Submerged super-amphiphobic Ag2S-MoS2 (at) CF oil-water separation filter membrane and preparation method thereof

By preparing a submerged superamphiphobic Ag2S-MoS2@CF filter membrane, we solved the problem that existing materials can only separate one oil-water mixture, achieved efficient separation of light oil/water and heavy oil/water mixtures, and had excellent reproducibility. The cycle performance expands the application scope of oil-water separation materials.

CN118807494AInactive Publication Date: 2024-10-22SHAANXI EXCELLENT NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410965817.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing oil-water separation materials can only separate one type of oil-water mixture and cannot effectively separate light oil/water and heavy oil/water mixtures at the same time, which limits its application scope.

Method used

Using the preparation method of submerged superamphiphobic Ag2S-MoS2@CF oil-water separation filter membrane, Ag2S-MoS2@ with submerged superamphiphobicity was prepared by pretreatment of carbon fiber, coating with nanosilver particles and hydrothermal reaction. CF filter membrane achieves oil-water separation.

Benefits of technology

This method does not require the modification of low surface energy substances and directly constructs submersible superamphiphobic materials, achieving more than 90% separation efficiency of oil-water mixtures. It also broadens the application scenarios of separation materials through renewable cycles of ultraviolet irradiation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807494A_ABST
    Figure CN118807494A_ABST
Patent Text Reader

Abstract

The invention discloses an under-liquid super-amphiphobic Ag2S-MoS2 (at) CF oil-water separation filter membrane and a preparation method thereof. The preparation method is specifically implemented according to the following steps: step 1, pretreating the surface of carbon fiber; step 2, preparing a carbon fiber material uniformly coated with nano-silver particles; and step 3, preparing the Ag2S-MoS2 (at) CF filtering membrane with the submerged super-amphiphobic property. The oil-water separation filter membrane can be applied to separation of oil-water mixtures, oil-in-water emulsions and water-in-oil emulsions, the separation efficiency is 90% or above, and the problem that an existing separation membrane can only be applied to separation of one oil-water mixture or one oil-water emulsion on the surface of the same material is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of oil-water mixture separation materials, and specifically relates to a method for preparing an underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane, and also relates to an underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane. Background Art

[0002] With the rapid development of industrialization in my country, the number of steel mills, petrochemical plants and textile mills has increased dramatically, making outstanding contributions to my country's economy. But there are also some problems, a large number of oily wastewater discharges and marine oil spills occur frequently, posing a serious threat to the ecological environment. At present, oil-water separation materials are divided into two types: super hydrophilic / underwater super oleophobic "water removal" membranes and super oleophilic / under oil super hydrophobic "oil removal" membranes. But they can only be used for the separation of an oil-water mixture (light oil / water mixture, heavy oil / water mixture), which greatly limits its application in the separation of oil-water mixtures. It can be seen from this that it is crucial to develop a membrane (submerged super-double-repellent membrane) separation material that can separate both light oil / water mixtures and heavy oil / water mixtures. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing an underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane to solve the problem that the existing oil-water separation materials can only separate one oil-water mixture.

[0004] Another object of the present invention is to provide an underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane.

[0005] The technical solution adopted by the present invention is a method for preparing an underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane, which is specifically implemented according to the following steps:

[0006] Step 1, pre-treating the carbon fiber surface;

[0007] Step 2, preparing nano silver particles uniformly coating carbon fiber materials;

[0008] Step 3, prepare Ag2S-MoS2@CF filter membrane with underwater super amphiphobicity.

[0009] The present invention is also characterized in that:

[0010] The specific process of step 1 is:

[0011] Step 1.1, immersing the carbon fiber in an acetone solution for degumming, taking it out and drying it;

[0012] Step 1.2, soaking the carbon fiber treated in step 1.1 in a concentrated nitric acid solution, taking it out and washing it with distilled water until the aqueous solution is neutral, and drying it;

[0013] Step 1.3, subjecting the carbon fiber surface treated in step 1.2 to alternating front and back ultraviolet irradiation.

[0014] In step 1.1, the immersion time is 1 h to 3 h, the drying temperature is 10° C. to 100° C., and the drying time is 1 h to 7 h;

[0015] In step 1.2, the soaking time is 5 h to 7 h, the drying temperature is 10° C. to 100° C., and the drying time is 1 h to 7 h;

[0016] In step 1.3, the wavelength of ultraviolet light used in ultraviolet irradiation is 184nm to 254nm, and the irradiation time is 1h to 3h.

