Three-dimensional nanofiber composite aerogel as well as preparation method and application thereof

The nanofiber composite aerogel prepared through electrospinning technology combines chemical cross-linking of cellulose nanocrystals and blocked isocyanate and polymer nanoparticle coating to solve the problems of poor mechanical stability and low adsorption capacity of traditional aerogels. problem, achieving efficient removal of organic dyes.

CN118807623AActive Publication Date: 2024-10-22XI AN JIAOTONG UNIV
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410894425.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-22
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

Traditional three-dimensional nanofiber aerogels suffer from poor mechanical stability and low adsorption capacity, which limits their practical application in the field of pollutant removal.

Method used

Using electrospinning nanofibers, cellulose nanocrystals and blocked isocyanate as the main materials, through freeze setting, freeze drying and thermal cross-linking treatments, a nanofiber composite aerogel with a stable structure is formed, and its surface is covered with polymerization material nanoparticles to improve adsorption performance.

Benefits of technology

The mechanical stability and adsorption capacity of nanofiber composite aerogels are significantly improved, and they can efficiently adsorb and remove anionic and cationic organic dyes, solving the shortcomings of traditional aerogels in pollutant removal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807623A_ABST
    Figure CN118807623A_ABST
Patent Text Reader

Abstract

The invention discloses a three-dimensional nanofiber composite aerogel and a preparation method and application thereof, and relates to the technical field of nanofiber composite aerogel materials.The preparation method comprises the steps that firstly, nanofibers are prepared through the electrostatic spinning technology, then the electrostatic spinning nanofibers, cellulose nanocrystals, chemical cross-linking agent terminated isocyanate and water are mixed and homogenized, and the three-dimensional nanofiber composite aerogel is prepared. The preparation method comprises the following steps: preparing a stable dispersion liquid by using a sol-gel method, then sequentially carrying out freeze-shaping, freeze-drying and thermal crosslinking treatment, and finally, loading polymer nanoparticles on the surface of the product to obtain the three-dimensional nanofiber composite aerogel with a porous three-dimensional network structure, good mechanical stability and excellent adsorption performance. The technical problems that an existing nanofiber aerogel adsorption material is poor in mechanical stability and low in adsorption capacity are solved. The three-dimensional nanofiber composite aerogel provided by the invention is simple in preparation method and strong in operability, and can efficiently adsorb and separate anionic and cationic dyes at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanofiber composite aerogel materials, and specifically relates to a three-dimensional nanofiber composite aerogel and a preparation method and application thereof. Background Art

[0002] Water bodies are the main carriers of pollutants in the environment. With the circulation of aquatic ecosystems, pollutants enter surface water and groundwater through runoff, diffusion, infiltration and other pathways, causing pollution of drinking water sources and food, posing a serious threat to the ecological environment and human health. Among them, organic dyes are widely used in food, leather, papermaking and textile industries, and are one of the most common and typical pollutants in water bodies. Organic dyes in wastewater may cause dysfunction of multiple organs, reproductive system and central nervous system in the human body, and most organic dyes are stable in nature and poorly degradable. Therefore, it is necessary to develop methods for efficiently removing organic dyes from wastewater. Among the many methods, adsorbent-based water purification technology is considered to be one of the most promising methods due to its simple process, strong operability and high efficiency.

[0003] Electrospinning technology is one of the most effective methods for preparing nanofibers. It has the characteristics of simple equipment, wide range of raw material sources, and good controllability of fiber structure. The high specific surface area and long diameter of electrospun nanofibers make them exhibit excellent mass transfer performance. The three-dimensional nanofiber aerogel constructed with electrospun nanofibers not only has a high specific surface area and high porosity, but also has a unique multi-level mesh interconnection structure. The micro-nano network transport channel formed can achieve more efficient mass transfer, effectively improve the application performance of nanofiber materials in the field of adsorption and separation, and is an ideal pollutant removal material. However, traditional three-dimensional nanofiber aerogels have problems such as poor mechanical stability and low adsorption capacity, which limit their practical application. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a three-dimensional nanofiber composite aerogel and a preparation method and application thereof, so as to solve the technical problems of poor mechanical stability and low adsorption capacity of existing nanofiber aerogel adsorption materials.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention discloses a method for preparing a three-dimensional nanofiber composite aerogel, comprising the following steps:

[0007] Step 1: mixing and homogenizing the electrospun nanofibers, cellulose nanocrystals, blocked isocyanate and water to obtain a uniform dispersion;

[0008] Step 2: subjecting the above dispersion to freeze-setting, freeze-drying and thermal cross-linking treatment in sequence to obtain a cross-linked product, namely, electrospun nanofiber-cellulose nanocrystal composite aerogel;

[0009] Step 3: coating the surface of the electrospun nanofiber-cellulose nanocrystal composite aerogel with polymer nanoparticles to obtain a three-dimensional nanofiber composite aerogel.

[0010] Preferably, the electrospun nanofibers described in step 1 are prepared by mixing one or more of polyacrylonitrile, nylon, cellulose acetate and polyethyleneimine.

