodes that is not regulated by the gate are cut off, the turn-off leakage current, gate leakage current and subthreshold swing of the organic thin film transistor are reduced, the switching speed of the organic thin film transistor circuit is improved, and the power consumption of the organic thin film transistor circuit is reduced.
[0035] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. Moreover, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:
[0037] Figure 1 It is a flow chart in an embodiment of the present invention;
[0038] Figure 2 The process diagram of the manufacturing method in the embodiment of the present invention is shown in FIG. Figure 1 ;
[0039] Figure 3 for Figure 2 A-A' section diagram;
[0040] Figure 4 The process diagram of the manufacturing method in the embodiment of the present invention is shown in FIG. Figure 2 ;
[0041] Figure 5 for Figure 4 B-B' section diagram in;
[0042] Figure 6 The process diagram of the manufacturing method in the embodiment of the present invention is shown in FIG. Figure 3 ;
[0043] Figure 7 for Figure 4 C-C' section diagram in;
[0044] Figure 8 The process diagram of the manufacturing method in the embodiment of the present invention is shown in FIG. Figure 4 ;
[0045] Fig. 9 for Figure 4 D-D' section diagram in;
[0046] Fig.10 This is a test result diagram of an organic thin film transistor without a patterned active layer in an embodiment of the present invention;
[0047] Fig.11 This is a test result diagram of an organic thin film transistor with a patterned active layer in an embodiment of the present invention. DETAILED DESCRIPTION
[0048] Exemplary embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings.
[0049] Various structural schematic diagrams according to embodiments of the present disclosure are shown in the accompanying drawings. These figures are not drawn to scale, and some details are magnified and some details may be omitted for the purpose of clear expression. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships therebetween are only exemplary, and may deviate in practice due to manufacturing tolerances or technical limitations, and those skilled in the art may further design regions / layers with different shapes, sizes, and relative positions according to actual needs.
[0050] In the context of the present disclosure, when a layer / element is referred to as being "on" another layer / element, the layer / element may be directly on the other layer / element, or there may be an intervening layer / element therebetween. Additionally, if a layer / element is "on" another layer / element in one orientation, the layer / element may be "below" the other layer / element when the orientation is reversed. In the context of the present disclosure, similar or identical components may be denoted by the same or similar reference numerals.
[0051] In order to better understand the above-mentioned technical scheme, the above-mentioned technical scheme will be described in detail below in combination with specific implementation methods. It should be understood that the embodiments of the present disclosure and the specific features in the embodiments are detailed descriptions of the technical scheme of the present application, rather than limitations on the technical scheme of the present application. In the absence of conflict, the embodiments of the present application and the technical features in the embodiments can be combined with each other.
[0052] The present invention provides a transistor manufacturing method, please refer to Figure 1 , Figure 1 It is a flow chart in an embodiment of the present invention, including:
[0053] Step S1, forming a gate layer on a substrate; the gate layer includes a gate electrode and a gate dielectric layer arranged in sequence;
[0054] Step S2, patterning the gate dielectric layer to form a first through hole connected to the gate electrode;
[0055] Step S3, forming a source-drain electrode, an active layer, a protective layer, and an encapsulation layer on the gate layer in sequence;
[0056] Step S4, patterning the encapsulation layer, the protection layer, and the active layer in sequence at the position of the first through hole to form a second through hole connected to the gate electrode.
[0057] At present, there are many types of processes used for large-area integration of organic thin film transistors, among which the more mature ones are spin coating, drip coating, inkjet printing and roll-to-roll processes. With the increase in the integration density, speed and circuit power consumption requirements of thin film transistors, the off leakage current, gate leakage current and subthreshold swing of organic thin film transistors need to be reduced accordingly. However, the active layer film area of the organic thin film transistor prepared based on the above process is large and the above process does not pattern the active layer, which greatly limits its switching speed and power consumption level in the development of organic thin film transistors. Therefore, it has become a top priority to be able to pattern the channel active layer more accurately. The method of the present invention enables the active layer to be patterned, reduces the off leakage current, gate leakage current and subthreshold swing of the organic thin film transistor, improves the switching speed of the organic thin film transistor circuit, and reduces the power consumption of the organic thin film transistor circuit.
[0058] Combine the following Figure 2-9 The implementation process steps of this embodiment are described in detail:
[0059] A substrate 1 is provided. The substrate 1 is an insulating layer substrate. The insulating layer substrate can be selected from hard and flexible substrates 1 made of materials including but not limited to SiO2, glass, PI, etc., and no limitation is made here.
