Pig manure carbon-based functional material, preparation method and application

By preparing pig manure carbon-based functional materials and using pyrolysis and magnetic recovery technology, the problem of antibiotic treatment in livestock and poultry breeding wastewater has been solved, resource recycling and environmental protection have been achieved, and pollutant emissions have been reduced.

CN118807690APending Publication Date: 2024-10-22SHANDONG UNIV OF SCI & TECH

Patent Information

Application Number
CN202411140574.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The use of antibiotics in the livestock and poultry breeding industry has made it more difficult to treat breeding wastewater, and pig manure contains heavy metals, pathogens and other pollutants, which cannot be effectively treated and utilized harmlessly and resourcefully, causing environmental pollution.

Method used

Using the preparation method of pig manure carbon-based functional materials, by mixing pig manure with iron sources, urea and ascorbic acid and then pyrolyzing, materials with antibiotic adsorption and degradation capabilities were prepared, and resource recycling efficiency was improved through magnetic recovery.

Benefits of technology

It realizes the resource utilization of pig manure, reduces environmental pollution, uses a low-cost method to remove antibiotics from livestock and poultry breeding wastewater, improves the antibiotic removal and degradation effect, and improves the recycling efficiency of materials through magnetic recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807690A_ABST
    Figure CN118807690A_ABST
Patent Text Reader

Abstract

The invention discloses a pig manure carbon-based functional material as well as a preparation method and application thereof, and belongs to the field of resource utilization of livestock and poultry breeding wastes. The method comprises the following steps: (1) drying pig manure to constant weight; (2) dissolving an iron source, urea and ascorbic acid in water to obtain a modified solution; (3) mixing the dried pig manure with the modified solution to obtain a mixture; performing heating and heat preservation on the mixture; (4) taking out the pig manure in the mixture after heating and heat preservation, and drying to constant weight; then putting into a tubular furnace, and pyrolyzing in a nitrogen atmosphere; after the pyrolysis is completed, washing, drying, grinding and sieving to obtain the pig manure carbon-based functional material. According to the invention, pig manure is used as a raw material, ferrous sulfate, urea and ascorbic acid are used as modified substances, and the pig manure carbon-based functional material is prepared by continuously optimizing conditions. The pig manure carbon-based functional material can effectively remove antibiotics in pig breeding wastewater and has the advantages of being low in cost, green, environmentally friendly and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of resource utilization of livestock and poultry breeding waste, and in particular to a pig manure carbon-based functional material, a preparation method and an application thereof. Background Art

[0002] With the development of the economy, people's living standards have gradually improved, and people's demand for meat, eggs, milk, etc. has also increased. Therefore, livestock and poultry farming in my country has gradually become large-scale, and the livestock and poultry farming industry has achieved unprecedented development. However, behind the large-scale development is the large-scale generation of wastewater from the livestock and poultry farming industry. The use of antibiotics in the livestock and poultry farming industry has increased the difficulty of treating breeding wastewater. The use of antibiotics in livestock and poultry farms in my country is nearly 100,000 tons / year, accounting for about half of the annual consumption of antibiotics in the country. However, after antibiotics enter the body of livestock and poultry, most of them are excreted in the form of prototype drugs or primary metabolites with animal feces and urine, which seriously damages the environment and people's daily life.

[0003] At the same time, the rapid development of livestock and poultry farming has brought about the generation of a large amount of livestock and poultry manure. Since measures in this regard have not been perfected, a large amount of livestock and poultry manure has not been treated and utilized harmlessly and as a resource. Take pig manure as an example. There are still a lot of organic matter and nitrogen, phosphorus and potassium nutrients in pig manure, which are suitable for base fertilizer. However, pig manure also contains pollutants such as heavy metals, pathogens, and antibiotics. Random use will also cause pollution to the environment. Therefore, how to rationally use pig manure and ensure the reuse of resources is a technical problem that needs to be solved urgently. Summary of the invention

[0004] Based on the above technical problems, the present invention proposes a pig manure carbon-based functional material, a preparation method and an application.