[0011] Further preferably, the mass ratio of the electrospun nanofibers and cellulose nanocrystals in step one is 1:0.25-0.67; the total mass of the electrospun nanofibers and cellulose nanocrystals in step one accounts for 0.6-2.4wt% of the dispersion.

[0012] Further preferably, the amount of the blocked isocyanate added in step 1 accounts for 10-30% of the total mass of the electrospun nanofibers and cellulose nanocrystals.

[0013] Further preferably, in step 1, the homogenization speed is 8000-15000 rpm, and the homogenization time is 5-20 min.

[0014] Preferably, in step 2, the freezing setting temperature is -80 to -40°C, and the freezing setting time is 30 to 60 minutes; the freeze drying temperature is -80 to -60°C, and the freeze drying time is 20 to 30 hours; the temperature of the thermal crosslinking treatment is 120 to 130°C, and the time of the thermal crosslinking treatment is 1 to 2 hours.

[0015] Further preferably, the dispersion in step 2 needs to be dispensed into a mold first, and then subjected to subsequent freeze-setting, freeze-drying and heat treatment.

[0016] Preferably, in step three, the loaded nanoparticles include at least one of polyaniline and polypyrrole.

[0017] The present invention discloses a three-dimensional nanofiber composite aerogel prepared based on any one of the above-mentioned methods for preparing a three-dimensional nanofiber composite aerogel.

[0018] The invention discloses application of a three-dimensional nanofiber composite aerogel as an organic dye adsorbent.

[0019] The invention discloses application of a three-dimensional nanofiber composite aerogel as an anionic and cationic organic dye adsorbent.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The method for preparing the three-dimensional nanofiber composite aerogel disclosed in the present invention uses electrospun nanofibers as a skeleton, cellulose nanocrystals as a reinforcing phase, and blocked isocyanate as a chemical crosslinking agent to prepare a nanofiber composite aerogel with a stable structure, and then coats the fiber surface of the aerogel with polymer nanoparticles. The three-dimensional nanofiber composite aerogel provided by the present invention has a simple preparation process, strong operability, and no secondary pollution. It is an environmentally friendly material and is suitable for industrial production and application. Compared with traditional aerogels, the three-dimensional nanofiber composite aerogel proposed by the present invention shows better flexibility and good mechanical stability. The advantages are mainly reflected in:

[0022] 1. Electrospun nanofibers have strong flexibility, good uniformity, high specific surface area and excellent mass transfer performance;

[0023] 2. Cellulose nanocrystals, as a natural nano-rod-shaped cellulose material, have high crystallinity and high strength. They are a green reinforcement phase that can improve the mechanical properties of composite materials.

[0024] 3. Both nanofibers and cellulose nanocrystals have rich chemical groups on their surfaces. Experimental data show that the two are randomly interlaced to form a hierarchical porous three-dimensional network structure that is interconnected. As an adsorbent, it is beneficial to improve the adsorption efficiency. By combining electrospun nanofibers and cellulose nanocrystals, the pore structure inside the aerogel can be made more robust. Experiments show that the three-dimensional nanofiber composite aerogel composed of electrospun nanofibers and cellulose nanocrystals exhibits a larger specific surface area and total pore volume, which improves the adsorption capacity of the composite aerogel.

[0025] 4. The blocked isocyanate is unblocked under heating conditions to produce active -NCO groups, which can chemically cross-link with the hydroxyl groups on the cellulose nanocrystals to form a strong adhesion between the fibers;

[0026] 5. Loading polymer nanoparticles on the surface of aerogel fibers can further improve their adsorption performance and increase their adsorption capacity.

[0027] The three-dimensional nanofiber composite aerogel prepared by the method of the present invention has been shown by experimental data to have smaller deformation and better mechanical stability, thus effectively solving the problem of poor mechanical stability of nanofiber aerogel in the prior art.

[0028] Since the surfaces of the electrospun nanofibers and cellulose nanocrystals used in the present invention have abundant chemical groups, they are useful for improving the adsorption efficiency as adsorbents; the polymer nanoparticles are coated on the surface of the aerogel fibers to further improve their adsorption performance and increase the adsorption capacity. Therefore, the three-dimensional nanofiber composite aerogel prepared by the present invention can simultaneously and efficiently adsorb and remove anionic and cationic dyes by utilizing the synergistic effect of electrospun nanofibers, cellulose nanocrystals and polypyrrole. Experiments have shown that the composite aerogel of the present application has a better comprehensive adsorption effect on acid orange 7, acid red 14 and rhodamine B dyes; and the adsorption effect on anionic and cationic dyes is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a scanning electron microscope image of the polyacrylonitrile nanofiber membrane synthesized by the present invention;

[0030] Figure 2 This is a scanning electron microscope image of the three-dimensional nanofiber composite aerogel prepared in Example 6 of the present invention;