[0060] like Figure 2 , 3As shown, step S1 is performed to form a gate layer on the substrate 1, wherein the gate layer includes a gate electrode 2 and a gate dielectric layer 3 arranged in sequence. The process of forming the gate layer on the substrate 1 can be: forming a gate electrode 2 on the substrate 1, and patterning the gate electrode 2 to expose a portion of the surface of the substrate 1. The gate electrode 2 can be grown on the insulating layer substrate by electron beam evaporation process. The gate electrode 2 material is one or a combination of TiN, Au, Ti, Mo, and Ag, and the thickness of the gate electrode 2 is 30nm to 300nm. The gate electrode 2 is patterned by photolithography and stripping process. The photoresist used in the photolithography is selected as negative photoresist 1500 and positive photoresist 5141; the photolithography exposure method is selected as contact / proximity photolithography. The gate dielectric layer 3 is formed on the surface of the substrate 1 and the surface of the gate electrode 2. The gate dielectric layer 3 is grown on the gate electrode 2 and the insulating layer substrate by atomic layer deposition, magnetron sputtering and inductively coupled plasma chemical vapor deposition equipment. The gate dielectric layer 3 is formed on the gate electrode 2 after being patterned according to the shape of the gate electrode 2. The growth temperature of the atomic layer deposition is 100°C-300°C. A High-κ gate dielectric layer 3 with a higher dielectric constant can be selected to change the capacitance of the gate dielectric layer 3, speed up the opening and closing speed of the thin film transistor, and reduce the power consumption of the thin film transistor. The control ability of the gate over the active layer 5 is enhanced, the threshold voltage of the device is reduced, and the short channel effect of the device is weakened. The selection of materials for the High-κ gate dielectric layer 3 includes but is not limited to AlOx. The thickness of the gate dielectric layer is 10nm to 70nm.
[0061] Execute step S2 to pattern the gate dielectric layer 3 to form a first through hole connected to the gate electrode 2, wherein the gate dielectric layer 3 is patterned by a dry etching process using a photoresist mask formed by photolithography to form a first through hole, and the first through hole is located on the gate electrode 2, and a portion of the surface of the gate electrode 2 is exposed through the first through hole.
[0062] like Figures 4 to 7 As shown, the process of performing step S3 to sequentially form source-drain electrodes 4, active layer 5, protective layer 6, and encapsulation layer 7 on the gate layer is specifically as follows: forming source-drain electrodes 4 on the gate dielectric layer 3; patterning the source-drain electrodes 4 to expose a portion of the surface of the gate dielectric layer 3; modifying the gate dielectric layer 3 and the source-drain electrodes 4; forming an active layer 5 on the surface of the gate dielectric layer 3, the surface of the source-drain electrodes 4, and the surface of the gate electrode 2; forming a protective layer 6 on the active layer 5; and forming an encapsulation layer 7 on the protective layer 6. Among them, the source-drain electrodes 4 are grown on the gate dielectric layer 3 by electron beam evaporation, and the source-drain electrodes 4 are patterned by photolithography and lift-off processes to form the source-drain electrodes 4, and the gate dielectric layer 3 is formed as shown. Figure 4 , 5 The structure shown.
[0063] Among them, the source-drain electrode 4 uses a material of one or a combination of Au, Ti, and Ag, with a thickness of 30nm to 80nm. For example, a Ti / Au (5nm / 35nm) stack is grown on the gate dielectric layer 3 by electron beam evaporation as the source-drain electrode 4, and the source-drain electrode 4 is patterned by photolithography and stripping processes. The channel length between the formed source-drain electrodes 4 is 50nm-500μm.
[0064] In an optional embodiment, after forming the source-drain electrode 4, the gate dielectric layer 3 is modified by soaking in a gate dielectric modification layer solution. The material that can be selected for the gate dielectric modification layer is one of decylphosphonic acid solution, n-tetradecyl phosphoric acid solution, and n-octadecyl phosphate solution. The solvent of the gate dielectric modification layer solution is isopropanol, the concentration is selected to be 0.5mM-3mM, and the soaking time is 1 hour to 2 hours. Different gate dielectric modification layer materials are selected to modify the gate dielectric layer 3, repair the interface between the gate dielectric layer 3 and the active layer 5 material, reduce the interface scattering between the gate dielectric layer 3 and the active layer 5 of the thin film transistor, and improve the mobility of the thin film transistor. The source-drain electrode 4 is modified by soaking in a metal modification layer solution or thermal evaporation modification layer. The metal modification layer can be made of one or a combination of 2,3,4,5,6-pentafluorothiophenol (PFBT) solution and MoO3 film. The solvent of the PFBT solution is anhydrous ethanol. The concentration of the PFBT solution is 0.5μL / mL to 5μL / mL, and the soaking time is 5 to 6 hours. The thickness of the thermally evaporated MoO3 film is 1 to 10nm. Different source and drain metal modification layer materials are selected to modify the source and drain metals, adjust the Schottky barrier between the source and drain metals and the active layer 5 material, reduce the contact resistance between the source and drain electrodes 4 of the thin film transistor and the active layer 5, and improve the mobility of the thin film transistor.