[0017] The specific process of step 2 is:

[0018] Step 2.1, immersing the carbon fiber treated in step 1 in an AgNO3 aqueous solution, adding polyvinyl pyrrolidone and then performing ultrasonic vibration;

[0019] Step 2.2, subjecting the carbon fiber treated in step 2.1 to a water bath treatment, after which the carbon fiber is washed with distilled water, and dried to obtain uniformly coated Ag Nps@CF.

[0020] In step 2.1, the concentration of the AgNO3 aqueous solution is 0.2 mol / L, the molar ratio of polyvinyl pyrrolidone to AgNO3 is 1 to 2:1; the immersion time is 10 min to 50 min; the ultrasonic time is 6 h to 10 h;

[0021] In step 2.2, the temperature of the water bath is 60°C to 80°C, and the water bath time is 3h to 5h; the drying temperature is 30°C to 100°C, and the drying time is 3h to 10h.

[0022] The specific process of step 3 is:

[0023] Step 3.1, adding thioacetamide and sodium molybdate dihydrate into deionized water and mixing them evenly to obtain a hydrothermal reaction solution;

[0024] Step 3.2, transferring the uniformly coated Ag Nps@CF obtained in step 2.2 together with the hydrothermal reaction solution into a polytetrafluoroethylene stainless steel reactor for hydrothermal reaction;

[0025] In step 3.3, the uniformly coated Ag Nps@CF treated in step 3.2 is taken out, washed with deionized water and anhydrous ethanol, and dried to obtain an Ag2S-MoS2@CF filter membrane with underwater superamphiphobicity.

[0026] In step 3.1, the concentration of thioacetamide is 6 mmol / L, and the concentration of sodium molybdate dihydrate is 1 mmol / L to 3 mmol / L;

[0027] Step 3.2, the temperature of the hydrothermal reaction is 180°C to 220°C, and the time of the hydrothermal reaction is 22h to 26h.

[0028] Another technical solution adopted by the present invention is that the underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane is obtained by the above-mentioned preparation method.

[0029] The beneficial effects of the present invention are:

[0030] (1) Compared with the raw materials commonly used to prepare underwater super-amphiphobic materials, the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the present invention does not require modification of low surface energy substances or external stimulation. It only directly constructs underwater super-amphiphobic materials by using inorganic micro-nano metal sulfides, which provides a new research idea for the preparation of new underwater super-amphiphobic materials and their application in the field of oil-water separation.

[0031] (2) The Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the present invention can be used for the separation of oil-water mixtures, oil-in-water and oil-in-water emulsions, and the separation efficiency is above 90%, which solves the problem that the existing separation membrane can only be used for the separation of one oil-water mixture or oil-water emulsion on the same material surface, and broadens the application scenarios of the existing separation membranes;

[0032] (3) The preparation method of the present invention adopts a simple method combining ultrasound, water bath and hydrothermal to obtain a dense and non-detachable inorganic nano-coating by adjusting the reaction parameters; wherein the metal sulfide is a photocatalytic material, and after multiple water-oil separation operations, ultraviolet light irradiation is performed. With the help of the photocatalytic degradation of the metal sulfide, the Ag2S-MoS2@CF filter membrane can restore its underwater super-amphiphobic properties and continue to be used for water-oil separation, thereby showing excellent renewable cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is the XRD spectrum of the uniformly coated Ag Nps@CF prepared by the method of the present invention;

[0034] Figure 2 This is the XPS spectrum of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the method of the present invention;

[0035] Figure 3 is a scanning electron microscope image of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the method of the present invention;

[0036] Figure 4 The static contact angle in air, wettability diagram of underwater oil and underwater water of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the method of the present invention;

[0037] Figure 5 It is a data diagram of the separation efficiency of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the method of the present invention for different types of oil-water mixtures;

[0038] Figure 6 It is the separation flux diagram of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the method of the present invention for petroleum ether / water and trichloroethylene / water oil-water mixture;

[0039] Figure 7 The wettability of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the method of the present invention can be reversibly switched between underwater super-oleophobicity and underwater super-hydrophobicity;

[0040] Figure 8 The laser confocal microscope images and optical photographs of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the method of the present invention before and after separation of oil-in-water emulsion;

[0041] Fig. 9 Laser confocal microscope images and optical photographs of the Ag2S-MoS2@CF filter membrane with underwater super amphiphobicity prepared by the method of the present invention before and after separation of oil-in-water emulsion. DETAILED DESCRIPTION