[0031] Figure 3 The three-dimensional nanofiber composite aerogel prepared by the present invention and the digital photos of the aerogel with a weight of 20 g thereof are shown in Figure 1, wherein A1 is a digital photo of the aerogel of Example 6 after crosslinking, A2 is a digital photo of the aerogel of Example 6 after being coated with polypyrrole, and A3 is a digital photo of the aerogel of Example 6 after being coated with a weight of 20 g; B1 is a digital photo of the aerogel of Comparative Example 2 after crosslinking, B2 is a digital photo of the aerogel of Comparative Example 2 after being coated with polypyrrole, and B3 is a digital photo of the aerogel of Comparative Example 2 after being coated with a weight of 20 g;

[0032] Figure 4 The N2 adsorption-desorption curves and pore size distribution diagrams of the polyacrylonitrile nanofiber membrane and the three-dimensional nanofiber composite aerogel prepared in Example 6 of the present invention, wherein A is the N2 adsorption-desorption curves of the polyacrylonitrile nanofiber membrane and the three-dimensional nanofiber composite aerogel; B is the pore size distribution diagram of the polyacrylonitrile nanofiber membrane and the three-dimensional nanofiber composite aerogel;

[0033] Figure 5 Fourier infrared spectra of the polyacrylonitrile nanofiber membrane and the three-dimensional nanofiber composite aerogel prepared by the present invention before cross-linking, after cross-linking and after being coated with polypyrrole;

[0034] Figure 6 The present invention is a flow chart of the preparation method of the three-dimensional nanofiber composite aerogel. DETAILED DESCRIPTION

[0035] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0036] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0037] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0038] See also Figure 6 , is a flow chart of the preparation method of the three-dimensional nanofiber composite aerogel disclosed in the present invention, and the specific steps are:

[0039] (1) mixing and homogenizing electrospun nanofibers, cellulose nanocrystals, blocked isocyanate and water to obtain a uniform dispersion;

[0040] (2) dispensing the above dispersion into a mold, and sequentially performing freeze-setting, freeze-drying and heat treatment;

[0041] (3) The above product is coated with polymer nanoparticles to obtain a three-dimensional nanofiber composite aerogel.

[0042] Preferably, the electrospun nanofibers in step (1) are prepared by mixing one or more of polyacrylonitrile, nylon, cellulose acetate and polyethyleneimine.

[0043] Preferably, in step (1), the mass ratio of electrospun nanofibers to cellulose nanocrystals is 1:0.25-0.67; the total mass of electrospun nanofibers and cellulose nanocrystals accounts for 0.6-2.4wt% of the dispersion; and the amount of blocked isocyanate added is 10-30% of the total mass of electrospun nanofibers and cellulose nanocrystals.

[0044] Preferably, in step (1), the homogenization speed is 8000-15000 rpm, and the homogenization time is 5-20 min.

[0045] Preferably, in step (2), the freezing setting temperature is -80 to -40°C, and the freezing setting time is 30 to 60 minutes; the freeze drying temperature is -80 to -60°C, and the freeze drying time is 20 to 30 hours; the heat treatment temperature is 120 to 130°C, and the heat treatment time is 1 to 2 hours.

[0046] Preferably, the polymer nanoparticles in step (3) are at least one of polyaniline and polypyrrole.

[0047] Embodiment 1:

[0048] S1. Preparation of polyacrylonitrile nanofiber membrane: polyacrylonitrile powder was dissolved in N,N-dimethylformamide and magnetically stirred at room temperature for 8 hours to obtain a spinning sol with a concentration of 10wt%. Then, the polyacrylonitrile sol was placed in an electrospinning filament ejector with a nozzle aperture of 0.4mm, a sol injection rate of 1mL / h, a distance from the nozzle to the aluminum foil receiving plate of 15cm, and a voltage of 12kV. After electrospinning for 3 hours, the collected product was dried to obtain a polyacrylonitrile nanofiber membrane. See the scanning electron microscope image for details. Figure 1 It can be seen that the prepared polyacrylonitrile nanofibers have a smooth surface, uniform thickness, and a fiber diameter of about 315nm.

[0049] S2. Cut the prepared polyacrylonitrile nanofiber membrane into square pieces of 1cm×1cm, place it in deionized water, and homogenize it at 12000rpm for 10min; then add cellulose nanocrystals, polyacrylonitrile nanofibers and cellulose nanocrystals in a mass ratio of 1:0.67, and blocked isocyanate in an amount of 10% of the total mass of polyacrylonitrile nanofibers and cellulose nanocrystals, and continue homogenizing for 10min to obtain a dispersion with a total mass of polyacrylonitrile nanofibers and cellulose nanocrystals of 0.6wt%.

[0050] S3. The dispersion is placed in a mold, frozen at -80°C for 30 minutes, and then freeze-dried at -80°C for 20 hours. After freeze-drying, an uncrosslinked aerogel is obtained, which is then placed at 125°C for 90 minutes for thermal crosslinking treatment to obtain a crosslinked polyacrylonitrile-cellulose nanocrystal composite aerogel.