[0005] The technical solution adopted by the present invention is:

[0006] A method for preparing a pig manure carbon-based functional material comprises the following steps:

[0007] (1) Drying pig manure to constant weight;

[0008] (2) dissolving an iron source, urea and ascorbic acid in water to obtain a modified solution;

[0009] (3) mixing the pig manure dried in step (1) with the modified solution obtained in step (2) to obtain a mixture; and heating and keeping the mixture warm;

[0010] (4) taking out the pig manure from the mixture after heating and heat preservation in step (3), drying it to constant weight; then placing it in a tubular furnace for pyrolysis; after the pyrolysis is completed, washing, drying, grinding and sieving are performed to obtain pig manure carbon-based functional materials.

[0011] Preferably, in step (1): the pig manure is placed in an oven and dried at 70-80° C. to constant weight.

[0012] Preferably, in step (2): the iron source is ferrous sulfate heptahydrate, and the concentration of ferrous sulfate heptahydrate in the modified solution is 50-60 g / L; the concentration of urea in the modified solution is 30-40 g / L; and the concentration of ascorbic acid in the modified solution is 20-30 g / L.

[0013] Preferably, in step (3), the mass volume ratio of pig manure to modified solution is 8-15 g:1 L.

[0014] Preferably, in step (3): the mixture is heated to 80-85°C and kept at this temperature for 10-12 hours.

[0015] Preferably, in step (4): the pig manure in the mixture is taken out, placed in an oven, and dried at 70-80° C. to constant weight.

[0016] Preferably, in step (4): the heating rate of the tubular furnace is controlled to be 5-10°C / min, the temperature is raised to 800-850°C, and the temperature is maintained at this constant temperature for 2-3 hours, and then the temperature is naturally lowered to room temperature.

[0017] The above-mentioned tubular furnace pyrolysis is carried out in an inert gas environment, and the inert gas is preferably a nitrogen atmosphere.

[0018] The present invention also provides a pig manure carbon-based functional material, which is prepared by the method as described above.

[0019] The present invention also provides the use of the pig manure carbon-based functional material as described above in the adsorption or degradation of antibiotics in livestock and poultry wastewater. Specifically, the antibiotics include tetracycline and ciprofloxacin.

[0020] The beneficial technical effects of the present invention are as follows:

[0021] (1) The present invention uses pig manure as a raw material to prepare pig manure carbon-based functional materials, thereby realizing the resource utilization of pig farm manure and reducing the pollution of pig manure to the environment to a certain extent; at the same time, the preparation method of the present invention is simple and low in cost, and the prepared pig manure carbon-based functional materials can be used to remove antibiotics in livestock and poultry breeding wastewater, achieving the purpose of waste treatment and ensuring the recycling of resources.

[0022] (2) Due to the addition of N element, the pig manure carbon-based functional material prepared by the present invention enriches the types and quantities of active sites on the surface of the material, thereby promoting the removal of antibiotics.

[0023] (3) The pig manure carbon-based functional material prepared by the present invention also contains Fe element, which, in combination with N element and reducing agent ascorbic acid, can further enhance the degradation and removal effect of the material on antibiotics. Moreover, the addition of Fe element also endows the carbon-based functional material with excellent magnetic recovery ability, ensuring that the material can be recovered again under the action of an external magnetic field after removing the antibiotics, thereby improving the recycling efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The figures are the adsorption effect of PM1 and PM2 prepared in Examples 1 and 2 of the present invention on antibiotics in pig breeding wastewater; wherein (a) shows the adsorption effect of tetracycline (TC), and (b) shows the adsorption effect of ciprofloxacin (CIP);

[0025] Figure 2 The degradation effect diagram of PM1 and PM2 prepared in Example 1 and Example 2 of the present invention on antibiotics in pig breeding wastewater; wherein (a) shows the degradation effect of TC, and (b) shows the degradation effect of CIP;