[0042] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0043] The preparation method of the underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane of the present invention is specifically implemented according to the following steps:

[0044] Step 1, pre-treating the carbon fiber surface;

[0045] The specific process is:

[0046] Step 1.1, immerse the carbon fiber in an acetone solution for degumming for 1h to 3h, take it out and put it in a 10℃ to 100℃ oven for drying for 1h to 7h;

[0047] Step 1.2, soaking the carbon fiber treated in step 1.1 in a concentrated nitric acid solution for 5 h to 7 h, taking it out and washing it with distilled water until the aqueous solution is neutral, and drying it at 10° C. to 100° C. for 1 h to 7 h;

[0048] Step 1.3, irradiating the carbon fiber surface treated in step 1.2 with ultraviolet light alternately on the front and back sides, the wavelength of the ultraviolet light is 184nm to 254nm, and the irradiation time is 1h to 3h;

[0049] Step 2, preparing nano silver (Ag Nps) particles to uniformly coat the carbon fiber material;

[0050] The specific process is:

[0051] Step 2.1, immersing the carbon fiber treated in step 1 in an AgNO3 aqueous solution for 10 min to 50 min, then performing an ultrasonic treatment for 6 h to 10 h, and adding a polyvinyl pyrrolidone (PVP) aqueous solution to the AgNO3 aqueous solution during the ultrasonic treatment to obtain a redox reaction solution;

[0052] Wherein, the concentration of AgNO3 aqueous solution is 0.2mol / L;

[0053] The molar ratio of polyvinyl pyrrolidone to AgNO3 is 1 to 2:1;

[0054] Step 2.2, treating the carbon fiber treated in step 2.1 in a water bath at 60°C to 80°C for 3h to 5h, washing the carbon fiber with distilled water, and drying at 30°C to 100°C for 3h to 10h to obtain uniformly coated Ag Nps@CF;

[0055] Step 3, preparing an Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity;

[0056] The specific process is:

[0057] Step 3.1, adding thioacetamide and sodium molybdate dihydrate into deionized water and mixing them evenly to obtain a hydrothermal reaction solution;

[0058] The concentration of thioacetamide is 6mmol / L, and the concentration of sodium molybdate dihydrate is 1mmol / L to 3mmol / L;

[0059] Step 3.2, transferring the uniformly coated Ag Nps@CF obtained in step 2.2 together with the hydrothermal reaction solution into a polytetrafluoroethylene stainless steel reactor and performing a hydrothermal reaction at 180°C to 220°C for 22h to 26h;

[0060] Step 3.3, taking out the uniformly coated Ag Nps@CF treated in step 3.2, washing it with deionized water and anhydrous ethanol for 3 to 5 times, and drying it at a temperature of 60°C to 80°C for 3h to 5h to obtain an Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity;

[0061] After the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity obtained in step 3 is subjected to an oil-water separation experiment, an oil film is formed on the surface of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity. The membrane is washed with anhydrous ethanol for 1 to 5 times, and the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity is irradiated with ultraviolet light for 2 hours to 6 hours. The wavelength range of the ultraviolet light is 184nm to 254nm. With the help of the photocatalytic degradation of Ag2S-MoS2, the carbon fiber can restore its underwater super-amphiphobicity.

[0062] The oil-water separation principle of the submerged super-amphiphobic filter Ag2S-MoS2@CF material prepared by the present invention is as follows: for the separation of immiscible oil-water mixtures, when the Ag2S-MoS2@CF filter membrane is wetted with water, the Ag2S-MoS2@CF exhibits super-hydrophilic properties, and water permeates the filter membrane under the action of gravity, while the light oil gradually floats up because its density is smaller than that of water, thereby forming a layer of water film on the surface of the Ag2S-MoS2@CF filter membrane, and the light oil is retained above the material, thereby achieving the separation of the light oil / water mixture. Similarly, for the separation of heavy oil / water mixtures, after pre-wetting the filter membrane with heavy oil, the super-oleophilic / super-hydrophobic properties under oil enable the Ag2S-MoS2@CF filter membrane to quickly capture organic matter such as oil, forming an oil film on the surface of the material, and the heavy oil passes through the filter membrane, while the water with a lower density is retained above the filter membrane, thereby achieving the separation of the heavy oil / water mixture. In addition, during the separation of the above oil-water mixture, the filter membrane can be cleaned and irradiated with ultraviolet light to restore its underwater super-amphiphobic properties. The same is true for the separation of water-in-oil and oil-in-water emulsions. Therefore, in the water-oil-solid three-phase system, Ag2S-MoS2 has excellent underwater super-oleophobicity and oil-in-water super-hydrophobicity.