[0051] S4. Soak 10 mg of the above aerogel in 4 mL of ethanol solution containing 0.1 mmol of pyrrole monomer and shake for 2 h to ensure that the pyrrole monomer fully penetrates into the polyacrylonitrile-cellulose nanocrystal composite aerogel, and then add 1 mL of ethanol solution containing 0.1 mmol of FeCl3·6H2O, wherein ethanol is used as a solvent and FeCl3·6H2O is used as an initiator for the polymerization of pyrrole monomer to initiate the polymerization reaction of pyrrole monomer, and mix and react at room temperature for 12 h to allow the pyrrole monomer to polymerize under the catalysis of FeCl3·6H2O to form polypyrrole and attach to the polypropylene-cellulose nanocrystal composite aerogel. Take out the above composite aerogel and wash it with deionized water to remove unreacted pyrrole monomer, initiator and other impurities. The three-dimensional nanofiber composite aerogel obtained after drying is recorded as PPCA-1.

[0052] Embodiment 2:

[0053] S1. Same as Example 1.

[0054] S2. Cut the prepared polyacrylonitrile nanofiber membrane into square pieces of 1cm×1cm, place it in deionized water, and homogenize it at 12000rpm for 10min; then add cellulose nanocrystals, polyacrylonitrile nanofibers and cellulose nanocrystals in a mass ratio of 1:0.67, and end-capped isocyanate in an amount of 30% of the total mass of polyacrylonitrile nanofibers and cellulose nanocrystals, and continue homogenizing for 10min to obtain a dispersion with a total mass of polyacrylonitrile nanofibers and cellulose nanocrystals of 1.2wt%.

[0055] S3. The dispersion is placed in a mold, frozen at -70°C for 40 minutes, and then freeze-dried at -70°C for 24 hours. After freeze-drying, an uncrosslinked aerogel is obtained, which is then placed at 130°C for 60 minutes for thermal crosslinking treatment to obtain a crosslinked polyacrylonitrile-cellulose nanocrystal composite aerogel.

[0056] S4. Soak 20 mg of the above aerogel in 4 mL of ethanol solution containing 0.2 mmol of pyrrole monomer and shake for 2 h. Then, add 1 mL of ethanol solution containing 0.2 mmol of FeCl3·6H2O to initiate the polymerization of pyrrole monomer. Mix and react at room temperature for 12 h. After taking out, wash with deionized water and dry. The obtained three-dimensional nanofiber composite aerogel is recorded as PPCA-2.

[0057] Embodiment 3:

[0058] S1. Same as Example 1.

[0059] S2. Cut the prepared polyacrylonitrile nanofiber membrane into square pieces of 1 cm×1 cm, place it in deionized water, and homogenize it at 12000rpm for 10 minutes; then add cellulose nanocrystals, polyacrylonitrile nanofibers and cellulose nanocrystals in a mass ratio of 1:0.67, and blocked isocyanate in an amount of 10% of the total mass of polyacrylonitrile nanofibers and cellulose nanocrystals, and continue homogenizing for 10 minutes to obtain a dispersion with a total mass of 2.4wt% of polyacrylonitrile nanofibers and cellulose nanocrystals.

[0060] S3. The dispersion is placed in a mold, frozen at -70°C for 40 minutes, and then freeze-dried at -70°C for 30 hours. After freeze-drying, an uncrosslinked aerogel is obtained, which is then placed at 120°C for thermal crosslinking treatment for 120 minutes to obtain a crosslinked polyacrylonitrile-cellulose nanocrystal composite aerogel.

[0061] S4. 40 mg of the above aerogel was immersed in 4 mL of ethanol solution containing 0.4 mmol of pyrrole monomer and shaken for 2 h. Then, 1 mL of ethanol solution containing 0.4 mmol of FeCl3·6H2O was added to initiate the polymerization of the pyrrole monomer. The mixture was mixed and reacted at room temperature for 12 h. After being taken out, it was washed with deionized water and dried. The obtained three-dimensional nanofiber composite aerogel was recorded as PPCA-3.

[0062] Embodiment 4:

[0063] S1. Same as Example 1.

[0064] S2. Cut the prepared polyacrylonitrile nanofiber membrane into square pieces of 1cm×1cm, place it in deionized water, and homogenize it at 15000rpm for 5min; then add cellulose nanocrystals, polyacrylonitrile nanofibers and cellulose nanocrystals in a mass ratio of 1:0.43, and blocked isocyanate in an amount of 20% of the total mass of polyacrylonitrile nanofibers and cellulose nanocrystals, and continue homogenizing for 10min to obtain a dispersion with a total mass of polyacrylonitrile nanofibers and cellulose nanocrystals of 0.6wt%.

[0065] S3. The dispersion is placed in a mold, frozen at -40°C for 60 minutes, and then freeze-dried at -60°C for 24 hours. After freeze-drying, an uncrosslinked aerogel is obtained, which is then placed at 125°C for thermal crosslinking treatment for 90 minutes to obtain a crosslinked polyacrylonitrile-cellulose nanocrystal composite aerogel.

