Core material, skin-core structure, aerospace equipment, aircraft, and method for manufacturing skin-core structure
By forming a porous structure on the unit wall of the core material and optimizing the bonding process, the problem of strength reduction caused by enhanced air permeability in the existing technology is solved, achieving a balance between high air permeability, light weight and mechanical properties, and improving Improves the bonding strength and buckling resistance of the core material and skin material.
Patent Information
- Application Number
- CN202380024866.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-03
- Filing Date
- 2023-03-03
- Publication Date
- 2024-10-18
AI Technical Summary
When the existing technology enhances the breathability of the core material, it results in a reduction in strength or a decrease in the bonding strength with the leather material. Especially in fiber-reinforced plastics, the perforation process is unstable, making it difficult to achieve a balance between lightweight, mechanical properties and breathability.
Using a porous structural unit wall composed of fiber and resin, the fiber is coated with resin to form a wire-like film to ensure shape stability and mechanical properties. At the same time, the porous structure of the unit wall increases air permeability and optimizes the bonding process. Improve bonding strength with leather.
It achieves a balance between high air permeability, light weight and mechanical properties, improves the bonding strength and buckling resistance of the core material and the leather material, and enhances the overall performance of the core material.
Smart Images

Figure CN118804835A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a core material used in a skin-core structure. Background Art
[0002] The skin-core structure using a core material having a structure formed by an aggregate of hollow columnar units divided by cell walls as the core material has excellent mechanical properties such as light weight and high rigidity, and is therefore widely used in structural parts and building materials of aircraft, ships, etc. As these core materials, there are aluminum honeycomb core materials formed of aluminum foil, FRP honeycomb core materials formed of reinforcing fibers and matrix resin, etc. Among them, in aircraft such as aircraft with strong requirements for lightweight, aramid honeycomb core materials obtained by impregnating phenolic resin in non-woven fabrics of aramid fibers are mainly used.
[0003] In addition to lightness and mechanical properties, most core materials also require air permeability. For example, when the skin materials are bonded to form a sandwich structure, gases such as volatile components and hygroscopic moisture are generated from the material, and sometimes poor molding occurs due to gas pressure, so it is necessary to discharge the gas from each unit space to the outside. In addition, when used for aerospace equipment such as artificial satellites, the internal pressure of each unit space inside must be consistent with the external pressure (zero pressure space). In addition, when used for aircraft such as airplanes, sometimes due to repeated flights and changes in air pressure, the moisture contained in the air invades and condenses locally. The moisture in the core material freezes when flying at high altitudes, and sometimes the bonding portion between the core material and the skin material is peeled off due to its volume expansion when freezing.
[0004] In order to impart air permeability to the core material, attempts have been made to drill a large number of holes in the cell wall using a drill or the like (Patent Document 1) and to introduce a cutout structure into the opening end of the cell wall (Patent Document 2).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent No. 6804340
[0008] Patent Document 2: Japanese Patent No. 6549982 Summary of the invention
[0009] Problems to be solved by the invention
[0010] According to the methods described in Patent Documents 1 and 2, although a core material with air permeability can be obtained, the strength of the core material is reduced due to the perforation on the cell wall, or the adhesion between the core material and the skin material is reduced due to the cutout structure at the open end, etc., and there is a concern that the reliability as a structure will be reduced. In addition, when fiber reinforced plastic is used as the base material, the perforation process itself is unstable due to the combination of reinforcing fiber substrates and resins with different hardnesses, and it is particularly difficult to perforate the internal cell wall, and there are also problems in the processing operation. The purpose of the present invention is to provide a core material that has air permeability and achieves both lightness and mechanical properties.
[0011] Means for solving problems
[0012] The present invention for solving the above-mentioned problems is a core material having a structure formed by an aggregate (array) of hollow columnar units divided by unit walls, wherein the unit walls are formed by a fiber-reinforced composite material comprising fibers (Cf) and resin (Cr), and at least a portion of the unit walls is a porous structure portion composed of an aggregate (assembly) of fibers (Cf), and the fibers (Cf) are fibers coated with resin (Cr).
[0013] Another aspect of the present invention is a skin-core structure obtained by bonding the core material and the skin material described above.
[0014] Effects of the Invention
[0015] According to the present invention, it is possible to obtain a core material and a skin-core structure that have air permeability and achieve both lightness and mechanical properties at a high level. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] [ Figure 1 ] is a schematic diagram showing an embodiment of the core material of the present invention.
[0017] [ Figure 2 ] is a schematic diagram showing an embodiment of the sandwich structure of the present invention.
[0018] [ Figure 3 ] is a schematic diagram showing an embodiment of the fiber felt (A) contained in the sheet substrate (B).
[0019] [ Figure 4 ] is a schematic diagram obtained by enlarging the porous structure portion of the cell wall in one embodiment of the core material of the present invention.
[0020] [ Figure 5 ] is a schematic diagram showing an example of a manufacturing apparatus for fiber felt (A).
[0021] [ Figure 6 ] is a cross-sectional view showing the stacking / molding state in the evaluation of the buckling resistance of the core material of the present invention.
[0022] [ Figure 7 ] is a schematic diagram obtained by observing the sandwich structure before molding in the evaluation of the compression resistance of the core material of the present invention from above.
[0023] [ Figure 8 ] is a schematic diagram obtained by observing from above a sandwich structure in which core collapse occurred after molding in the evaluation of the buckling resistance of the core material of the present invention.
[0024] [ Fig. 9 ] is a three-dimensional schematic diagram showing the buckling condition of the core material after molding.
[0025] [ Fig.10 ] is a schematic diagram showing a situation in which a part of the discontinuous fibers (Cf) contained in the cell walls of the core material enters into the skin material.
[0026] [ Fig.11 ] is a schematic diagram showing the average fiber orientation angle in the out-of-plane direction relative to the cell wall of the present invention. DETAILED DESCRIPTION
[0027] <Core material>
[0028] Hereinafter, the core material of the present invention will be described with reference to the accompanying drawings as appropriate, but the present invention is not limited to these drawings. However, as those skilled in the art will readily understand, the description of the embodiments described in the accompanying drawings can also function as a description of the core material of the present invention as a higher concept.
[0029] Figure 1 Schematic diagram showing one embodiment of the core material of the present invention together with an enlarged image of a porous structure portion. The core material 1 has a structure formed by a collection of a large number of hollow columnar cells (hereinafter sometimes referred to as "columnar cells") divided by cell walls 4. The cell walls 4 are formed of a fiber-reinforced composite material containing fibers (Cf) and resin (Cr). The axial direction ( Figure 1 The end portion (in the direction of the arrow) is the porous structure portion 6. Figure 1 As shown in the enlarged view in FIG. 2 , the porous structure portion 6 is composed of an aggregate of fibers (Cf) 2 , and the fibers (Cf) 2 are fibers covered with a resin (Cr) 3 .
[0030] As for the coating state of the fiber (Cf) 2 coated with the resin (Cr) 3, as long as at least the intersections of the single fibers of the fiber (Cf) 2 constituting the porous structure 6 are coated, it is sufficient from the perspective of shape stability, ease of thickness control and degree of freedom of the porous structure 6. In a more ideal embodiment, the resin (Cr) 3 is in the following state: around the fiber (Cf) 2, the resin (Cr) 3 is coated with a thickness of 1 μm or more. This state means that the surface of the fiber (Cf) 2 is not exposed due to the resin (Cr) 3. In other words, the fiber (Cf) 2 forms a wire-shaped film using the resin (Cr) 3. As a result, the porous structure 6 also has shape stability and makes the presentation of mechanical properties sufficient.
[0031] The porous structure part 6 is preferably a structure in which the fiber (Cf) 2 coated with the resin (Cr) 3 becomes a columnar support, and contains a void 5 as a space formed by overlapping or crossing the support. By making such a structure, the porous structure part 6 has air permeability, and can utilize the reinforcing effect brought by the fiber (Cf) 2 to exert strength and elastic modulus. In addition, the porous structure part 6 preferably has holes that are continuous at least in the thickness direction of the cell wall. By having such a structure, the air permeability in the thickness direction of the cell wall can be easily ensured.