[0063] Example 1

[0064] Step 1, pre-treating the carbon fiber surface;

[0065] The specific process is:

[0066] Step 1.1, immerse the carbon fiber in an acetone solution for degumming for 1 hour, take it out and put it in a 30°C oven for drying for 5 hours;

[0067] Step 1.2, soaking the carbon fiber treated in step 1.1 in a nitric acid solution with a mass concentration of 68% for 5 hours, taking it out and washing it with distilled water until the aqueous solution is neutral, and drying it at 30° C. for 5 hours;

[0068] Step 1.3, irradiating the carbon fiber surface treated in step 1.2 with ultraviolet light alternately on the front and back sides, the wavelength of the ultraviolet light is 184nm to 254nm, and the irradiation time is 1h;

[0069] Step 2, preparing nano silver particles uniformly coating carbon fiber materials;

[0070] The specific process is:

[0071] Step 2.1, immersing the carbon fiber treated in step 1 in an AgNO3 aqueous solution for 20 minutes, and then performing ultrasonic treatment for 6 hours, and adding a polyvinyl pyrrolidone (PVP) aqueous solution to the AgNO3 aqueous solution during the ultrasonic treatment, the total amount of the polyvinyl pyrrolidone (PVP) aqueous solution and the AgNO3 aqueous solution is 100 ml;

[0072] The prepared AgNO3 aqueous solution is prepared by adding 1.7g of silver nitrate solid to 50ml of deionized water;

[0073] The polyvinyl pyrrolidone aqueous solution is prepared by adding 1.1 g of polyvinyl pyrrolidone to 50 ml of deionized water;

[0074] The molar ratio of polyvinyl pyrrolidone to AgNO3 is 1:1;

[0075] Step 2.2, the carbon fiber treated in step 2.1 is treated in a water bath at 60°C for 5 h. After the treatment, the carbon fiber is washed with distilled water and dried at 30°C for 8 h to obtain uniformly coated Ag Nps@CF;

[0076] Step 3, preparing an Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity;

[0077] The specific process is:

[0078] Step 3.1, adding thioacetamide and sodium molybdate dihydrate into deionized water and mixing them evenly to obtain a hydrothermal reaction solution, the volume of the hydrothermal reaction solution is 100 ml;

[0079] The concentration of thioacetamide was 6mmol / L, and the concentration of sodium molybdate dihydrate was 1mmol / L;

[0080] Step 3.2, the uniformly coated AgNps@CF obtained in step 2.2 and the hydrothermal reaction solution were transferred to a polytetrafluoroethylene stainless steel reactor with a capacity of 150 ml and subjected to a hydrothermal reaction at 180°C for 22 h;

[0081] In step 3.3, the uniformly coated AgNps@CF treated in step 3.2 is taken out, washed with deionized water and anhydrous ethanol three times, and dried at 60°C for 3 h to obtain an Ag2S-MoS2@CF filter membrane with underwater superamphiphobicity.

[0082] The uniformly coated AgNps@CF (nanosilver particles uniformly coated carbon fiber material) prepared in this embodiment is as follows Figure 1As shown in the AgNps@CF spectrum, it can be clearly observed that the spectrum has obvious diffraction peaks at 37.7°, 44.0°, 64.4° and 77.4°, which belong to the (111), (200), (220) and (311) crystal plane diffraction peaks of face-centered cubic (FCC)-Ag, respectively. A broad diffraction peak appears at 2θ=25°, corresponding to the diffraction peak of CF. No diffraction peak of Ag crystal is observed in CF, but there is an obvious diffraction peak in AgNps@CF, indicating that AgNps is successfully coated on the CF surface.

[0083] The Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared in this embodiment is as follows: Figure 2 As shown, the characteristic peaks of Mo 3d, S2p, Ag 3d and C1s can be observed in the full XPS spectrum of Ag2S-MoS2@CF. Detailed spectrum analysis shows that the Ag2S-MoS2@CF filter membrane was successfully prepared.

[0084] like Figure 3 As shown, it can be seen that the carbon fiber surface is densely coated with Ag2S-MoS2 nanosheets.