[0066] S4. 10 mg of the above aerogel was immersed in 4 mL of ethanol solution containing 0.1 mmol of pyrrole monomer and shaken for 2 h. Then, 1 mL of ethanol solution containing 0.1 mmol of FeCl3·6H2O was added to initiate the polymerization of the pyrrole monomer. The mixture was mixed and reacted at room temperature for 12 h. After being taken out, it was washed with deionized water and dried. The obtained three-dimensional nanofiber composite aerogel was recorded as PPCA-4.

[0067] Embodiment 5:

[0068] S1. Same as Example 1.

[0069] S2. Cut the prepared polyacrylonitrile nanofiber membrane into square pieces of 1 cm×1 cm, place them in deionized water, and homogenize them at 10,000 rpm for 20 minutes; then add cellulose nanocrystals, polyacrylonitrile nanofibers and cellulose nanocrystals in a mass ratio of 1:0.25, and blocked isocyanate in an amount of 10% of the total mass of polyacrylonitrile nanofibers and cellulose nanocrystals, and continue homogenizing for 10 minutes to obtain a dispersion with a total mass of polyacrylonitrile nanofibers and cellulose nanocrystals of 0.6 wt%.

[0070] S3. The dispersion is placed in a mold, frozen at -40°C for 60 minutes, and then freeze-dried at -60°C for 24 hours. After freeze-drying, an uncrosslinked aerogel is obtained, which is then placed at 125°C for thermal crosslinking treatment for 90 minutes to obtain a crosslinked polyacrylonitrile-cellulose nanocrystal composite aerogel.

[0071] S4. Soak 10 mg of the above aerogel in 4 mL of ethanol solution containing 0.1 mmol of pyrrole monomer and shake for 2 h. Then, add 1 mL of ethanol solution containing 0.1 mmol of FeCl3·6H2O to initiate the polymerization of pyrrole monomer. Mix and react at room temperature for 12 h. After taking out, wash with deionized water and dry. The obtained three-dimensional nanofiber composite aerogel is recorded as PPCA-5.

[0072] Embodiment 6:

[0073] S1. Same as Example 1.

[0074] S2. Cut the prepared polyacrylonitrile nanofiber membrane into square pieces of 1cm×1cm, place them in deionized water, and homogenize them at 12000rpm for 10min; then add cellulose nanocrystals, polyacrylonitrile nanofibers and cellulose nanocrystals in a mass ratio of 1:0.25, and blocked isocyanate in an amount of 10% of the total mass of polyacrylonitrile nanofibers and cellulose nanocrystals, and continue homogenizing for 10min to obtain a dispersion with a total mass of 1.2wt% of polyacrylonitrile nanofibers and cellulose nanocrystals.

[0075] S3. The above dispersion was placed in a mold, frozen at -80°C for 40 minutes, and then freeze-dried at -70°C for 24 hours. After freeze-drying, an uncrosslinked aerogel was obtained, which was then placed at 125°C for thermal crosslinking treatment for 90 minutes to obtain a crosslinked polyacrylonitrile-cellulose nanocrystal composite aerogel. The digital photo is shown in Figure 3 A1 in .

[0076] S4. 10 mg of the above aerogel was immersed in 4 mL of ethanol solution containing 0.3 mmol of pyrrole monomer and shaken for 2 h. Then, 1 mL of ethanol solution containing 0.3 mmol of FeCl3·6H2O was added to initiate the polymerization of pyrrole monomer. The mixture was mixed and reacted at room temperature for 12 h. After being taken out, it was washed with deionized water and dried. The obtained three-dimensional nanofiber composite aerogel was recorded as PPCA-6. The digital photo is shown in Figure 3 A2 in Figure 2. SEM images are shown in Figure 2 As shown in the figure, the prepared three-dimensional nanofiber composite aerogel is composed of polyacrylonitrile nanofibers and cellulose nanocrystals randomly interspersed together to form a hierarchical porous three-dimensional network structure that is interconnected.

[0077] Embodiment 7:

[0078] S1. Preparation of nylon 6 nanofiber membrane: Nylon 6 particles were dissolved in a mixed solution of m-cresol and formic acid at a ratio of 4:6, v / v, and magnetically stirred at room temperature for 12 h to obtain a spinning sol with a concentration of 32 wt%. Then, the spinning sol was placed in an electrospinning jet, the aperture of the jet was 0.7 mm, the sol injection rate was 0.5 mL / h, the distance from the jet to the aluminum foil receiving plate was 15 cm, the voltage was 15 kV, and after electrospinning for 2 h, the collected product was dried to obtain a nylon 6 nanofiber membrane.

[0079] S2. Cut the prepared nylon 6 nanofiber membrane into square pieces of 0.5 cm × 0.5 cm, place it in deionized water, and homogenize it at 12000 rpm for 30 minutes; then add cellulose nanocrystals, nylon 6 nanofibers and cellulose nanocrystals in a mass ratio of 1:0.67, and the amount of blocked isocyanate added is 10% of the total mass of nylon 6 nanofibers and cellulose nanocrystals, and continue homogenizing for 15 minutes to obtain a dispersion with a total content of nylon 6 nanofibers and cellulose nanocrystals of 0.6wt%.