[0026] Figure 3 This is a scanning electron microscope (SEM) image of the PM2 material prepared in Example 2 of the present invention;

[0027] Figure 4 This is an X-ray photoelectron spectrum (XPS) diagram of the PM2 material prepared in Example 2 of the present invention;

[0028] Figure 5 This is a graph showing the degradation effect of the PM2 material prepared in Example 2 of the present invention on antibiotics in pig breeding wastewater under different dosage conditions;

[0029] Figure 6 This is a graph showing the degradation effect of the PM2 material prepared in Example 2 of the present invention on antibiotics in pig breeding wastewater under different PMS concentration conditions;

[0030] Figure 7 The figure shows the degradation effect of the pig manure carbon-based functional material on the TC and CIP mixed system obtained by changing the mass ratio (material nitrogen ratio) of the pig manure material and the urea in the modified solution in the present invention; wherein (a) shows the degradation effect diagram for TC; (b) shows the degradation effect diagram for CIP;

[0031] Figure 8 The graphs show the degradation effects of the pig manure carbon-based functional material obtained by changing the pyrolysis temperature on the TC and CIP mixed system; wherein (a) shows the degradation effect graph on TC; and (b) shows the degradation effect graph on CIP. DETAILED DESCRIPTION

[0032] The present invention provides a pig manure carbon-based functional material, a preparation method and an application thereof, wherein pig manure is used as a raw material, ferrous sulfate (iron source), urea (nitrogen source) and ascorbic acid (reducing agent) are used as a modifying substance, and the pig manure carbon-based functional material is prepared by continuously optimizing the conditions. The pig manure carbon-based functional material can effectively remove antibiotics in pig breeding wastewater, and the selection of pig manure as a raw material ensures that the raw material is green and environmentally friendly, and achieves the recycling of waste. At the same time, the present invention fully achieves the recycling of breeding waste with a simple preparation process and low cost.

[0033] The present invention is further described below in conjunction with specific embodiments and application examples.

[0034] Example 1

[0035] (1) Place the dried pig manure in an oven and dry it at 80°C until constant weight is reached. The material is then sealed and stored in a dry place.

[0036] (2) The material obtained in step (1) was placed in a tubular furnace, heated to 800°C at a heating rate of 10°C / min in a nitrogen atmosphere, and kept at this temperature for 2 hours for calcination. After the tubular furnace was cooled to room temperature naturally, the material was taken out, washed several times, and then placed in an oven at 80°C to dry to constant weight, the material was taken out and ground through a 100-mesh sieve, and then the material was sealed and stored to prepare a pig manure carbon-based functional material, named PM1.

[0037] Example 2

[0038] (1) Place the dried pig manure in an oven and dry it at 80°C until constant weight is reached. The material is then sealed and stored in a dry place.

[0039] (2) Prepare 100 ml of distilled water, weigh 5.56 g of FeSO4·7H2O, 3 g of urea and 2.5 g of ascorbic acid, and dissolve them in 100 ml of distilled water respectively to obtain a modified solution. Weigh 1 g of the pig manure material obtained in step (1), and then add it to the modified solution to obtain a mixture. Put the mixture into an oven and heat it at 80°C for 10 hours for heat impregnation. Then take out the pig manure material from the mixture, put it into an oven and dry it at 80°C to constant weight, and seal it for dry storage.

[0040] (3) The material obtained in step (2) is placed in a tubular furnace, and the temperature is raised to 800°C at a heating rate of 10°C / min under a nitrogen atmosphere, and the temperature is maintained at a constant temperature for 2 hours to perform calcination and pyrolysis. After the pyrolysis is completed, the tubular furnace is cooled naturally to room temperature, the material is taken out, washed several times, and then placed in an oven at 80°C to dry to constant weight, the material is taken out and ground through a 100-mesh sieve, and the material is sealed and dried to obtain a pig manure carbon-based functional material, named PM2.