[0085] like Figure 4 As shown in the figure, water droplets and oil droplets can quickly penetrate the surface of carbon fiber coated with Ag2S-MoS2 coating. Among them, the water contact angle is 0°, the oil contact angle is 0°, the underwater oil contact angle of the renewable underwater superamphiphobic Ag2S-MoS2@CF is 158°, and the underwater water contact angle of the oil is 156°, showing excellent underwater superamphiphobic properties.

[0086] After the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity obtained in step 3 is subjected to an oil-water separation experiment, an oil film is formed on the surface of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity. The membrane is washed twice with anhydrous ethanol and irradiated with ultraviolet light for 3 hours. The wavelength range of ultraviolet light is 184nm to 254nm. With the help of the photocatalytic degradation of Ag2S-MoS2, the carbon fiber can restore its underwater super-amphiphobicity.

[0087] Depend on Figure 7 It can be seen that the underwater oil contact angle and the underwater water contact angle of the same filter membrane surface can be reversibly switched, that is, the filter membrane is irradiated with ultraviolet light, and with the help of the photocatalytic degradation of Ag2S-MoS2, the carbon fiber can restore the underwater super-amphiphobic properties and be applied to the field of oil-water separation. Therefore, the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the present invention has excellent regenerative recycling performance. In addition, the separation ability of Ag2S-MoS2 was studied using other types of oil-water mixtures (cyclohexane, gasoline, petroleum ether, trichloroethylene and chlorobenzene). Figure 5 and Figure 6 As shown in Figure 2, the separation efficiency of Ag2S-MoS2 for all light / heavy oil / water mixtures is higher than 97.3%, with the water (petroleum ether / water) flux and oil (trichloroethylene / water) flux being 2735 and 9352 L·m, respectively. -2 ·h -1 . Figure 8 and Fig. 9 Ag2S-MoS2 is applied to the separation of oil-in-water and water-in-oil emulsions. From the laser confocal microscope images and optical photos, we can conclude that the oil-water emulsion becomes clear and transparent after separation, and tiny droplets can also be blocked by the super-amphiphobic filter membrane prepared by the invention. The emulsion droplets are between 50-1000nm, and the emulsion droplets after separation are almost invisible, indicating that the filter membrane material also has a good separation efficiency for oil-water emulsions.

[0088] Example 2

[0089] Step 1, pre-treating the carbon fiber surface;

[0090] The specific process is:

[0091] Step 1.1, immerse the carbon fiber in an acetone solution for degumming for 2 hours, take it out and put it in a 50°C oven for drying for 4 hours;

[0092] Step 1.2, soaking the carbon fiber treated in step 1.1 in a nitric acid solution with a mass concentration of 68% for 6 hours, taking it out and washing it with distilled water until the aqueous solution is neutral, and drying it at 50° C. for 4 hours;

[0093] Step 1.3, irradiating the carbon fiber surface treated in step 1.2 with ultraviolet light alternately on the front and back sides, the wavelength of the ultraviolet light is 184nm to 254nm, and the irradiation time is 2h;

[0094] Step 2, preparing nano silver particles uniformly coating carbon fiber materials;

[0095] The specific process is:

[0096] Step 2.1, immersing the carbon fiber treated in step 1 in an AgNO3 aqueous solution for 30 min, then performing ultrasonic treatment for 7 h and adding a polyvinyl pyrrolidone (PVP) aqueous solution to the AgNO3 aqueous solution during the ultrasonic treatment, the total amount of the polyvinyl pyrrolidone (PVP) aqueous solution and the AgNO3 aqueous solution being 100 ml;

[0097] The prepared AgNO3 aqueous solution is prepared by adding 1.7g of silver nitrate solid to 50ml of deionized water;

[0098] The polyvinyl pyrrolidone aqueous solution is prepared by adding 1.7 g of polyvinyl pyrrolidone to 50 ml of deionized water;

[0099] The molar ratio of polyvinyl pyrrolidone to AgNO3 is 1.5:1;

[0100] Step 2.2, the carbon fiber treated in step 2.1 is treated in a water bath at 70°C for 4 hours. After the treatment, the carbon fiber is washed with distilled water and dried at 50°C for 6 hours to obtain uniformly coated Ag Nps@CF;

[0101] Step 3, preparing an Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity;

[0102] The specific process is:

[0103] Step 3.1, adding thioacetamide and sodium molybdate dihydrate into deionized water and mixing them evenly to obtain a hydrothermal reaction solution, the volume of the hydrothermal reaction solution is 100 ml;

[0104] The concentration of thioacetamide was 6mmol / L, and the concentration of sodium molybdate dihydrate was 2mmol / L;

[0105] Step 3.2, the uniformly coated Ag Nps@CF obtained in step 2.2 and the hydrothermal reaction solution were transferred to a polytetrafluoroethylene stainless steel reactor with a capacity of 150 ml and subjected to a hydrothermal reaction at 200° C. for 24 h;

[0106] In step 3.3, the uniformly coated Ag Nps@CF treated in step 3.2 is taken out, washed with deionized water and anhydrous ethanol for 4 times, and dried at 70°C for 4 hours to obtain an Ag2S-MoS2@CF filter membrane with underwater superamphiphobicity.