[0080] S3. The dispersion is placed in a mold, frozen at -80°C for 30 minutes, and then freeze-dried at -80°C for 20 hours. After freeze-drying, an uncrosslinked aerogel is obtained, which is then placed at 125°C for 90 minutes for thermal crosslinking treatment to obtain a crosslinked nylon 6-cellulose nanocrystal composite aerogel.

[0081] S4. Soak 10 mg of the above aerogel in 4 mL of 0.2 mol / L hydrochloric acid solution containing 0.2 mmol aniline monomer and shake for 2 h to ensure that the aniline monomer fully penetrates into the nylon 6-cellulose nanocrystal composite aerogel, and then add 1 mL of 0.2 mol / L hydrochloric acid solution containing 0.1 mmol ammonium persulfate, wherein 0.2 mol / L hydrochloric acid is used as a solvent and ammonium persulfate is used as an initiator for the polymerization of the aniline monomer to initiate the polymerization reaction of the aniline monomer, and mix and react at room temperature for 12 h to allow the aniline monomer to polymerize under the catalysis of ammonium persulfate to form polyaniline and attach to the polypropylene-cellulose nanocrystal composite aerogel. After taking out the above composite aerogel, it is repeatedly washed with 0.002 mol / L hydrochloric acid solution to remove unreacted aniline monomer, initiator and other impurities. The three-dimensional nanofiber composite aerogel obtained after drying is recorded as PPCA-7.

[0082] Embodiment 8:

[0083] S1. Preparation of polyacrylonitrile / polyethyleneimine composite nanofiber membrane: polyacrylonitrile powder and polyethyleneimine powder were dissolved in N,N-dimethylformamide at a ratio of 1:1, and magnetically stirred at room temperature for 10 hours to obtain a spinning sol with a concentration of 10wt%. Then, the spinning sol was placed in an electrospinning jet, the aperture of the jet was 0.5mm, the sol injection speed was 1mL / h, the distance from the jet to the aluminum foil receiving plate was 15cm, the voltage was 11kV, and after electrospinning for 2.5 hours, the collected product was dried to obtain a polyacrylonitrile / polyethyleneimine nanofiber membrane.

[0084] S2. Cut the prepared polyacrylonitrile / polyethyleneimine nanofiber membrane into square pieces of 1cm×1cm, place them in deionized water, and homogenize them at 12000rpm for 10min; then add cellulose nanocrystals in a mass ratio of 1:0.67 of polyacrylonitrile / polyethyleneimine nanofibers and cellulose nanocrystals, and add blocked isocyanate in an amount of 10% of the total mass of polyacrylonitrile / polyethyleneimine nanofibers and cellulose nanocrystals, and continue homogenizing for 10min to obtain a dispersion with a total mass of 0.6wt% of polyacrylonitrile / polyethyleneimine nanofibers and cellulose nanocrystals.

[0085] S3. The dispersion is placed in a mold, frozen at -80°C for 30 minutes, and then freeze-dried at -80°C for 20 hours. After freeze-drying, an uncrosslinked aerogel is obtained, which is then placed at 125°C for 90 minutes for thermal crosslinking treatment to obtain a crosslinked polyacrylonitrile / polyethyleneimine-cellulose nanocrystal composite aerogel.

[0086] S4. 10 mg of the above aerogel was immersed in 4 mL of 0.2 mol / L hydrochloric acid solution containing 0.1 mmol pyrrole monomer and 0.1 mmol aniline monomer and was shaken for 2 h to ensure that the pyrrole monomer and aniline monomer fully penetrated into the polyacrylonitrile / cellulose nanocrystal composite aerogel, and then 1 mL of 0.4 mmol 0.2 mol / L hydrochloric acid solution of FeCl3·6H2O, wherein 0.2 mol / L hydrochloric acid solution is used as a solvent, and FeCl3·6H2O is used as an initiator for the copolymerization of pyrrole and aniline monomers to initiate the polymerization reaction of pyrrole and aniline monomers, and the mixture is reacted at room temperature for 12 hours, so that the pyrrole monomer and the aniline monomer are copolymerized under the catalysis of FeCl3·6H2O to form a pyrrole and aniline copolymer and attached to the polyacrylonitrile-polyethyleneimine-cellulose nanocrystal composite aerogel, and the above-mentioned composite aerogel is taken out and repeatedly washed with 0.002 mol / L hydrochloric acid solution to remove unreacted monomers, initiators and other impurities, and the three-dimensional nanofiber composite aerogel obtained after drying is recorded as PPCA-8.

[0087] Comparative Example 1:

[0088] S1. Same as Example 1.