[0032] The core material of the present invention is not particularly limited, and is typically used in the form of a skin-core structure obtained by bonding a skin material to at least one side, preferably both sides, of the end face (core material opening face) of the columnar unit opening. Hereinafter, in this specification, the structure obtained by bonding a skin material to both sides of the core material as a particularly preferred method is referred to as a sandwich structure, especially among skin-core structures. Figure 2 Schematic diagram showing one embodiment of such a sandwich structure. Figure 2 In order to make the structure of the skin-core structure 8 clear, the core material 1 and the skin material 7 are depicted in a separated state. The sandwich structure 8 is formed by bonding the skin material 7 to the open end surface of the core material 1. An adhesive may also be used between the core material 1 and the skin material 7.
[0033] The porous structure of the cell wall can be a part of the cell wall, or the cell wall can be a porous structure as a whole. By having a porous structure at least near the opening end of the hollow columnar cell, the contact area with the skin material is increased, and a high bonding strength is exerted, so it is preferred. The contact area of the core material with the skin material is reduced in its structure, so it is difficult to obtain a strong bonding strength. In order to obtain a high bonding strength, it is necessary to control the fluidity of the adhesive and the resin of the skin material, form a resin storage part called a flange, and also use the side of the cell wall for bonding. The vicinity of the opening end of the core material of the present invention, that is, the vicinity of the part that contacts the skin material when bonding with the skin material, is a porous structure, thereby ensuring quality and strength and making the cell wall thick, so that the contact area with the skin material is increased, and a high bonding strength can be exerted. In addition, a part of the adhesive or the resin of the skin material can flow into the porous structure of the core material, so that the bonding between the skin material and the core material can be made stronger. In order to achieve high bonding strength between the core material and the skin material, the area ratio of the cell wall per unit core material density (bonding area ratio) in the area of the core material opening surface is preferably 0.075%·m 3 / kg or more, more preferably 0.100%·m 3 / kg or more. The area ratio of the cell wall per unit core density is less than 0.075%·m 3 / kg, the bonding area between the cell wall and the skin material is small, resulting in a decrease in the bonding strength between the core material and the skin material. Alternatively, the core material density increases due to the increase in the proportion of the cell wall, resulting in poor lightness. Here, the bonding strength between the core material and the skin material is the climbing roller peel strength (ASTMD1781-2004).
[0034] In addition, if the thickness near the opening end of the cell wall is thicker than the central part of the cell wall, the bonding area with the skin material can be increased, so it is preferred. At this time, if the cell wall near the opening end is thickened by changing the expansion of the porous structure, a structure containing more voids near the opening end compared to the central part can be made, so that the resin and adhesive constituting the skin material can flow in more easily during bonding with the skin material, and the bonding strength can be improved. The ratio Da / Db of the thickness (Da) of the thickest part of the cell wall of the core material to the thickness (Db) of the thinnest part is preferably in the range of 1.2 to 10. Typically, the relatively thick part in the cell wall is the porous structure part mentioned above. If this part is too thin, the formation of the porous structure is insufficient, so sometimes the air permeability cannot be exerted. On the other hand, if the formation of the porous structure progresses and the cell wall becomes too thick, sometimes the hollow columnar structure formed by division collapses and the strength is reduced. Da / Db is preferably in the range of 1.2 to 10, and more preferably in the range of 1.5 to 5.
[0035] In addition, when the cell wall is made into a porous structure as a whole, in addition to the high bonding strength with the above-mentioned leather material, the air permeability is improved and the buckling resistance and impact resistance of the cell wall are improved, so it is preferred. Usually, the cell wall of the core material is thin, so the resistance to the load in the direction perpendicular to the axial direction of the cell wall is weak. For example, when the leather material is bonded, sometimes the core collapses due to the buckling of the cell wall due to the sliding of the leather material. In order to prevent the buckling of the cell wall, it is usually considered to reduce the cell size or thicken the cell wall, but these methods are inevitably accompanied by an increase in mass. In the present invention, by making the cell wall as a whole into a porous structure, lightness and buckling resistance can be achieved at the same time. In addition, with respect to the impact, the impact energy is absorbed by the sequential destruction of the porous structure, so that excellent impact resistance can be imparted.
[0036] In order to make the core material exhibit high resistance to compression buckling, a high elastic modulus is required. The elastic modulus of the core material is preferably 1 GPa or more at room temperature (20°C ± 15°C), and more preferably 1 GPa or more at 120-200°C (which is the usual molding temperature of the skin-core structure). Here, the so-called elastic modulus refers to the storage elastic modulus measured by dynamic mechanical analysis (DMA), which is the storage elastic modulus at room temperature or the molding temperature (120-200°C) of the skin-core structure obtained in the following manner: the cell wall is collected from the core material, and the thickness direction of the core material (the axial direction of the cell wall) is used as the long side direction of the test piece, and DMA Q800 (manufactured by TA Instruments) is used to perform DMA measurement at a heating rate of 5°C / min, a frequency of 1Hz, and a single cantilever mode.
[0037] In addition, the density of the cell wall represented by the mass per unit volume Wc is preferably 0.1 g / cm 3 Above and 1.3g / cm 3 Below, more preferably 0.3 g / cm 3 Above and 1.0g / cm 3 If it is smaller than the above range, the mechanical properties may be reduced, and if it is larger than the above range, the lightweight effect and air permeability may become insufficient. Here, Wc is the mass [g] of the sample obtained by cutting only the cell wall from the core material divided by the volume [cm 3 ] is the arithmetic mean of the specific gravity measured by 5 randomly selected samples.
[0038] The average fiber orientation angle in the out-of-plane direction of the cell wall of the fiber (Cf) is preferably 0 to 10 degrees. By orienting the fibers in this range, the compression properties of the core material and the skin-core structure can be improved. The average fiber orientation angle in the out-of-plane direction of the fiber (Cf) can be measured based on observation of a cross section (zy plane) perpendicular to the plane direction of the cell wall. Fig.11The fiber orientation in the plane direction of the cell wall of the present invention is shown in FIG. Fig.11 (a)) and vertical section ( Fig.11 (b)) is an example. Fig.11 In (a), focusing on fibers 2a to 2d, it can be confirmed by observing their cross sections that Fig.11 (b) is a cross section of elliptical fibers 2a to 2d as shown. In the case where the fiber is not elliptical but circular, it means that the fiber is oriented in the x direction (orthogonal to the y axis) and is not inclined in the z direction. At this time, the angle between the major axis of the ellipse in the elliptical shape of the fiber cross section and the z axis is roughly the same as the out-of-plane direction of the fiber relative to the cell wall. Therefore, the cell wall is cut out, and the major axis of the ellipse is calculated for any 600 fibers based on the cross section perpendicular to the surface direction of the cell wall, and the arithmetic mean of the absolute value of the angle formed with the z axis is taken as the average fiber orientation angle in the out-of-plane direction relative to the cell wall.
[0039] The unit shape of the core material of the present invention (the cross-sectional shape perpendicular to the axial direction of the columnar unit) is a polygon such as a triangle, a quadrilateral, a hexagon, a circle, an ellipse, etc., and is not particularly limited, but from the perspective of impact resistance, it is preferably a regular hexagon, that is, a honeycomb structure. In the case where the shape of the unit is a regular hexagon, the length of one side of the regular hexagon is usually 3mm to 20mm, but from the perspective of the contact point with the adhesive, the length of one side of the regular hexagon is preferably 3mm to 10mm, and more preferably 3mm to 7mm. In addition, in the case where a unit aggregate is composed of units having a plurality of polygonal unit shapes, and in the case where unit shapes of different sizes are combined, the characteristic deviation in the core material can be reduced, and the shape-forming property corresponding to the skin-core structure of a complex shape can be given, so it is preferred. As a combination of polygons, for example, a truncated icosahedron formed by combining pentagons and hexagons, a curved surface shape using a part thereof, etc., can be cited, so that the core material opening surface can be a curved surface shape such as a spherical shape, so it is preferred.