[0107] After the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity obtained in step 3 is subjected to an oil-water separation experiment, an oil film is formed on the surface of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity. The membrane is washed with anhydrous ethanol three times and irradiated with ultraviolet light for 5 hours. The wavelength range of ultraviolet light is 184nm~254nm. With the help of the photocatalytic degradation of Ag2S-MoS2, the carbon fiber can restore its underwater super-amphiphobicity.

[0108] The underwater oil contact angle of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity obtained in this embodiment is 165°, and the underwater water contact angle is 163°, showing excellent underwater super-amphiphobic properties. After 30 cycles, the separation flux decreased slightly. Subsequently, the filter membrane was irradiated with ultraviolet light, and with the help of the photocatalytic degradation of Ag2S-MoS2, the carbon fiber can restore the underwater super-amphiphobic properties and be applied to the field of oil-water separation. Therefore, the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the present invention has excellent renewable cycle performance. In addition, the separation ability of Ag2S-MoS2 was studied using other types of oil-water mixtures (cyclohexane, gasoline, petroleum ether, trichloroethylene and chlorobenzene). As Figure 5 and Figure 6 As shown in Figure 2, the separation efficiency of Ag2S-MoS2 for all light / heavy oil / water mixtures is higher than 97.3%, and the water (petroleum ether / water) flux and oil (trichloroethylene / water) flux are 3125 and 11582 L·m, respectively. -2 ·h -1 .

[0109] Example 3

[0110] Step 1, pre-treating the carbon fiber surface;

[0111] The specific process is:

[0112] Step 1.1, immerse the carbon fiber in an acetone solution for degumming for 3 hours, take it out and put it in a 70°C oven for drying for 3 hours;

[0113] Step 1.2, soaking the carbon fiber treated in step 1.1 in a nitric acid solution with a mass concentration of 68% for 7 hours, taking it out and washing it with distilled water until the aqueous solution is neutral, and drying it at 70° C. for 3 hours;

[0114] Step 1.3, irradiating the carbon fiber surface treated in step 1.2 with ultraviolet light alternately on the front and back sides, the wavelength of the ultraviolet light is 184nm to 254nm, and the irradiation time is 3h;

[0115] Step 2, preparing nano silver particles uniformly coating carbon fiber materials;

[0116] The specific process is:

[0117] Step 2.1, immersing the carbon fiber treated in step 1 in an AgNO3 aqueous solution for 40 min, then performing ultrasonic treatment for 8 h and adding a polyvinyl pyrrolidone (PVP) aqueous solution to the AgNO3 aqueous solution during the ultrasonic treatment, the total amount of the polyvinyl pyrrolidone (PVP) aqueous solution and the AgNO3 aqueous solution being 100 ml;

[0118] The prepared AgNO3 aqueous solution is prepared by adding 1.7g of silver nitrate solid to 50ml of deionized water;

[0119] The polyvinyl pyrrolidone aqueous solution is prepared by adding 2.4 g of polyvinyl pyrrolidone to 50 ml of deionized water;

[0120] The molar ratio of polyvinyl pyrrolidone to AgNO3 is 2:1;

[0121] Step 2.2, the carbon fiber treated in step 2.1 is treated in a water bath at 80°C for 3 h. After the treatment, the carbon fiber is washed with distilled water and dried at 70°C for 3 h to obtain uniformly coated Ag Nps@CF;

[0122] Step 3, preparing an Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity;

[0123] The specific process is:

[0124] Step 3.1, adding thioacetamide and sodium molybdate dihydrate into deionized water and mixing them evenly to obtain a hydrothermal reaction solution, the volume of the hydrothermal reaction solution is 100 ml;

[0125] The concentration of thioacetamide was 6mmol / L, and the concentration of sodium molybdate dihydrate was 3mmol / L;

[0126] Step 3.2, the uniformly coated Ag Nps@CF obtained in step 2.2 and the hydrothermal reaction solution were transferred to a polytetrafluoroethylene stainless steel reactor with a capacity of 150 ml and subjected to a hydrothermal reaction at 220°C for 26 h;

[0127] In step 3.3, the uniformly coated Ag Nps@CF treated in step 3.2 is taken out, washed with deionized water and anhydrous ethanol for 5 times, and dried at 80°C for 5 h to obtain an Ag2S-MoS2@CF filter membrane with underwater superamphiphobicity.