[0089] S2. Cut the prepared polyacrylonitrile nanofiber membrane into square pieces of 1cm×1cm, place them in deionized water, and homogenize them at 12000rpm for 10min; then add cellulose nanocrystals, polyacrylonitrile nanofiber membrane and cellulose nanocrystals in a mass ratio of 1:0.67, and blocked isocyanate in an amount of 10% of the total mass of electrospun nanofibers and cellulose nanocrystals, and continue homogenizing for 10min to obtain a dispersion with a total content of electrospun nanofibers and cellulose nanocrystals of 0.6wt%.

[0090] S3. The dispersion was placed in a mold, frozen at -80°C for 30 minutes, and then freeze-dried at -80°C for 20 hours. After freeze-drying, it was thermally cross-linked at 125°C for 90 minutes to obtain a cross-linked polyacrylonitrile-cellulose nanocrystal composite aerogel, which was recorded as PCA-1.

[0091] Comparative Example 2:

[0092] S1. Same as Example 1.

[0093] S2. Cut the prepared polyacrylonitrile nanofiber membrane into square pieces of 1 cm×1 cm, place it in deionized water, and homogenize it at 12000rpm for 10 minutes; then add blocked isocyanate in an amount of 10% of the mass of the electrospun nanofibers, and continue homogenizing for 10 minutes to obtain a dispersion with an electrospun nanofiber content of 0.6wt%.

[0094] S3. The above dispersion was placed in a mold, frozen at -80°C for 30 min, and then freeze-dried at -80°C for 20 h to obtain an uncrosslinked aerogel, which was then thermally crosslinked at 125°C for 90 min to obtain a polyacrylonitrile nanofiber aerogel, denoted as PA-1. The digital photo is shown in Figure 3 B1 in.

[0095] S4. 10 mg of the above aerogel was immersed in 4 mL of ethanol solution containing 0.1 mmol of pyrrole monomer and shaken for 2 h. Then, 1 mL of ethanol solution containing 0.1 mmol of FeCl3·6H2O was added to initiate the polymerization of pyrrole monomer. The mixture was mixed and reacted at room temperature for 12 h. After being taken out, it was washed with deionized water and dried. The obtained three-dimensional nanofiber composite aerogel was recorded as PPA-1. The digital photo is shown in Figure 3 B2 in.

[0096] Test Example 1:

[0097] The BET specific surface area and pore size distribution of the polyacrylonitrile nanofiber membrane and three-dimensional nanofiber composite aerogel (PPCA-6) prepared in Example 6 were measured by a fully automatic specific surface area and porosity analyzer.

[0098] like Figure 4 As shown, compared with the polyacrylonitrile nanofiber membrane, the three-dimensional nanofiber composite aerogel composed of polyacrylonitrile nanofibers and cellulose nanocrystals exhibits a larger specific surface area and total pore volume.

[0099] Test Example 2:

[0100] The functional group composition of polyacrylonitrile nanofiber membrane and three-dimensional nanofiber composite aerogel was analyzed by Fourier transform infrared spectroscopy.

[0101] like Figure 5 As shown, compared with the polyacrylonitrile nanofiber membrane, the three-dimensional nanofiber composite aerogel before cross-linking has a peak at 3343 cm -1 -OH, -NH, 1022cm -1 The vibration peak at C=C becomes stronger, indicating the successful introduction of cellulose nanocrystals and blocked isocyanate. In comparison, the vibration peak at 3343 cm-1 of the cross-linked three-dimensional nanofiber composite aerogel is -1 、1022cm -1 The vibration peak intensity at these two locations is weakened, indicating that the blocked isocyanate undergoes a cross-linking reaction with the cellulose nanocrystals; while the vibration peak intensity of the three-dimensional nanofiber composite aerogel coated with polypyrrole is enhanced, which is related to the successful introduction of polypyrrole.

[0102] Test Example 3:

[0103] The mechanical strengths of the three-dimensional nanofiber composite aerogels prepared in Example 6 and Comparative Example 2 were compared by loading a 20 g weight.

[0104] like Figure 3 As shown in A3 and B3 in FIG, the three-dimensional composite nanofiber aerogel (A3) with the addition of cellulose nanocrystals exhibits smaller deformation after being loaded with a 20g weight, indicating that the introduction of cellulose nanocrystals significantly improves the mechanical properties of the nanofiber aerogel. It can be seen that the preparation scheme of the nanofiber composite aerogel proposed in the present invention is conducive to improving the mechanical strength of the material.

[0105] Test Example 4:

[0106] 10 mg of three-dimensional nanofiber composite aerogel was added to 5 mL of 5 μg / mL dye mixed solution of acid orange 7, acid red 14 and rhodamine B. After shaking at room temperature for 6 hours, the aerogel was taken out with tweezers. Then, HPLC-DAD was used to detect acid orange 7, acid red 14 and rhodamine B in the solution before and after adsorption, and the adsorption efficiency of each aerogel for the three dyes was calculated.