[0040] The core material of the present invention can be manufactured, for example, by using a sheet substrate (B) obtained by impregnating a fiber felt (A) formed by fibers (Cf) with a resin (Cr) as a base material, using a known stretching method or corrugation method. In the stretching method, a bonding material such as an adhesive is applied to the sheet substrate (B) in a strip-like shape, and a plurality of sheets of the applied bonding material are overlapped in a positional relationship of half a pitch, and then heated and pressurized for bonding, and stretched (stretched) in the overlapping direction, thereby obtaining a core material. In the corrugation method, the sheet substrate (B) is first bent into a corrugated board, and a plurality of corrugated boards are stacked into a block in a positional relationship of half a pitch of each wave, with bonding materials such as an adhesive interposed in each valley and top, and then heated and pressurized for bonding, thereby obtaining a core material.
[0041] The fiber mat (A) is preferably composed of discontinuous fibers (Cf). As a method for manufacturing a fiber mat, for example, there is a method for manufacturing a fiber mat by pre-dispersing the fibers (Cf) into a bundle and / or a roughly single fiber shape. As a method for manufacturing a fiber mat, dry processes such as an air-laid method in which the fibers (Cf) are dispersed and flaked by air flow, a combing method in which the fibers (Cf) are mechanically combed while trimming the shape and flakes, and a wet process based on the Radlite method in which the fibers (Cf) are stirred in water and papermaking is performed. As a means for making the fibers (Cf) closer to a single fiber shape, in a dry process, a method of setting a fiber opening rod, a method of further vibrating the fiber opening rod, a method of further refining the holes of a carding machine, a method of adjusting the rotation speed of a carding machine, etc. can be exemplified. In a wet process, a method of adjusting the stirring conditions of the fibers (Cf), a method of thinning the fiber concentration of a dispersion, a method of adjusting the viscosity of a dispersion, a method of suppressing eddy currents when conveying a dispersion, etc. can be exemplified. In particular, the fiber mat is preferably manufactured by a wet method, and the proportion of the fiber (Cf) in the fiber mat can be easily adjusted by adjusting the concentration of the input fiber, the flow rate (flow rate) of the dispersion, and the speed of the mesh belt conveyor. For example, by slowing down the speed of the mesh belt conveyor compared to the flow rate of the dispersion, the orientation of the fibers in the obtained fiber mat is not easy to be in the pulling direction, and a fluffy fiber mat can be manufactured. The fiber mat can be composed of a fiber (Cf) monomer, or the fiber (Cf) can be mixed with a powder-shaped or fiber-shaped matrix resin component, or the fiber (Cf) can be mixed with an organic compound or an inorganic compound, or the fibers (Cf) can be filled with a resin component.
[0042] Furthermore, the fiber felt (A) can be impregnated with a resin (Cr) to prepare a sheet substrate (B) to be used as a base material for the core material. As a method for manufacturing a sheet substrate, from the viewpoint of ease of manufacturing, the following method is preferred: a resin (Cr) heated to a temperature above the melting or softening temperature is applied to the fiber felt, and pressure is applied to impregnate the fiber felt. Specifically, a method of melt-impregnating a laminated material provided with the resin (Cr) from both sides of the fiber felt in the thickness direction can be preferably exemplified. On the other hand, in the method of melting or softening the resin, the following method can be exemplified: in addition to heating, the resin component is diluted with a solvent soluble in the resin component to reduce the apparent viscosity, and then the resin is infiltrated into the fiber felt, and then only the solvent is removed by volatilization or evaporation.
[0043] As equipment for implementing the above methods, a compression molding machine and a double belt press machine can be preferably used. In the case of a batch method, the former is used, and an intermittent pressurizing system formed by connecting two or more equipments for heating and cooling in parallel can achieve an improvement in productivity. In the case of a continuous method, the latter is used, and continuous processing can be easily performed, so the continuous productivity is excellent.
[0044] Figure 3 This is a schematic diagram showing an embodiment of the fiber felt (A) contained in the sheet substrate (B) and the resin (Cr) impregnated therein. In this embodiment, the fiber felt (A) is a non-woven fabric composed of discontinuous fibers (Cf) 2. The fiber felt (A) impregnated with the resin (Cr) 3 and in a compressed state is released from the compressed state by melting or softening the resin (Cr) 3, thereby causing rebound. Figure 4 As shown, by forming voids 5 due to the rebound, a porous structure composed of fibers (Cf) 2 covered with resin (Cr) 3 can be formed at any position of the cell wall.
[0045] In order for the fiber mat (A) to exhibit rebound properties, the fibers therein are preferably dispersed in a single fiber shape. If the fibers are dispersed in a single fiber shape, the number of contact points between the fibers increases, so that the fiber mat (A) becomes a further three-dimensional structure and becomes easy to rebound.
[0046] As the fiber (Cf) used in the core material of the present invention, for example, carbon fiber, glass fiber, aramid fiber, alumina fiber, silicon carbide fiber, boron fiber, metal fiber, natural fiber, mineral fiber, etc. can be used, and they can be used 1 or more than 2 kinds. Among them, from the viewpoint of specific strength, high specific stiffness, and lightweight effect, it is preferred to use carbon fibers of PAN series, asphalt series, rayon series, etc. In addition, from the viewpoint of improving the economy of the obtained molded product, glass fiber can be preferably used, and from the viewpoint of the balance between mechanical properties and economy, carbon fiber and glass fiber are preferably used in combination. In addition, from the viewpoint of improving the impact absorbency and shapeability of the obtained molded product, aramid fiber can be preferably used, especially from the viewpoint of the balance between mechanical properties and impact absorbency, carbon fiber and aramid fiber are also preferably used in combination. In addition, from the viewpoint of improving the conductivity of the obtained molded product, fibers coated with metals such as nickel, copper, and ytterbium can also be used.
[0047] As the fiber (Cf), it is preferred to use a fiber having a tensile elastic modulus of 100 GPa or more. By using a fiber having a tensile elastic modulus of 100 GPa or more for the fiber felt (A), it becomes easy to rebound, which is beneficial to the formation of a porous structure. As fibers having a tensile elastic modulus of 100 GPa or more, for example, para-aramid fibers, boron fibers, carbon fibers, and graphite fibers can be cited, among which carbon fibers having no water absorption problem and excellent strength and elastic modulus are preferably used.
[0048] The tensile modulus of the carbon fiber used as the fiber (Cf) of the present invention is preferably in the range of 200 to 600 GPa. The tensile modulus of carbon fiber is affected by the crystallinity of the graphite structure constituting the carbon fiber, and the higher the crystallinity, the higher the elastic modulus. In addition, the higher the crystallinity, the higher the conductivity. If the tensile modulus is in this range, the conductivity, rigidity, and strength of the fiber-reinforced composite material are all balanced at a high level, so it is preferred. A more preferred elastic modulus is in the range of 230 to 400 GPa, and further preferably in the range of 260 to 370 GPa. Here, the tensile modulus of the fiber is a value measured in accordance with JIS R7601-2006. Commercially available products of carbon fiber include "TORECA (registered trademark)" T800S-24K, "TORECA (registered trademark)" T300-3K, "TORECA (registered trademark)" M55J-6K, and "TORECA (registered trademark)" T700S-12K (all manufactured by Toray Industries, Inc.).