[0041] Application Example 1

[0042] The pig manure carbon-based functional materials prepared in Example 1 and Example 2 were used for adsorption of antibiotics in pig breeding wastewater.

[0043] Adsorption experiment: Take 24 mg (300 mg / L) of PM1 and PM2 respectively and put them into 80 mL of pig breeding wastewater. Oscillate them at room temperature and pH 7.0 for 5, 10, 15, 20, 25, 30, 40, 60, 90 and 120 min respectively. Use ultraviolet spectrophotometer to detect the implementation process at each time point.

[0044] Adsorption performance evaluation: Figure 1 As shown in the figure, it is found that PM2 has a better adsorption effect on antibiotics within 120 minutes, compared with PM1 that is only pyrolyzed and PM2 that is added with elements such as iron and nitrogen. Taking TC and CIP as examples, the removal rates of TC and CIP by PM2 are 35% and 33% respectively, while the removal rates of TC and CIP by PM1 are only 17% and 20% respectively. It can be seen that the addition of Fe and N elements promotes the removal of antibiotics. However, the overall adsorption effect is poor, and pollutant desorption is found during the adsorption process, which indicates that secondary pollution may occur through adsorption. Therefore, in order to improve the removal effect of antibiotics and ensure that the phenomenon of re-pollution is reduced, it is preferred to use degradation to remove antibiotics from pig breeding wastewater.

[0045] Application Example 2

[0046] The pig manure carbon-based functional materials obtained in Example 1 and Example 2 were used to degrade antibiotics in pig breeding wastewater.

[0047] Degradation experiment: Take 24 mg (300 mg / L) PM1, PM2, and 0.1 mM potassium persulfate (PMS) and put them into 80 mL of pig breeding wastewater. Oscillate them at room temperature and pH 7.0 for 5, 10, 15, 20, 25, 30, 40, and 60 min, respectively. Use a UV spectrophotometer to detect the implementation process at each time point.

[0048] Degradation performance evaluation: Figure 2 As shown in the results, it can be seen that the antibiotic removal rate within 60 minutes is higher than the removal rate during adsorption, especially for PM2 material, which is significantly improved. This is also related to the doping of Fe and N elements. Under high temperature conditions, Fe generally exists in the form of Fe2O3 and Fe3O4. When PMS is adsorbed to PM2, it will react with Fe on the catalyst. 3+ The reaction generates Fe 2+ (See formula (1)), then Fe 2+Then it reacts with PMS to generate active oxides (see formula (2)), which in turn promotes the removal of antibiotics. Similarly, the doping of N elements also promotes the generation of free radicals. Pyridine N has a long pair of electrons that can promote the transfer of free-flowing π electrons from the sp2 carbon of the biological carbon base to activate PMS and generate active oxides to participate in the degradation process of antibiotics.

[0049]

[0050] Figure 3 This is a SEM image of the PM2 material prepared in Example 2 of the present invention. From the image, it can be seen that after high-temperature pyrolysis, the material is carbonized and iron oxides are obviously attached to the surface of the material.

[0051] Figure 4 This is the XPS graph of the PM2 material prepared in Example 2 of the present invention. From the graph, it can be clearly observed that Fe and N elements exist on the scanning curve of the PM2 material, indicating that Fe and N elements are successfully doped on the PM2 material.

[0052] Application Example 3

[0053] The PM2 prepared in Example 2 was used to degrade antibiotics in pig breeding wastewater under different dosage conditions.

[0054] The degradation experiment is roughly the same as the process of degrading antibiotics in pig breeding wastewater in Application Example 2. The difference is that the PM2 dosage is increased to 40 mg (500 mg / L), 64 mg (800 mg / L), and 80 mg (1 g / L), respectively.