[0107] Table 1 tests the aerogels in Examples 1 to 6, Comparative Example 1 and Comparative Example 2, and shows the test results of the adsorption performance of organic dyes. It can be seen from Table 1 that compared with the aerogels without polypyrrole PCA-1 and PA-1 and without adding cellulose nanocrystals PPA-1 and PA-1, the composite aerogels PPCA-1 to PPCA-6 have better comprehensive adsorption effects on the three dyes. The aerogels PCA-1 and PA-1 without polypyrrole have almost no adsorption effect on the anionic dyes acid orange 7 and acid red 14, but after being coated with polypyrrole, the aerogels significantly improve the adsorption effect of anionic dyes. In addition, the adsorption effect of the composite aerogel on cationic dyes is better than that of the aerogels without adding cellulose nanocrystals PPA-1 and without polypyrrole PCA-1. In summary, the three-dimensional nanofiber composite aerogel described in the embodiment of the present invention can simultaneously achieve efficient removal of anionic dyes and cationic dyes by utilizing the synergistic effect of electrospun nanofibers, cellulose nanocrystals and polypyrrole.

[0108] Table 1 Adsorption efficiency of three-dimensional nanofiber composite aerogels for organic dyes

[0109]

[0110] In summary, the present invention discloses the preparation of nanofibers by electrospinning technology; the electrospun nanofibers, cellulose nanocrystals, blocked isocyanate and water are mixed and homogenized to obtain a stable dispersion, and then freeze-set, freeze-dried and heat-crosslinked in sequence; finally, polymer nanoparticles are coated on the surface of the above product to obtain a three-dimensional nanofiber composite aerogel with a porous network structure, good mechanical stability and excellent adsorption performance. The preparation method of the three-dimensional nanofiber composite aerogel of the present invention is simple and easy to operate, and can simultaneously and efficiently adsorb and separate anionic and cationic dyes, and has great application prospects in the fields of treating industrial wastewater and repairing water environments.

[0111] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a three-dimensional nanofiber composite aerogel, characterized in that: The following steps are involved: Step 1: mixing the electrospun nanofibers, cellulose nanocrystals, blocked isocyanate and water and homogenizing them to prepare a dispersion; Step 2: subjecting the above dispersion to freeze-setting, freeze-drying and thermal cross-linking treatment in sequence to obtain a cross-linked product, namely, electrospun nanofiber-cellulose nanocrystal composite aerogel; Step 3: coating the electrospun nanofiber-cellulose nanocrystal composite aerogel with nanoparticles to obtain a three-dimensional nanofiber composite aerogel.

2. The method for preparing a three-dimensional nanofiber composite aerogel according to claim 1, characterized in that: The electrospun nanofibers described in step 1 are prepared by mixing one or more of polyacrylonitrile, nylon, cellulose acetate and polyethyleneimine.

3. The method for preparing a three-dimensional nanofiber composite aerogel according to claim 1, characterized in that: The added amount of the blocked isocyanate accounts for 10% to 30% of the total mass of the electrospun nanofibers and cellulose nanocrystals.

4. The method for preparing a three-dimensional nanofiber composite aerogel according to claim 1, characterized in that: In step 1, the mass ratio of the electrospun nanofibers to the cellulose nanocrystals is 1:0.25-0.67; in the prepared dispersion, the total mass of the electrospun nanofibers and the cellulose nanocrystals accounts for 0.6%-2.4% of the dispersion.

5. The method for preparing a three-dimensional nanofiber composite aerogel according to claim 1, characterized in that: In step 1, the homogenization speed is 8000-15000 rpm, and the homogenization time is 5-20 min.

6. The method for preparing a three-dimensional nanofiber composite aerogel according to claim 1, characterized in that: In step 2, the freezing setting temperature is -80 to -40°C, and the freezing setting time is 30 to 60 minutes; the freeze drying temperature is -80 to -60°C, and the freeze drying time is 20 to 30 hours; the thermal cross-linking treatment temperature is 120 to 130°C, and the thermal cross-linking treatment time is 1 to 2 hours.

7. The method for preparing a three-dimensional nanofiber composite aerogel according to claim 1, characterized in that: In step three, the loaded nanoparticles are at least one of polyaniline and polypyrrole.

8. A three-dimensional nanofiber composite aerogel prepared by the method for preparing a three-dimensional nanofiber composite aerogel according to any one of claims 1 to 7.

9. Use of the three-dimensional nanofiber composite aerogel according to claim 8 as an organic dye adsorbent.

10. The use according to claim 9, characterized in that The organic dyes include anionic dyes and cationic dyes.

Citation Information

Patent Citations

  • Polypyrrole / titanium dioxide composite adsorbent, its preparation, application and regeneration methods

    CN102350317A

  • Nano-crystalline cellulose based aerogel enhanced based on electrostatic adsorption cooperated with chemical crosslinking and preparation method of nano-crystalline cellulose based aerogel

    CN110437503A

  • Preparation method, product and application of polyaniline-coated cellulose nanocrystalline aerogel

    CN111607122A

  • Preparation of polypyrrole-polyacrylonitrile nanofiber membrane and application of polypyrrole-polyacrylonitrile nanofiber membrane in chromium ion adsorption

    CN112657474A

  • Polyaniline / cellulose composite nanofiber aerogel, and preparation and application thereof