[0049] The fiber (Cf) contained in the fiber-reinforced composite material constituting the core material of the present invention is a discontinuous fiber, more specifically, the number average fiber length is preferably 1 mm or more and 50 mm or less, and the number average fiber length is more preferably 3 mm or more and 20 mm or less, and more preferably 4 mm or more and 10 mm or less. By setting it to the above range, it is easy to expand the interval between the fibers (Cf) and it is easy to control the formation of the porous structure, so it is preferred. In addition, the fibers (Cf) are randomly dispersed, so that the concentration of the fibers (Cf) and the resin (Cr) in the porous structure is uneven, and an isotropic porous structure with excellent properties can be obtained, so it is a preferred mode.
[0050] In addition, the fibers (Cf) of the cell walls of the core material are preferably composed of 0 to 50% by mass of fibers having a fiber length greater than 10 mm, 50 to 100% by mass of fibers having a fiber length of 2 to 10 mm, and 0 to 50% by mass of fibers having a fiber length less than 2 mm. If the fibers longer than 10 mm account for more than 50% by mass, the thickness expansion in the molding process may become large, thereby impairing operability. In addition, if the fibers less than 2 mm account for more than 50% by mass, the mechanical properties of the obtained core material and the skin-core structure may be reduced. Moreover, the fiber felt (A) or the sheet substrate (B) obtained by impregnating the fiber felt with a resin may not have sufficient strength, thereby impairing moldability. From these viewpoints, it is preferably composed of 80 to 100% by mass of fibers having a fiber length of 3 to 8 mm, and more preferably composed of fibers having a fiber length distribution having at least two peaks, one peak in the range of 5 to 10 mm in fiber length and the other peak in the range of 2 to 5 mm. By making the distribution of fiber length within a more preferred range, it is possible to use fibers that ensure mechanical properties and fibers that ensure operability of preforming from the lamination process to the molding process, and it is easy to achieve both properties at the same time. It should be noted that the mass ratio of the fibers here represents the ratio of the number average fiber length when the fibers are recorded as 100%.
[0051] The average pore diameter of the porous structure measured by the mercury intrusion method is preferably 1 μm or more and 200 μm or less, and more preferably 10 μm or more and 100 μm or less. If the average pore diameter is too small, the lightweight effect is sometimes insufficient, and if the average pore diameter is too large, the mechanical properties are sometimes reduced. The so-called mercury intrusion method is a method for measuring the pore diameter using a mercury intrusion porosimeter. Mercury can be injected into the sample under high pressure, and the pore diameter can be calculated from the applied pressure and the amount of mercury injected. The average pore diameter is a value that can be calculated by the following formula (1).
[0052] (Average pore diameter)=4×(pore volume) / (specific surface area)···Formula (1).
[0053] The resin (Cr) contained in the fiber-reinforced composite material constituting the core material of the present invention can be a thermoplastic resin or a thermosetting resin. As a thermoplastic resin, for example, polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyolefins such as polyethylene, polypropylene, polybutene, and modified polypropylene, polyoxymethylene, polyamide 6, polyamide 66, polyamides such as polycarbonate, polymethyl methacrylate, polyvinyl chloride, polyphenylene sulfide, polyphenylene ether, modified polyphenylene ether, polyimide, polyamide-imide, polyetherimide, polysulfone, modified polysulfone, polyethersulfone, polyketone, polyetherketone, polyetheretherketone, polyetherketoneketone, polyarylene etherketone, polyarylate, polyethernitrile, phenoxy resin, etc. can be cited. In addition, these thermoplastic resins can also be copolymers, modified materials, and / or resins obtained by blending two or more resins. Among them, at least one thermoplastic resin selected from the group consisting of polyarylene sulfide, polyetherimide, polyethersulfone, polysulfone, and polyarylene ether ketone is more preferred in view of heat resistance and mechanical properties.
[0054] Examples of the thermosetting resin include unsaturated polyester resins, vinyl ester resins, epoxy resins, phenolic resins, urea resins, melamine resins, thermosetting polyimide resins, BT resins, cyanate ester resins, bismaleimide resins, benzophenone resins, Azine resin or a copolymer thereof, a modified product thereof and / or a resin obtained by blending two or more resins, etc. Among them, epoxy resin, phenolic resin, benzophenone resin, At least one thermosetting resin selected from the group consisting of oxazine resin, BT resin, cyanate ester resin, bismaleimide resin, and polyimide resin.
[0055] In addition, the resin (Cr) contained in the fiber-reinforced composite material constituting the core material of the present invention may contain other fillers and additives as appropriate within the scope of not impairing the purpose of the present invention according to the application, etc. Examples thereof include inorganic fillers, flame retardants, conductivity imparting agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, vibration damping agents, antibacterial agents, insect repellents, deodorants, anti-coloring agents, heat stabilizers, mold release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foaming agents, coupling agents, etc.
[0056] As for the resin (Cr) and the resin (Sr) used in the skin-core structure of the present invention, from the viewpoint of improving the flame retardancy of the structure, the LOI value (limiting oxygen index) is preferably 26% or more, and more preferably 30% or more. The LOI value can be measured, for example, in accordance with JIS K7201-2 (2007). Examples of resins having an LOI value of 26% or more include polyarylene sulfide resins, polyetherimide resins, polyethersulfone resins, polyarylene ether ketone resins, polyimide resins, and phenolic resins. The above range of LOI values can be achieved by adding a flame retardant to the resin. For example, a resin composition obtained by adding a flame retardant to an epoxy resin is preferred because it can obtain a high bonding strength between the skin material and the core material. Among the flame retardants, phosphorus-based flame retardants, nitrogen-based flame retardants, and inorganic flame retardants are preferably used.
[0057] Regarding the flammability of the skin-core structure involved in the present invention, the burning time can be measured according to FAR25.853 Appendix F. In addition, the quality related to its burning time can be judged based on Advisory Circular (AC) 25.853-1a (1) i "Flammability Requirements for Aircraft Seat Cushions" issued by the Federal Aviation Administration. The burning time of the structure after the ignition source is extinguished is preferably less than 30 seconds, and preferably less than 15 seconds. If the burning time of the structure is longer than 30 seconds, it means that it is easy to burn, which is not ideal from a safety point of view. Regarding the shortness of the burning time of the structure, the shorter the burning time, the better the flammability, so there is no limit. In the above-mentioned FAR25.853 Appendix F of the Federal Aviation Regulations (FAR), the test piece is fixed in a vertical state with the long side, and a burner is used to spray flames from directly below the center of the bottom edge of the test piece to make it burn, thereby measuring and evaluating. In the evaluation method, the distance between the burner and the test piece was set to 19 mm, and after the test piece was baked for 60 seconds, the time for the flame to be emitted from the test piece was measured as the burning time.
[0058] <Skin-core structure>
[0059] As described above, the core material of the present invention is preferably used in the form of a skin-core structure obtained by bonding a skin material to at least one side, preferably both sides, of the core material opening surface of the columnar unit opening. There is no particular limitation on the method of bonding the skin material to the core material, and examples include bonding using an adhesive, thermal fusion bonding, and the like. For example, an adhesive sheet and a skin material or a prepreg blank as a precursor thereof may be arranged on both sides of the core material opening surface, and bonded to the core material while being heated and cured. From the viewpoint of the lightness of the skin-core structure, it is more preferred to directly bond the core material to the skin material without using an adhesive film, and preferably the skin material is arranged / laminated in a manner that the skin material is in contact with the core material opening surface, and is heated and pressurized to bond them together. In addition, the bonding process is not particularly limited, and molding may be performed by vacuum bag molding, autoclave molding, press molding, and the like.
[0060] The skin material preferably contains a resin. When the resin (Sr) of the skin material is a thermosetting resin, it is preferred to perform so-called co-curing, that is, the uncured prepreg is arranged in contact with the open surface of the core material, and is bonded while being heated and pressurized. Compared with the so-called co-bonding (co-bond) in which the skin material is cured in advance and then bonded to the core material using an adhesive, the molding times are small, so it is advantageous in terms of molding cost and can achieve molding in a short time. In addition, by co-curing the skin material, the fiber (Cf) can enter the skin material, so it can be firmly bonded.