[0128] After the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity obtained in step 3 is subjected to an oil-water separation experiment, an oil film is formed on the surface of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity. The membrane is washed with anhydrous ethanol for 5 times, and the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity is irradiated with ultraviolet light for 6 hours. The wavelength range of ultraviolet light is 184nm~254nm. With the help of the photocatalytic degradation of Ag2S-MoS2, the carbon fiber can restore its underwater super-amphiphobicity.

[0129] The underwater oil contact angle of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity obtained in this embodiment is 152°, and the underwater water contact angle is 155°, showing excellent underwater super-amphiphobic properties. After 30 cycles, the separation flux decreased slightly. Subsequently, the filter membrane was irradiated with ultraviolet light, and with the help of the photocatalytic degradation of Ag2S-MoS2, the carbon fiber can restore the underwater super-amphiphobic properties and be applied to the field of oil-water separation. Therefore, the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity prepared by the present invention has excellent renewable cycle performance. In addition, the separation ability of Ag2S-MoS2 was studied using other types of oil-water mixtures (cyclohexane, gasoline, petroleum ether, trichloroethylene and chlorobenzene). As Figure 5 and Figure 6 As shown in Figure 2, the separation efficiency of Ag2S-MoS2 for all light / heavy oil / water mixtures is higher than 97.3%, and the water (petroleum ether / water) flux and oil (trichloroethylene / water) flux are 2808 and 10592 L·m, respectively. -2 ·h -1 .

[0130] Example 4

[0131] Step 1, pre-treating the carbon fiber surface;

[0132] The specific process is:

[0133] Step 1.1, immerse the carbon fiber in an acetone solution for degumming for 3 hours, take it out and put it in a 90°C oven for drying for 1 hour;

[0134] Step 1.2, soaking the carbon fiber treated in step 1.1 in a nitric acid solution with a mass concentration of 68% for 7 hours, taking it out and washing it with distilled water until the aqueous solution is neutral, and drying it at 90° C. for 1 hour;

[0135] Step 1.3, irradiating the carbon fiber surface treated in step 1.2 with ultraviolet light alternately on the front and back sides, the wavelength of the ultraviolet light is 184nm to 254nm, and the irradiation time is 3h;

[0136] Step 2, preparing nano silver particles uniformly coating carbon fiber materials;

[0137] The specific process is:

[0138] Step 2.1, immersing the carbon fiber treated in step 1 in an AgNO3 aqueous solution for 50 min, then performing ultrasonic treatment for 9 h and adding a polyvinyl pyrrolidone (PVP) aqueous solution to the AgNO3 aqueous solution during the ultrasonic treatment, the total amount of the polyvinyl pyrrolidone (PVP) aqueous solution and the AgNO3 aqueous solution being 100 ml;

[0139] The prepared AgNO3 aqueous solution is prepared by adding 1.7g of silver nitrate solid to 50ml of deionized water;

[0140] The polyvinyl pyrrolidone aqueous solution is prepared by adding 2.4 g of polyvinyl pyrrolidone to 50 ml of deionized water;

[0141] The molar ratio of polyvinyl pyrrolidone to AgNO3 is 2:1;

[0142] Step 2.2, the carbon fiber treated in step 2.1 is treated in a water bath at 80°C for 3 h. After the treatment, the carbon fiber is washed with distilled water and dried at 90°C for 1 h to obtain uniformly coated Ag Nps@CF;

[0143] Step 3, preparing an Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity;

[0144] The specific process is:

[0145] Step 3.1, adding thioacetamide and sodium molybdate dihydrate into deionized water and mixing them evenly to obtain a hydrothermal reaction solution, the volume of the hydrothermal reaction solution is 100 ml;

[0146] The concentration of thioacetamide was 6mmol / L, and the concentration of sodium molybdate dihydrate was 3mmol / L;

[0147] Step 3.2, the uniformly coated Ag Nps@CF obtained in step 2.2 and the hydrothermal reaction solution were transferred to a polytetrafluoroethylene stainless steel reactor with a capacity of 150 ml and subjected to a hydrothermal reaction at 180°C for 26 h;

[0148] In step 3.3, the uniformly coated Ag Nps@CF treated in step 3.2 is taken out, washed with deionized water and anhydrous ethanol for 5 times, and dried at 80°C for 5 h to obtain an Ag2S-MoS2@CF filter membrane with underwater superamphiphobicity.