[0055] Degradation performance evaluation: passed Figure 5 It can be observed that the higher the dosage of PM2, the better the antibiotic removal effect, taking TC and CIP as examples. Under the condition of 1g / L dosage, the removal rate of TC and CIP can reach 75% within 60min. This shows that the increase in the amount of catalyst can significantly improve the removal effect of antibiotics. A higher amount of catalyst will provide more active sites for the activation of PMS, thereby promoting the degradation of TC and CIP. Therefore, the present invention selects 80mg (1g / L) as the condition to carry out the next stage of the experimental process.

[0056] Application Example 4

[0057] The PM2 prepared in Example 2 was used to degrade antibiotics in pig breeding wastewater under different PMS concentration conditions.

[0058] The degradation experiment is roughly the same as the process of degrading antibiotics in pig breeding wastewater in Application Example 2, except that the PM2 dosage is increased to 80 mg (1 g / L). The difference is that the PMS concentration is increased to 0.3 mM, 0.5 mM, 0.8 mM, and 1 mM.

[0059] Degradation performance evaluation: passed Figure 6 It can be observed that with the increase of PMS concentration, PM2 has different changes in antibiotic removal, taking TC and CIP as examples. In terms of TC removal, as the PMS concentration increases (0.3mM, 0.5mM), the TC removal rate gradually increases, reaching 91% in 60min, and when the PMS concentration is further increased (0.8mM, 1mM), the TC removal rate shows a decreasing trend, retreating to 80% in 60min. The situation of CIP removal is different. As PMS increases to 0.3mM, the CIP removal rate decreases to 68%. When it is further increased to 0.5mM, the CIP removal rate increases to 72% (but still lower than 76% when PMS is 0.1mM). When PMS is further increased (0.8mM, 1mM), the CIP removal rate decreases again to 70%. This shows that under certain conditions, the increase in PMS concentration will produce more active oxides together with the catalyst, thereby removing antibiotics. When the PMS concentration is further increased, the excess SO4 ﹒ - will react with each other and no longer participate in the removal of antibiotics, which will lead to a decrease in the antibiotic removal rate.

[0060] Example 3

[0061] In order to select the conditions such as the amount of raw materials, the present invention studies the effect of removing antibiotics under different proportions of nitrogen doping. The preparation method is the same as Example 2. The mass ratios of the dried pig manure material and urea are 1:1, 1:2, 1:3, 1:4, and 1:5, respectively, and the corresponding pig manure carbon-based functional materials are named PM 1∶1 、PM 1∶2 、PM 1∶3 、PM 1∶4 、PM 1∶5 .

[0062] Degradation performance evaluation: Figure 7 As shown in the figure, it can be observed that there is competition between TC and CIP, and the removal rate of TC is much higher than that of CIP. The removal of TC is very fast in the first 5 minutes, and then gradually slows down with the passage of time. PM 1∶3 , showed good removal effect in the early stage, and the removal of TC reached 50% within 10 minutes, but the removal effect was weak in the later stage. 1∶1 PM with a nitrogen ratio of 1:2 1∶2With the poor removal performance in the early stage, the two materials with the most TC removal in the end were nearly 60%. For CIP removal, the removal effect of each material was far less than that of TC. 1∶3 In the first 20 minutes, the removal effect was much better than other materials, and the removal balance was reached. Although other modified materials were always in the removal state, the removal effect within 60 minutes was lower than that of PM 1:3 Therefore, the removal effects of the two pollutants were comprehensively compared and PM 1:3 Condition of the materials, proceed to the next stage of the experimental process.

[0063] Example 4

[0064] The preparation method is the same as that of Example 2, except that the pyrolysis temperature is changed. The ability of materials prepared at different pyrolysis temperatures (300°C, 400°C, 500°C, 700°C, 800°C) to degrade antibiotics is observed.