[0061] When the resin (Sr) of the skin material is a thermoplastic resin, it is preferred to heat and pressurize the skin material at a temperature above the melting point of the resin (Sr) while bonding it to the core material. By co-curing the skin material, the fiber (Cf) can easily enter the resin (Sr) of the skin material, thereby forming a strong bond between the skin material and the core material. In addition, when an adhesive is used to bond the core material of the skin-core structure to the skin material, it is preferred that a portion of the resin (Sr) constituting the skin material and / or the resin (Ar) contained in the adhesive flows into the porous structure of the core material.
[0062] In the skin-core structure of the present invention, it is preferred that a portion of the discontinuous fibers (Cf) contained in the cell walls of the core material penetrate into the skin material. The state in which the fibers (Cf) penetrate into the skin material is Fig.10 That is, the fiber (Cf) 2 in contact with both the resin (Sr) 17 and the resin (Cr) 3 exists across the interface layer formed by the resin (Sr) 17 of the skin material and the resin (Cr) 3 of the core material. The penetration distance of the fiber (Cf) 2 into the skin material ( Fig.10The penetration distance 18 of the fiber (Cf) 2e into the skin material is not limited as long as it does not impair the effect of the present invention, but the maximum penetration distance of the fiber (Cf) 2 into the skin material is preferably greater than 5 μm, and more preferably greater than 10 μm. The penetration distance of the fiber (Cf) 2 into the skin material is based on a certain fiber (Cf) 2 that penetrates into the skin material, and is defined as the shortest distance from an imaginary plane (a horizontal plane parallel to the skin material) existing at the depth of the front end of the fiber (Cf) 2 that penetrates into the resin (Sr) 17 side of the skin material to the boundary between the resin (Sr) 17 of the skin material and the resin (Cr) 3 of the core material, Fig.10 In the case of the fiber (Cf) 2e in the skin material, it is represented by the distance marked with reference numeral 18. Then, the distance of the maximum value among the measured invasion distances is taken as the maximum invasion distance. Specifically, the maximum invasion distance of the fiber (Cf) 2 into the skin material can be measured as described below. Cut out the bonding part of the skin material and the core material of the structure, use a laser microscope to take pictures of any 10 parts (10 images) at a magnification of 1000 times for the cross-section in the thickness direction, and based on the obtained images, calculate the invasion distance of each single fiber of the fiber (Cf) entering the skin material, and take the maximum value as the maximum invasion distance.
[0063] For the structure thus bonded, the average peeling moment M (climbing roller peeling strength) of the skin material and the core material measured according to ASTM D1781 (2004) is preferably 30 N·m / m or more, more preferably 35 N·m / m or more. By having a climbing roller peeling strength of 30 N·m / m or more, it can withstand high loads and exert a lightweight effect, so it is suitable as a structure.
[0064] From the perspective of bonding the skin material to the core material by heat welding, the heat resistance temperature Ts of the resin (Sr) constituting the above-mentioned skin material and the heat resistance temperature Tc of the resin (Cr) constituting the core material preferably satisfy Ts≤Tc. The so-called heat resistance temperature here refers to the melting point in the case of crystalline resins and the glass transition temperature in the case of amorphous resins and thermosetting resins. Since Ts≤Tc, it is easy to maintain the shape of the core material, it is easy to obtain a molded body with good quality, or it can be molded in a short time. In addition, it is also easy to bond the skin material to the core material by heat welding, which simplifies the molding process, so it is preferred. Preferably, Tc is higher than Ts by more than 10°C, and more preferably, Tc is higher than Ts by more than 20°C.
[0065] When a porous structure is formed in the cell wall, the core material having the porous structure formed therein in advance may be prepared and then the skin material may be bonded, or the porous structure may be formed while bonding the skin material. As the latter method, for example, the core material may be bonded to the skin material by heating and pressurizing at a temperature above the melting point or softening temperature of the resin (Cr), thereby causing the fiber (Cf) to rebound, and bonding may be performed while forming the porous structure at the bonding portion between the core material and the skin material.
[0066] In a preferred embodiment, the skin material is a fiber-reinforced composite material comprising a fiber (Sf) and a resin (Sr). In this case, the fiber-reinforced composite material as a skin material is preferably formed by a prepreg (D), which is obtained by impregnating a resin (Sr) in a reinforcing fiber substrate (C) in which the fiber (Sf) is a reinforcing fiber. Regarding the morphology of the reinforcing fiber, its shape and arrangement are not limited, and it can be, for example, a single direction, a random direction, a sheet, a felt, a fabric, or a braid. Among them, a two-dimensional fabric can be preferably used. As a fabric structure, it is not particularly limited, but preferably a fabric such as a plain weave, a twill weave, a gauze weave, and a satin weave. In particular, a plain weave structure is suitable from the point of view of easy manufacture of a thin molded body. The woven yarn of the fabric is composed of a fiber bundle, and the number of filaments in a fiber bundle is preferably in the range of 2500 to 50000. If there are less than 2500, the fiber arrangement is easy to be tortuous, which is easy to become the cause of reduced strength. In addition, if the number of the fibers is more than 50,000, it is difficult to impregnate the prepreg with the resin during production or molding. A more preferred range is 2,800 to 25,000. From the viewpoint of improving the surface smoothness of the skin-core structure, a fiber bundle having 5,000 or more filaments is particularly preferred.
[0067] The fiber (Sf) of the prepreg (D) preferably has a weight per unit area of 150 to 550 g / m 2 . Thus, a leather material with excellent mechanical strength can be obtained. If the unit area weight of the fiber (Sf) is less than 150g / m 2 , the mechanical strength is sometimes insufficient. If the unit area weight of the fiber (Sf) is greater than 550g / m 2 The weight per unit area of the fiber (Sf) is more preferably 170 to 500 g / m 2 In addition, if the mass fraction of the fiber (Sf) in the prepreg is less than 40 mass %, the rigidity of the obtained skin material may be insufficient, and if the mass fraction of the fiber (Sf) in the prepreg is greater than 85 mass %, voids may be easily generated in the obtained skin material.
[0068] As specific examples of the fiber (Sf) used in the present invention, carbon fiber, graphite fiber, aramid fiber, silicon carbide fiber, alumina fiber, boron fiber, tungsten carbide fiber, glass fiber, etc. can be cited. These fibers can also be used in combination. Among them, carbon fiber and graphite fiber, which have good specific strength and specific elastic modulus and are considered to greatly contribute to lightweighting, are good for the present invention. Carbon fiber and graphite fiber can use all kinds of carbon fiber and graphite fiber according to the purpose. From the perspective of the original tensile strength of the fiber and the high impact resistance when the skin-core structure is made, it is preferred to use a fiber with a bundle strength of 3000MPa or more and 7500MPa or less and an elastic modulus of 200GPa or more and 600GPa or less in the bundle tensile test. It should be noted that the so-called bundle tensile test refers to the following test: a matrix resin of the following composition is impregnated into a bundle of carbon fibers, and after curing for 35 minutes at a temperature of 130°C, it is carried out based on JIS R7601 (2006).
[0069] The number of filaments of the carbon fiber used as the fiber (Sf) used in the present invention is preferably 1000 to 100000, and more preferably 3000 to 50000. If the number of carbon fiber filaments is less than 1000, the operation of prepreg becomes complicated, and if the number of carbon fiber filaments is more than 100000, it is difficult to impregnate the filaments with resin, and impregnation failure may occur.
[0070] The fiber (Sf) used in the present invention preferably has a tensile modulus E of 200 GPa or more and a breaking strain strength ε of 40 MPa or more. When using fibers with a high tensile modulus, high strength can be obtained in the climbing roller peeling method, which is one of the evaluation methods for the adhesion between the skin material and the core material. It should be noted that the so-called breaking strain strength ε here is based on the following formula: ε = σ, using the tensile strength (σ: MPa) and elastic modulus (E: MPa) measured in accordance with JIS-R7601 (2006): 2 As specific examples of such high-strength and high-elongation carbon fibers, for example, commercially available products of carbon fibers include "Toreka (registered trademark)" T800G-24K, "Toreka (registered trademark)" T800S-24K, "Toreka (registered trademark)" T700G-24K, "Toreka (registered trademark)" T700S-24K, "Toreka (registered trademark)" T300-3K, and "Toreka (registered trademark)" T1100G-24K (all manufactured by Toreka Co., Ltd.).