[0065] In an optional embodiment, the process of forming the active layer 5 on the surface of the gate dielectric layer 3, the surface of the source-drain electrode 4 and the surface of the gate electrode 2 is specifically: forming the organic thin film active layer 5 on the gate dielectric layer 3 and the source-drain electrode 4 by thermal evaporation, spin coating and pulling process; preferably, the evaporation rate used in the thermal evaporation process is The spin coating speed used in the spin coating process is 500rpm-6000rpm. The pulling speed used in the pulling process is 50μm / s-1000μm / s. Among them, the pulling method, as a process method for growing the active layer 5, can grow an organic active layer 5 with a thickness of a monolayer to a thin film. The parameters such as the energy band, dielectric constant, and mobility of the active layer 5 of different thicknesses do not change significantly, so that an active layer 5 as thin as 2 to 4 nanometers can be selected to optimize the contact characteristics between the source and drain metal of the short channel device and the active layer 5, thereby weakening the short channel effect of the device. The selection of the active layer 5 includes a solution of all organic semiconductor materials such as conjugated small molecules such as pentacene and C8-BTBT and conjugated polymers such as PffBT4T-2DT and P3HT (poly (3-hexylthiophene-2,5-diyl), the solvent of the organic semiconductor solution is chloroform, and the concentration is 0.1mg / mL to 10mg / mL. The pulling speed is 100μm / s.
[0066] In an optional embodiment, the process of forming the protective layer 6 on the active layer 5 is specifically as follows: a spin coating process and annealing are used to form the protective layer 6 on the active layer 5; the protective layer protects the active layer from being affected by the encapsulation layer growth process and participates in the patterning process. Preferably, the spin coating speed used in the spin coating process is 1200rpm to 4000rpm, and the spin coating time is 1 minute. The annealing temperature is 50℃ to 120℃, and the annealing time is 30 minutes to 90 minutes. The material used for the protective layer 6 is a mixed solution of Cytop stock solution and Cytop solvent, and the ratio of the mixed solution is selected as Cytop stock solution: Cytop solvent = 1:0, 1:1 or 1:2. Cytop is selected as the protective layer 6 of the active layer 5. After the thin film transistor is patterned by photolithography and oxygen plasma etching, the parasitic channel and the current bypass are shielded, and the off leakage current, gate leakage current and subthreshold swing are greatly reduced, which speeds up the opening and closing speed of the thin film transistor and reduces the power consumption of the thin film transistor. A good interface can be formed between the Cytop protective layer 6 grown at low temperature and the active layer 5, which will not affect the performance of the thin film transistor; in addition, the Cytop protective layer 6 and the active layer 5 can be in-situ etched, and other factors will not be introduced in the preparation of the thin film transistor.
[0067] In an optional embodiment, the process of forming the encapsulation layer 7 on the protective layer 6 is specifically as follows: forming the encapsulation layer 7 on the protective layer 6 by a thermal evaporation process, forming Figure 6 , 7 Parylene is selected as the encapsulation layer 7 of the active layer 5, which can isolate external factors, such as water, oxygen, etc., from affecting the active layer 5, thereby increasing the working life of the thin film transistor. The thickness of the encapsulation layer 7 is 50nm-5μm
[0068] like Figure 8 , 9 As shown, step S4 is performed to pattern the encapsulation layer 7, the protection layer 6, and the active layer 5 in sequence at the position of the first through hole to form a second through hole connected to the gate electrode 2. According to the channel shape, the encapsulation layer 7, the protection layer 6, and the active layer 5 are patterned simultaneously using a photoresist mask formed by photolithography and an oxygen plasma etching process, so that a portion of the gate electrode 2 is exposed through the second through hole, thereby forming an organic thin film transistor with a patterned active layer 5.