[0149] After the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity obtained in step 3 is subjected to an oil-water separation experiment, an oil film is formed on the surface of the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity. The membrane is washed with anhydrous ethanol for 5 times, and the Ag2S-MoS2@CF filter membrane with underwater super-amphiphobicity is irradiated with ultraviolet light for 6 hours. The wavelength range of ultraviolet light is 184nm~254nm. With the help of the photocatalytic degradation of Ag2S-MoS2, the carbon fiber can restore its underwater super-amphiphobicity.

Claims

1. A method for preparing an underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane, characterized in that: Follow the steps below to implement it: Step 1, pre-treating the carbon fiber surface; Step 2, preparing nano silver particles uniformly coating carbon fiber materials; Step 3, prepare Ag2S-MoS2@CF filter membrane with underwater super amphiphobicity.

2. The method for preparing the underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane according to claim 1, characterized in that: The specific process of step 1 is: Step 1.1, immersing the carbon fiber in an acetone solution for degumming, taking it out and drying it; Step 1.2, soaking the carbon fiber treated in step 1.1 in a nitric acid solution, taking it out and washing it with distilled water until the aqueous solution is neutral, and drying it; Step 1.3, subjecting the carbon fiber surface treated in step 1.2 to alternating front and back ultraviolet irradiation.

3. The method for preparing the underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane according to claim 2, characterized in that: In step 1.1, the immersion time is 1 h to 3 h, the drying temperature is 10° C. to 100° C., and the drying time is 1 h to 7 h; In step 1.2, the soaking time is 5 h to 7 h, the drying temperature is 10° C. to 100° C., and the drying time is 1 h to 7 h; In step 1.3, the wavelength of ultraviolet light used in ultraviolet irradiation is 184nm to 254nm, and the irradiation time is 1h to 3h.

4. The method for preparing the underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane according to claim 1, characterized in that: The specific process of step 2 is: Step 2.1, immersing the carbon fiber treated in step 1 in an AgNO3 aqueous solution, followed by ultrasonic treatment and adding a polyvinyl pyrrolidone aqueous solution to the AgNO3 aqueous solution during the ultrasonic treatment; Step 2.2, subjecting the carbon fiber treated in step 2.1 to a water bath treatment, after which the carbon fiber is washed with distilled water, and dried to obtain uniformly coated Ag Nps@CF.

5. The method for preparing the underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane according to claim 4, characterized in that: In step 2.1, the concentration of the AgNO3 aqueous solution is 0.2 mol / L; the molar ratio of polyvinyl pyrrolidone to AgNO3 is 1 to 2:1; the immersion time is 10 min to 50 min; the ultrasonic time is 6 h to 10 h; In step 2.2, the temperature of the water bath is 60°C to 80°C, and the water bath time is 3h to 5h; the drying temperature is 30°C to 100°C, and the drying time is 3h to 10h.

6. The method for preparing the underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane according to claim 4, characterized in that: The specific process of step 3 is: Step 3.1, adding thioacetamide and sodium molybdate dihydrate into deionized water and mixing them evenly to obtain a hydrothermal reaction solution; Step 3.2, transferring the uniformly coated Ag Nps@CF obtained in step 2.2 together with the hydrothermal reaction solution into a polytetrafluoroethylene stainless steel reactor for hydrothermal reaction; In step 3.3, the uniformly coated Ag Nps@CF treated in step 3.2 is taken out, washed with deionized water and anhydrous ethanol, and dried to obtain an Ag2S-MoS2@CF filter membrane with underwater superamphiphobicity.

7. The method for preparing the underwater super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane according to claim 4, characterized in that: In step 3.1, the concentration of thioacetamide is 6 mmol / L, and the concentration of sodium molybdate dihydrate is 1 mmol / L to 3 mmol / L; Step 3.2, the temperature of the hydrothermal reaction is 180°C to 220°C, and the time of the hydrothermal reaction is 22h to 26h.

8. Submerged super-amphiphobic Ag2S-MoS2@CF oil-water separation filter membrane, characterized in that: The method is as described in any one of claims 1 to 7.