[0071] The resin (Sr) contained in the leather material can be a thermoplastic resin or a thermosetting resin. As the thermoplastic resin, for example, polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyolefins such as polyethylene, polypropylene, polybutene, and modified polypropylene, polyoxymethylene, polyamide 6, polyamide 66, polyamides such as polycarbonate, polymethyl methacrylate, polyvinyl chloride, polyphenylene sulfide, polyphenylene ether, modified polyphenylene ether, polyimide, polyamide-imide, polyetherimide, polysulfone, modified polysulfone, polyethersulfone, polyketone, polyetherketone, polyetheretherketone, polyetherketoneketone, polyarylene etherketone, polyarylate, polyethernitrile, phenoxy resin, etc. can be cited. In addition, these thermoplastic resins can also be copolymers, modified products, and / or resins obtained by blending two or more resins. Among them, at least one thermoplastic resin selected from the group consisting of polyarylene sulfide, polyetherimide, polyethersulfone, polysulfone, and polyarylene ether ketone is more preferred in view of heat resistance and mechanical properties.
[0072] Examples of the thermosetting resin include unsaturated polyester resins, vinyl ester resins, epoxy resins, phenolic resins, urea resins, melamine resins, thermosetting polyimide resins, cyanate ester resins, BT resins, bismaleimide resins, benzophenone resins, Azine resin or a copolymer thereof, a modified product thereof and / or a resin obtained by blending two or more resins, etc. Among them, epoxy resin, phenolic resin, benzophenone resin, At least one thermosetting resin selected from the group consisting of oxazine resin, BT resin, cyanate ester resin, bismaleimide resin, and polyimide resin.
[0073] In addition, the resin (Sr) contained in the leather material of the present invention may contain other fillers and additives as appropriate within the scope of not impairing the purpose of the present invention according to the application, etc. Examples thereof include inorganic fillers, flame retardants, conductivity imparting agents, crystal nucleating agents, ultraviolet absorbers, antioxidants, vibration damping agents, antibacterial agents, insect repellents, deodorants, anti-coloring agents, heat stabilizers, mold release agents, antistatic agents, plasticizers, lubricants, colorants, pigments, dyes, foaming agents, foaming agents, coupling agents, etc.
[0074] Example
[0075] The materials used in Examples and Comparative Examples are as follows.
[0076] [Carbon Fiber 1]
[0077] A copolymer containing polyacrylonitrile as a main component was spun, calcined and surface-oxidized to obtain a continuous carbon fiber having a total number of 12,000 single fibers. The properties of the continuous carbon fiber are shown below.
[0078] Single fiber diameter: 7μm
[0079] Specific gravity: 1.8
[0080] Tensile strength: 4600MPa
[0081] Tensile elastic modulus: 220GPa
[0082] [PEKK resin]
[0083] A polyetherketoneketone resin (KEPSTAN (registered trademark) 7002 manufactured by Alkama Co., Ltd.) having a unit weight of 60 g / m 2 of resin film.
[0084] [PPS resin]
[0085] A polyphenylene sulfide resin (Toray Industries, Inc. "Toray" (registered trademark) M2888) having a unit area weight of 60 g / m 2 of resin film.
[0086] [PEI resin]
[0087] The weight per unit area of the polyetherimide resin (ULTEM (registered trademark) 1000 manufactured by SABIC) was 60 g / m 2 of resin film.
[0088] [Carbon fiber felt 1]
[0089] The carbon fiber 1 was cut into 6 mm pieces using a machine chuck cutter to obtain chopped carbon fibers. A dispersion having a concentration of 0.1% by mass was prepared from water and a surfactant (polyoxyethylene lauryl ether (trade name) manufactured by Nakalai Tech Co., Ltd.). The dispersion and the chopped carbon fibers were used to prepare the chopped carbon fibers. Figure 5 The carbon fiber felt manufacturing device shown is used to manufacture the carbon fiber felt. Figure 5 The manufacturing device shown has a cylindrical container with a diameter of 1000 mm and an open stopcock at the bottom of the container as a dispersion tank, and a linear conveying portion (inclined at an angle of 30°) connecting the dispersion tank and the papermaking tank. A stirrer is attached to the opening on the upper surface of the dispersion tank, and chopped carbon fibers and a dispersion liquid (dispersion medium) can be added from the opening. The papermaking tank is a tank having a mesh belt conveyor with a papermaking surface with a width of 500 mm at the bottom, and the mesh belt conveyor is connected to a conveyor capable of transporting a carbon fiber substrate (papermaking substrate). Papermaking is carried out by setting the carbon fiber concentration in the dispersion liquid to 0.05% by mass. The papermade carbon fiber substrate is dried in a drying furnace at 200°C for 30 minutes to obtain a carbon fiber felt 1. The obtained unit area weight is 40g / m 2 .
[0090] [Sheet base material 1]
[0091] A carbon fiber felt 1 as a carbon fiber felt and a PEKK resin as a resin film are arranged in the order of [resin film / carbon fiber felt / resin film] to prepare a laminate. Then, the following steps (I) to (IV) are performed to obtain a sheet base material 1.
[0092] (I) The laminate was placed in a cavity of a press-molding mold preheated to 250° C., and the mold was closed and maintained for 120 seconds.
[0093] (II) Next, a pressure of 5 MPa was applied, and the temperature was raised to 350° C. and maintained for 10 minutes.
[0094] (III) The cavity temperature was cooled to 50° C. while maintaining the pressure.
[0095] (IV) Open the mold and take out the sheet substrate.
[0096] [Sheet base material 2]
[0097] A carbon fiber felt 1 as a carbon fiber felt and a PPS resin as a resin film are arranged in the order of [resin film / carbon fiber felt / resin film] to form a laminate. Then, the following steps (I) to (IV) are performed to obtain a sheet base material 2.
[0098] (I) The laminate was placed in a cavity of a press-molding mold preheated to 200° C., and the mold was closed and maintained for 120 seconds.
[0099] (II) Next, a pressure of 5 MPa was applied, and the temperature was raised to 300° C. and maintained for 10 minutes.
[0100] (III) The cavity temperature was cooled to 50° C. while maintaining the pressure.
[0101] (IV) Open the mold and take out the sheet substrate.
[0102] [Sheet base material 3]
[0103] A carbon fiber felt 1 as a carbon fiber felt and a PEI resin as a resin film are arranged in the order of [resin film / carbon fiber felt / resin film] to form a laminate. Then, the following steps (I) to (IV) are performed to obtain a sheet base material 3.
[0104] (I) The laminate was placed in a cavity of a press-molding mold preheated to 250° C., and the mold was closed and maintained for 120 seconds.
[0105] (II) Next, a pressure of 5 MPa was applied, and the temperature was raised to 350° C. and maintained for 10 minutes.
[0106] (III) The cavity temperature was cooled to 50° C. while maintaining the pressure.
[0107] (IV) Open the mold and take out the sheet substrate.
[0108] [Honeycomb core material 1]
[0109] The honeycomb core material 1 is made by a corrugation method using a sheet substrate 1 as a base material. First, the base material is bent into a corrugated plate, and a plurality of corrugated plates are stacked into blocks with adhesive interposed at each valley and top at a positional relationship of half the spacing of the waves, and then heated and pressurized to bond them together, thereby obtaining a honeycomb core material precursor. Next, the open end of the honeycomb core material precursor is heated to 320°C using a press, thereby obtaining a honeycomb core material 1 having a porous structure at the open end of the cell wall (the thickness of the core material (the axial direction of the cell wall) is 12.7 mm, and the mass per unit volume is 45 kg / m 3 ).