[0069] The following is a specific example of the method for preparing a patterned organic thin film transistor:
[0070] On a 2-inch silicon wafer with 300nm thermally oxidized SiOx, first, a Ti / Au (5nm / 30nm) stack is grown as a gate electrode 2 by electron beam evaporation, and the gate electrode 2 is patterned by photolithography and lift-off process. Next, 20nm of AlOx is grown on the SiOx substrate 1 and the gate electrode 2 at 300°C by atomic layer deposition. Using spin-coated photoresist as a masking layer, the gate dielectric layer 3 is patterned by dry etching process to form a first through hole, exposing a portion of the gate electrode 2. Then, a Ti / Au (5nm / 35nm) stack is grown on the gate dielectric layer 3 by electron beam evaporation as a source-drain electrode 4, and the source-drain electrode 4 is patterned by photolithography and lift-off process. Afterwards, the silicon wafer was immersed in a 1 mM tetradecylphosphoric acid solution for 1 hour to modify the surface of the gate dielectric layer 3 and in a 1.5 μL / mL PFBT solution for 6 hours to modify the surface of the source and drain electrodes 4. The silicon wafer was pulled at a speed of 100 μm / s in a 0.5 mg / mL PffBT4T-2DT solution to form an organic thin film active layer 5 on the gate dielectric layer 3, the source and drain electrodes 4 and the gate electrode 2 exposed through the first through hole. The active layer 5 was spin-coated at a speed of 4000 rpm, and a mixed solution of Cytop stock solution: Cytop solvent = 1:1 was spin-coated for 60 seconds, and annealed at 100° C. for 60 minutes to form a protective layer 6 with a thickness of 200 nm. Afterwards, 0.3 g of Parylene was thermally evaporated to form a 300 nm thick encapsulation layer 7 on the protective layer 6. Finally, a spin-coated photoresist is used as a masking layer, and an oxygen plasma etching process is used to simultaneously pattern the encapsulation layer 7, the protective layer 6 and the active layer 5 at the position of the first through hole to form a second through hole, so that a portion of the gate electrode 2 is exposed through the second through hole, thereby forming an organic thin film transistor with a patterned active layer 5.
[0071] The organic thin film transistor without patterned active layer 5 and the organic thin film transistor with patterned active layer 5 were tested, and the parameters included off-leakage current, gate leakage current and subthreshold swing. Subthreshold swing refers to the parameter of the device being turned off quickly with gate voltage, representing the change in gate voltage required when the source-drain current changes by one order of magnitude. The results are shown in Figure 2. Fig.10 , 11 As shown, the organic thin film transistor with the patterned active layer 5 has lower off leakage current, gate leakage current and subthreshold swing than the device without the patterned active layer 5, and is more suitable for application in integrated circuits requiring high speed and low power consumption.
[0072] Based on the same inventive concept, the embodiment of the present invention further provides a transistor, please refer to Figures 6 to 9 , comprising: a substrate 1, and a gate layer, a source-drain electrode 4, an active layer 5, a protective layer 6, and an encapsulation layer 7 sequentially arranged on the substrate 1; the gate layer comprises a gate electrode 2 and a gate dielectric layer 3 sequentially arranged; a through hole 8 is arranged on the transistor, and the through hole 8 sequentially passes through the encapsulation layer 7, the protective layer 6, the active layer 5, and the gate dielectric layer 3 and is connected to the gate electrode 2. Specifically, the bottom surface of the gate electrode 2 contacts and at least partially covers the substrate 1; the bottom surface of the source-drain electrode 4 contacts and at least partially covers the gate dielectric layer 3; the bottom surface of the active layer 5 contacts and covers the surface of the gate dielectric layer 3 and the surface of the source-drain electrode 4.
[0073] The technical solution provided in the embodiment of the present invention has at least the following technical effects or advantages: the transistor and the preparation method provided in the embodiment of the present invention, on the one hand, form a through hole in the gate dielectric layer to expose the gate electrode, and then form a protective layer and a packaging layer on the active layer, so that the active layer can be patterned, while avoiding damage to the transistor by the patterning operation. On the other hand, through two patterning operations, through holes are processed on the gate dielectric layer and the active layer at the same position to connect to the gate electrode, so that patterning is achieved on the active layer, the off leakage current, gate leakage current and subthreshold swing of the organic thin film transistor are reduced, the switching speed of the organic thin film transistor circuit is improved, and the power consumption of the organic thin film transistor circuit is reduced.
[0074] In the description provided herein, a large number of specific details are described. However, it is understood that embodiments of the present invention can be practiced without these specific details. In some instances, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this description.