[0065] Degradation performance evaluation: Figure 8 As shown in the figure, with the increase of pyrolysis temperature (400, 500°C), the removal rate of TC and CIP of the obtained pig manure carbon-based functional material PM gradually decreased, and when the temperature further increased to 700°C, the removal rate of TC and CIP of PM was improved again. When the pyrolysis temperature was further increased to 800°C, the removal rate of TC and CIP of PM was greatly improved compared with the PM obtained at 700°C, and the removal effect of TC and CIP was the best among all materials. From a simple analysis, the main reason for the good removal effect is that the pyrolysis temperature is high, the carbonization effect of the material is better, and the material can be in better contact with the pollutant. At the same time, the specific surface area is increased, providing more active sites, greatly improving the degradation ability of the material. Therefore, the preferred pyrolysis temperature is 800°C.

[0066] The parts not mentioned in the above methods can be realized by adopting or drawing on existing technologies.

[0067] The above description is only for the preferred embodiments of the present invention and does not limit the present invention. Any improvement or change made by a person skilled in the art without departing from the creative thinking of the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing pig manure carbon-based functional materials, characterized in that The following steps are involved: (1) Drying pig manure to constant weight; (2) dissolving an iron source, urea and ascorbic acid in water to obtain a modified solution; (3) mixing the pig manure dried in step (1) with the modified solution obtained in step (2) to obtain a mixture; and heating and keeping the mixture warm; (4) taking out the pig manure from the mixture heated and kept warm in step (3), drying it to constant weight; and then placing it in a tube furnace for pyrolysis; After the pyrolysis is completed, the product is washed, dried, ground and sieved to obtain pig manure carbon-based functional materials.

2. The method for preparing a pig manure carbon-based functional material according to claim 1, characterized in that: In step (1): the pig manure is placed in an oven and dried at 70-80° C. to a constant weight.

3. The method for preparing a pig manure carbon-based functional material according to claim 1, characterized in that: In step (2), the iron source is ferrous sulfate heptahydrate, and the concentration of ferrous sulfate heptahydrate in the modified solution is 50-60 g / L; the concentration of urea in the modified solution is 30-40 g / L; and the concentration of ascorbic acid in the modified solution is 20-30 g / L.

4. The method for preparing a pig manure carbon-based functional material according to claim 1, characterized in that: In step (3): the mass volume ratio of pig manure to modified solution is 8-15g:1L.

5. The method for preparing a pig manure carbon-based functional material according to claim 1, characterized in that: In step (3): the mixture is heated to 80-85°C and kept at this temperature for 10-12 hours.

6. The method for preparing a pig manure carbon-based functional material according to claim 1, characterized in that: In step (4): the pig manure in the mixture is taken out, placed in an oven, and dried at 70-80° C. to constant weight.

7. The method for preparing a pig manure carbon-based functional material according to claim 1, characterized in that: In step (4): the heating rate of the tubular furnace is controlled to be 5-10°C / min, the temperature is raised to 800-850°C, and the temperature is maintained at this temperature for 2-3 hours, and then the temperature is naturally lowered to room temperature.

8. A pig manure carbon-based functional material, characterized in that: It is prepared by the method according to any one of claims 1 to 7.

9. Use of the pig manure carbon-based functional material as claimed in claim 8 in the adsorption or degradation of antibiotics in livestock and poultry breeding wastewater.

10. The use of the pig manure carbon-based functional material as claimed in claim 9, characterized in that: The antibiotics include tetracycline and ciprofloxacin.

Citation Information

Patent Citations

  • Preparation method and application of iron-loaded pig manure biochar

    CN109317099A

  • Iron-nitrogen co-doped biochar catalyst and preparation method and application thereof

    CN113198516A

  • Livestock and poultry waste recycling water treatment catalyst as well as preparation method and application thereof

    CN117463388A

Cited By

  • Method for removing antibiotics by coupling magnetic biochar with dissimilatory iron reducing bacteria

    CN120622689A

  • Cow dung and liquid dung recycling product and preparation method thereof

    CN120698834A