[0110] [Honeycomb core material 2]
[0111] The honeycomb core material 2 is made by the corrugation method using the sheet substrate 1 as the base material. First, the base material is heated to 320°C and bent into a corrugated plate, thereby making a corrugated plate with a porous structure. The multiple corrugated plates are stacked into a block with adhesive placed in each valley and top at a positional relationship of half the spacing of each wave, and then heated and pressed to bond them together, thereby obtaining a honeycomb core material 2 with a porous structure in the cell wall (the thickness of the core material is 12.7 mm, and the mass per unit volume is 45 kg / m 3 ).
[0112] [Honeycomb core material 3]
[0113] The honeycomb core material 3 is made by the corrugation method using the sheet substrate 2 as the base material. First, the base material is heated to 280°C and bent into a corrugated plate, thereby making a corrugated plate with a porous structure. The multiple corrugated plates are stacked into a block with adhesive placed in each valley and top at a positional relationship of half the spacing of each wave, and then heated and pressed to bond them together, thereby making a honeycomb core material 3 with a porous structure in the cell wall (the thickness of the core material is 12.7 mm, and the mass per unit volume is 50 kg / m 3 ).
[0114] [Honeycomb core material 4]
[0115] Aramid honeycomb (Showa Aircraft Industry Co., Ltd., model: SAH1 / 8-3.0) was used, the core material thickness was 12.7 mm, and the mass per unit volume was 48 kg / m 3 ) as honeycomb core material 4.
[0116] [Honeycomb core material 5]
[0117] The sheet substrate 1 is used as the base material and is manufactured by the corrugation method. First, the base material is heated to 320°C and bent into a corrugated plate, thereby manufacturing a corrugated plate having a porous structure. The thickness of the corrugated plate is made thinner than the core material 2, thereby adjusting the average pore diameter and density of the porous structure. The plurality of corrugated plates are stacked into blocks with adhesive interposed at each valley and top in a positional relationship of half the spacing of each wave, and then heated and pressurized to bond them together, thereby obtaining a honeycomb core material 5 having a porous structure in the unit wall (the thickness of the core material is 12.7 mm, and the mass per unit volume is 50 kg / m 3 ).
[0118] [Honeycomb core material 6]
[0119] The sheet substrate 3 is used as the base material and is made by the corrugation method. First, the base material is heated to 350°C and bent into a corrugated plate, thereby making a corrugated plate with a porous structure. The multiple corrugated plates are stacked into a block with adhesive interposed between the valleys and the top, and then heated and pressed to bond them together, thereby making a honeycomb core material 6 with a porous structure in the cell wall (the thickness of the core material is 12.7 mm, and the mass per unit volume is 50 kg / m 3 ).
[0120] [Prepreg 1 used for leather material]
[0121] Using a kneader, polyethersulfone ("Sumicon (registered trademark)" PES manufactured by Sumitomo Chemical Co., Ltd. 5003P: 5 parts by mass) is heated and kneaded until the epoxy resin ("Armantec (Registered Trademark)" manufactured by Harmon Chemical Co., Ltd. MY721: 40 parts by mass, "Estron (registered trademark)" manufactured by Semantec Co., Ltd. 828: 35 parts by mass, "Estron (registered trademark)" After the polyethersulfone was uniformly dissolved in the mixture (1001 parts by mass of "Amiran (registered trademark)" manufactured by Toray Industries, Ltd.: 13 parts by mass) and the curing agent (154 parts by mass of "Epicoat (registered trademark)" manufactured by Seika Co., Ltd.: 25 parts by mass), the polyamide particles (13 parts by mass of "Amiran (registered trademark)" SP-500 manufactured by Toray Industries, Ltd.: 13 parts by mass) and the curing agent (154 parts by mass of "Seika Curia (registered trademark)" manufactured by Seika Co., Ltd.) were mixed with a kneader. )" S: 36 parts by mass are kneaded to prepare an uncured epoxy resin composition, from which an epoxy resin film is prepared using a doctor blade coater. Next, it is superimposed on both sides of the carbon fiber fabric, and a hot roller is used to impregnate the resin composition while heating and pressurizing it to prepare a prepreg blank 1 having a fiber volume content of 60%. It should be noted that as the carbon fiber fabric, a plain fabric CF6273H (fiber weight per unit area of 193 g / m) made of carbon fiber "トレカ (registered trademark)" T700G-12K manufactured by Toray Co., Ltd. (the number of fibers is 12,000, the tensile strength is 4.9 GPa, the tensile elastic modulus is 240 GPa, and the tensile elongation is 2.1%) is used. 2 ).
[0122] The evaluation methods of the structures, physical properties, etc. in each Example / Comparative Example are as follows.
[0123] [Evaluation of average pore diameter]
[0124] As a mercury intrusion porosimeter, Autopore IV9510 manufactured by Micromeritics was used to measure the pore diameter within a mercury intrusion pressure range of 4 kPa to 400 MPa. The average pore diameter was determined by using the formula (1) from the pore volume and specific surface area obtained as the measurement results.
[0125] (Average pore diameter) = 4 × (pore volume) / (specific surface area) Formula (1)
[0126] [Evaluation of the mass W per unit volume of the cell wall]
[0127] The mass W per unit volume of the cell wall is obtained by cutting the cell wall from the core material and dividing the sample mass [g] by the volume [cm 3The value obtained by the arithmetic mean of the values measured by 5 randomly selected samples can be obtained. In order to remove the influence of the adhesive between the cell walls, a portion of the cell wall as a single sheet is cut out as a sample.
[0128] [Evaluation of the Area Ratio Occupied by Cell Walls in the Core Material Opening Surface (Adhesion Area Ratio)]
[0129] The opening surface of the core material was photographed using an optical microscope, and a 50 mm×50 mm area randomly selected on the photograph was processed using an image processing device (CV-3000 manufactured by KEYENCE) to evaluate the area ratio (bonding area ratio) occupied by the cell walls in the opening surface.
[0130] [Sandwich structure]
[0131] A sandwich structure in which a skin material was bonded to a honeycomb core material (hereinafter referred to as a "honeycomb sandwich structure") was produced by the following steps (1) and (2).
[0132] (1) Sample stacking
[0133] The prepreg 1 is used to form a symmetrical stacking structure of two layers (±45°) / (0° / 90°) above and below the core opening surface of each honeycomb core (the outermost layer is ±45° to the honeycomb core).
[0134] (2) Sample molding
[0135] Through the following steps (a) to (d), Figure 6 Implement as shown.
[0136] (a) An unformed body obtained by laminating a prepreg as the skin material 7 on a honeycomb core material (core material) 1 is placed on an aluminum tool plate 15 coated with a release agent.
[0137] (b) A Teflon (registered trademark) film 9, a silicone rubber 10, and a diffusant 11 are stacked in this order on the surface of the prepreg, and the whole is covered with a nylon bag film 12. A sealing material 14 is arranged between the aluminum tool plate 15 and the nylon bag film 12 to form a closed space. Then, the inside of the nylon bag film 12 (hereinafter referred to as the system) is sucked by a vacuum nozzle 13, and the system is directly placed in an autoclave while maintaining a vacuum state.
[0138] (c) The pressure in the autoclave was raised to 0.15 MPa, and then the pressure in the system was returned to normal pressure. The pressure in the autoclave was then raised to 0.30 MPa, and then the temperature was started to rise.
[0139] (d) The pressure in the autoclave is maintained at 0.30 MPa until molding is completed, and the temperature is raised to 180°C at a rate of 1.5°C / min. Next, the autoclave is left at 180°C for 2 hours to allow the resin to solidify and bond to the honeycomb core material. The autoclave is then cooled to room temperature at a rate of 2°C / min to produce a honeycomb sandwich structure.