[0075] Similarly, it should be understood that in order to streamline the present disclosure and aid in understanding one or more of the various inventive aspects, in the above description of exemplary embodiments of the present invention, various features of the present invention are sometimes grouped together into a single embodiment, figure, or description thereof. However, this disclosed method should not be interpreted as reflecting the intention that the claimed invention requires more features than those explicitly recited in each claim. More specifically, as reflected in the claims below, inventive aspects lie in less than all the features of the individual embodiments disclosed above. Therefore, the claims that follow the specific embodiment are hereby expressly incorporated into the specific embodiment, with each claim itself serving as a separate embodiment of the present invention.
[0076] It should be noted that the above embodiments illustrate the present invention rather than limit it, and that those skilled in the art may devise alternative embodiments without departing from the scope of the appended claims. In the claims, any reference symbol between brackets shall not be construed as a limitation on the claims. The word "comprising" does not exclude the presence of components or steps not listed in the claims. The word "one" or "an" preceding a component does not exclude the presence of a plurality of such components. The present invention may be implemented by means of hardware comprising a number of different components and by means of a suitably programmed computer. In a unit claim enumerating a number of devices, several of these devices may be embodied by the same hardware item. The use of the words first, second, and third, etc., does not indicate any order. These words may be interpreted as names.
Claims
1. A method for preparing a transistor, characterized in that: include: A gate layer is formed on the substrate; the gate layer comprises a gate electrode and a gate dielectric layer arranged in sequence; Patterning the gate dielectric layer to form a first through hole connected to the gate electrode; forming a source-drain electrode, an active layer, a protective layer, and a packaging layer on the gate layer in sequence; The encapsulation layer, the protection layer, and the active layer are patterned in sequence at the position of the first through hole to form a second through hole connected to the gate electrode.
2. The preparation method according to claim 1, characterized in that The step of forming a gate layer on a substrate comprises: forming a gate electrode on a substrate, and patterning the gate electrode to expose a portion of a surface of the substrate; A gate dielectric layer is formed on the surface of the substrate and the surface of the gate electrode.
3. The preparation method according to claim 1, characterized in that: The step of patterning the gate dielectric layer to form a first through hole connected to the gate electrode comprises: The gate dielectric layer is patterned by a dry etching process to form a first through hole, and a portion of the surface of the gate electrode is exposed through the first through hole.
4. The preparation method according to claim 1, characterized in that: The step of sequentially forming a source-drain electrode, an active layer, a protective layer, and a packaging layer on the gate layer includes: forming source and drain electrodes on the gate dielectric layer; Patterning the source and drain electrodes to expose a portion of the surface of the gate dielectric layer; Modifying the gate dielectric layer and the source-drain electrode; forming an active layer on the surface of the gate dielectric layer, the surface of the source and drain electrodes, and the surface of the gate electrode; forming a protective layer on the active layer; An encapsulation layer is formed on the protection layer.
5. The preparation method according to claim 4, characterized in that: The patterning of the source-drain electrode comprises: The source and drain electrodes are patterned by photolithography and stripping processes, so that the channel length between the source and drain electrodes is 50nm-500μm.
6. The preparation method according to claim 4, characterized in that: The modifying of the gate dielectric layer and the source-drain electrode comprises: Modifying the gate dielectric layer by immersing it in a gate dielectric modification layer solution; The source and drain electrodes are modified by immersing in a metal modification layer solution or by thermally evaporating a modification layer.
7. The preparation method according to claim 1, characterized in that: The step of sequentially patterning the encapsulation layer, the protection layer, and the active layer at the position of the first through hole to form a second through hole connected to the gate electrode comprises: The encapsulation layer, the protection layer and the active layer at the location of the first through hole are patterned by photolithography and oxygen plasma etching processes to form a second through hole, and a portion of the surface of the gate electrode is exposed through the second through hole.
8. A transistor, characterized in that: include: A substrate, and a gate layer, a source-drain electrode, an active layer, a protective layer, and an encapsulation layer sequentially arranged on the substrate; The gate layer includes a gate electrode and a gate dielectric layer arranged in sequence; A through hole is arranged on the transistor, and the through hole passes through the encapsulation layer, the protection layer, the active layer and the gate dielectric layer in sequence and is connected with the gate electrode.
9. The transistor according to claim 8, characterized in that The bottom surface of the gate electrode contacts and at least partially covers the substrate; the bottom surface of the source-drain electrode contacts and at least partially covers the gate dielectric layer; the bottom surface of the active layer contacts and covers the surface of the gate dielectric layer and the surface of the source-drain electrode.
10. The transistor according to claim 8, characterized in that The thickness of the active layer is 2-4 nm.