[0140] [Determination of climbing roller peel strength]
[0141] Samples were cut out from the honeycomb sandwich structure, and the climbing roller peel strength between the skin face sheet on the aluminum tool plate side and the honeycomb core material was measured according to ASTM D1781.
[0142] [Buckling resistance of honeycomb core material]
[0143] The core material retention rate during molding was measured by the following procedures (1) to (4), and the buckling resistance of the cell wall of the honeycomb core material was evaluated according to the following three levels.
[0144] Good: The core material retention rate is 99% or more.
[0145] Fair: The core material retention rate is 90% or more and less than 99%.
[0146] Bad: The core material retention rate is less than 90%.
[0147] (1) Prepreg 1 is stacked in two layers at (±45°) / (0° / 90°) on the upper and lower sides of each chamfered honeycomb core material.
[0148] (2) Measure the horizontal and vertical dimensions A and B of the upper surface before molding. (Shown in Figure 7 and Fig. 9 )
[0149] (3) Measure the horizontal and vertical dimensions a and b of the upper surface after molding. (Shown in Figure 8 and Fig. 9 )
[0150] (4) Core material retention rate (%) = (a×b)×100 / (A×B)
[0151] It should be noted that the molding Figure 6 As shown, the lamination / molding preparation was carried out under the same conditions as the molding of the sample (2) of the above-mentioned [honeycomb sandwich structure].
[0152] [Compression strength]
[0153] Samples were cut out from the above-mentioned skin-core structure and tested according to MIL-STD-401 to measure the compressive strength (tested by stabilized compression).
[0154] Hereinafter, the honeycomb core materials and sandwich structures produced in Examples and Comparative Examples will be described.
[0155] [Example 1]
[0156] The honeycomb core material 1 and the prepreg 1 obtained by the above method were used to produce a honeycomb sandwich structure having a laminated structure of [prepreg / adhesive film / honeycomb core material / adhesive film / prepreg].
[0157] [Example 2]
[0158] A honeycomb sandwich structure was produced in the same manner as in Example 1 except that the honeycomb core material 2 obtained by the above method was used.
[0159] [Example 3]
[0160] The honeycomb sandwich structure was produced in the same manner as in Example 1 except that the honeycomb core material 3 obtained by the above method was used.
[0161] [Example 4]
[0162] The sandwich structure was produced in the same manner as in Example 1 except that the honeycomb core material 5 obtained by the above method was used.
[0163] [Example 5]
[0164] The sandwich structure was produced in the same manner as in Example 1 except that the honeycomb core material 6 obtained by the above method was used.
[0165] [Comparative Example 1]
[0166] A sandwich structure was produced in the same manner as in Example 1 except that the honeycomb core material 4 was used.
[0167] The core material of the present invention has air permeability due to the porous structure of the unit wall. In addition, based on the comparison of Examples 1 to 5 with Comparative Example 1, it can be seen that the adhesion between the skin material and the core material, as indicated by the climbing roller peel strength, and the core material's resistance to buckling and compression strength are very excellent.
[0168] [surface@@]
[0169]
[0170] Industrial Availability
[0171] The core material and skin-core structure of the present invention can be suitably used as structural parts such as automobile interior and exterior decoration materials, solar cell reinforcement bodies, structural materials for sports equipment, aircraft interior decoration materials, aircraft structural materials, artificial satellite frames, and transportation boxes.
[0172] The core material and the skin-core structure of the present invention can be used as air-permeable structural components to make the internal pressure of each unit space inside the core material structure consistent / assimilated with the external pressure (zero-pressure space), and thus can be particularly suitable for aerospace equipment such as artificial satellites, spacecraft, and lunar exploration vehicles. In addition, as for the core material and the skin-core structure of the present invention, the porous structure in the core material absorbs impact energy by sequentially destroying, and thus can be particularly suitable for aircraft such as UAM (Urban airmobility), drones, and helicopters as impact absorbing components.
[0173] Description of Reference Numerals
[0174] 1: Core material
[0175] 2. 2a~2e: Fiber Cf
[0176] 3: Resin Cr
[0177] 4: Cell wall
[0178] 5: Gap
[0179] 6: Porous structure
[0180] 7: Leather material (prepreg blank)
[0181] 8: Skin-core structure
[0182] 9: Teflon (registered trademark) film
[0183] 10: Silicone rubber
[0184] 11: Seepage
[0185] 12: Nylon bag film
[0186] 13: Vacuum nozzle
[0187] 14: Sealing material
[0188] 15: Aluminum tool plate
[0189] 17: Resin Sr
[0190] 18: The penetration distance of fiber Cf into the leather material
[0191] A: Transverse dimension of the core material before forming
[0192] B: Longitudinal dimension of the core material before forming
[0193] a: Transverse dimension of the core material after forming
[0194] b: Longitudinal dimension of the core material after forming
Claims
1. A core material having a structure formed by an aggregate of hollow columnar units divided by unit walls, wherein the unit walls are formed by a fiber-reinforced composite material containing fibers (Cf) and resin (Cr), and at least a portion of the unit walls is a porous structure portion composed of an aggregate of fibers (Cf), and the fibers (Cf) are fibers coated with resin (Cr). 2 . The core material according to claim 1 , wherein the porous structure portion has pores that are continuous at least in a thickness direction of the cell wall.
3. The core material according to claim 1, wherein the area ratio of the cell wall per unit core material density in the area of the end surface of the cell opening is 0.075%·m 3 / kg or more. 4 . The core material according to claim 1 , wherein an average pore diameter of the porous structure portion measured by mercury porosimetry is 1 μm or more and 200 μm or less.
5. The core material according to any one of claims 1 to 3, wherein the density of the cell wall is 0.1 to 1.3 g / cm 3 . 6 . The core material according to claim 1 , wherein an average fiber orientation angle of the fibers (Cf) in the cell walls in an out-of-plane direction is 0 to 10 degrees. 7 . The core material according to claim 1 , wherein the fiber (Cf) has a tensile elastic modulus of 100 GPa or more. 8 . The core material according to claim 1 , wherein the structure formed by the assembly of the units is a honeycomb structure. 9 . The core material according to claim 1 , wherein the aggregate of the units is composed of units having a plurality of polygonal unit shapes. 10 . The core material according to claim 9 , wherein an opening surface of the hollow columnar unit has a curved surface shape. 11 . A skin-core structure, wherein a skin material is bonded to at least one end surface of the cell opening of the core material according to claim 1 . 12 . The skin-core structure according to claim 11 , which has a structure in which a part of the fiber (Cf) contained in the core material enters the skin material. 13 . The skin-core structure according to claim 11 , wherein the skin material is formed of a fiber-reinforced composite material comprising fibers (Sf) and resin (Sr). The skin-core structure according to claim 13 , wherein the fibers (Sf) are carbon fibers. 15 . The skin-core structure according to claim 11 , wherein the porous structure portion is provided near the opening end of the hollow columnar unit, and the skin material is bonded to the porous structure portion. 16 . The skin-core structure according to claim 15 , wherein a portion of the resin (Sr) constituting the skin material and / or the resin (Ar) contained in the adhesive flows into the porous structure portion of the core material. 17 . The skin-core structure according to claim 15 , wherein the thickness of the cell wall near the opening end is thicker than the center portion of the cell wall.
18. An aerospace device comprising the core material according to any one of claims 1 to 3 as an air-permeable structural component.
19. An aircraft comprising the core material according to any one of claims 1 to 3 as a shock absorbing member.
20. A method for producing a skin-core structure, comprising laminating the core material according to any one of claims 1 to 3 so that the opening surface of the core material is in contact with the skin material, and bonding them together by heating and pressurizing.
Citation Information
Patent Citations
Sandwich laminate, sandwich structure and unified molded product using same and processes for producing both
CN105073403A
Method for producing fiber reinforced composite material
CN108698268A
Manufacture of honeycomb core made of fiber-reinforced plastic with gas permeability
JP1999320724A
Fiber reinforced resin-made sandwich structure
JP2011224873A